Straight-through microporous metal net and preparation method

By combining the template method and the investment method, taking advantage of the characteristics of easy-to-separate materials, and using powder metallurgy technology to prepare straight-through microporous metal mesh, it solves the problems of high equipment investment, low material utilization and high preparation cost in the existing technology, and achieves Efficient and low-cost microporous metal mesh preparation, suitable for straight-through microporous metal mesh with complex structure.

CN118720139APending Publication Date: 2024-10-01UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410811568.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing straight-through microporous metal mesh preparation method has problems such as high investment in equipment and technology, low material utilization rate, difficult preparation and easy wear of tools, difficulty in obtaining micropores with high dimensional accuracy requirements, high preparation cost, and low production efficiency.

Method used

Using binder and metal powder as raw materials, combining the template method and the investment method, taking advantage of the characteristics of easily separated materials, the straight-through microporous metal mesh is prepared through powder metallurgy technology, including micro-pillar mold preparation, metal slurry preparation, drying and Demoulding, sintering and other steps enable precise control of pore size, pore wall size and pore distribution density.

Benefits of technology

It achieves a short process flow, low equipment requirements, easy operation, low production cost, and high efficiency. It can meet different shapes, sizes and performance requirements, and is suitable for complex structures such as ultra-thin hole walls, thin thickness, variable thickness, and special-shaped micropores. The preparation of straight-through microporous metal mesh improves material utilization and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720139A_ABST
    Figure CN118720139A_ABST
Patent Text Reader

Abstract

The invention discloses a straight-through microporous metal net and a preparation method, and belongs to the technical field of metal net preparation. The method comprises the specific steps of micro-column mold preparation, metal slurry preparation, metal blank preparation, drying, demolding and sintering. The method has the advantages that the shape and size, the hole form, the hole diameter, the hole wall size and the hole distribution density of the straight-through microporous metal net can be accurately adjusted and controlled, the equipment investment is small, operation is easy, the material utilization rate and the production efficiency are high, the production cost is low, and automatic large-batch production is easy to achieve; the straight-through microporous metal net is high in internal and surface quality, good in hole size precision, excellent in performance, multiple in variety specification and wide in application range. The method is particularly suitable for preparing straight-through microporous metal nets which have ultra-thin hole walls, thin thickness, variable thickness, special-shaped micropores, special-shaped structures, non-periodic hole distribution or layered compounding and enhanced compounding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal mesh preparation, and in particular to a straight-through microporous metal mesh and a preparation method thereof, which is particularly suitable for the preparation of a straight-through microporous metal mesh with ultra-thin hole walls, thin thickness, variable thickness, special-shaped micropores, special-shaped structures, non-periodic pore distribution or layered composite and reinforced composite. Background Art

[0002] The through-hole microporous metal mesh has a large number of through holes arranged periodically or non-periodically and the aperture is ≤1mm. It has the characteristics of large number of holes and small aperture, including through-hole single metal mesh and through-hole layered composite metal mesh. It is a new type of metal material, playing an active role in the fields of petrochemical, precision instruments, printing and textile. However, the harsh working conditions and high-end use requirements have put forward higher requirements on the dimensional accuracy, micropore density, production cost, preparation efficiency, material utilization rate and product quality of the through-hole microporous metal mesh.

[0003] The existing methods for preparing straight-through microporous metal mesh mainly include the method of using metal wire weaving mesh, or punching, mechanical processing, electric spark processing, electrochemical processing and laser processing of metal plate, strip and foil. The method of using metal wire weaving mesh has the problems of complex mesh forming process, difficult layer thickness control, poor hole accuracy, difficulty in adjusting thickness and hole wall separately, easy entanglement and breakage between metal wires, and its preparation process has high requirements on the quality of metal wire raw materials, weaving technology and equipment investment. The method of micro-hole processing of metal plates, strips and foils requires the use of special precision tools, such as micro-punches for punching, micro-drills for machining, and micro-electrodes for electric spark and electrochemical machining. There are problems such as difficulty in tool preparation, high processing cost and easy wear, easy burrs on the edges of micro-holes, great influence of tools on thin-walled structures and low material utilization. Although laser processing can solve the above-mentioned machining problems, the surface of the micro-holes is easily affected by high temperature and recast layers, holes or micro-cracks will appear, which greatly reduces the dimensional accuracy and quality of the micro-holes. At the same time, the efficiency of laser processing is low and the cost is high, which is not suitable for mass production.

[0004] In summary, the existing methods for preparing straight-through microporous metal mesh have problems such as large equipment and technical investment, low material utilization rate, difficult and easy wear of tools, difficulty in obtaining micropores with high dimensional accuracy requirements, high preparation cost and low production efficiency. Therefore, it is urgent to develop a low-cost, easy-to-operate and high-efficiency method for preparing straight-through microporous metal mesh, which is of great significance to prepare high-quality straight-through microporous metal mesh with precisely controllable pore size, pore wall size, pore distribution density and thickness shape size. Summary of the invention

[0005] The purpose of the present invention is to provide a straight-through microporous metal mesh and a preparation method to solve the problems existing in the existing straight-through microporous metal mesh preparation method. The preparation method uses a binder and metal powder as raw materials, combines a template method with a melt casting method, utilizes the characteristics of easily separable materials, and adopts powder metallurgy technology to prepare the straight-through microporous metal mesh. The straight-through microporous metal mesh prepared by this method has the advantages of short process flow, low equipment requirements, convenient operation, unlimited product size, low production cost, high efficiency, and the ability to meet different shape, size and performance requirements. It is particularly suitable for the preparation of straight-through microporous metal meshes with ultra-thin pore walls (size ≤ 1mm), thin thickness, variable thickness, special-shaped micropores, special-shaped structures, non-periodic pore distribution or layered composites, and reinforced composites.

[0006] According to a first aspect of the technical solution of the present invention, a method for preparing a straight-through microporous metal mesh is provided, comprising the following steps:

[0007] S1, preparation of micro-column mold: using a straight-through microporous mesh template to imprint or cut the easily separable material, and separating the two after solidification and forming, to obtain a micro-column mold whose horizontal cross section is precisely matched with the straight-through microporous mesh template;

[0008] S2, metal slurry preparation: mixing the binder solution and the metal powder and stirring them evenly to obtain metal slurry;

[0009] S3, metal blank preparation: pouring the metal slurry into the gap of the microcolumn mold, and then pressing and leveling to obtain a metal blank;

[0010] S4, drying and demoulding: drying and degreasing the integral part composed of the metal blank and the micro-column mold, and then separating the two to achieve demoulding, so as to obtain a straight-through microporous metal mesh preform;

[0011] S5, sintering: sintering the straight microporous metal mesh preform in a protective gas atmosphere for the first time and the second time in sequence, and then cooling the preform to room temperature in a furnace to obtain the straight microporous metal mesh.

[0012] Furthermore, in S1, the material of the straight-through microporous mesh template is one of metal material, ceramic material, polymer material or composite material;

[0013] Wherein, there are no impurities in the pores of the straight-through microporous mesh template.

[0014] Further, in S1, the easily separable material is at least one of a resin, paraffin or glass that is easily melted, easily decomposed or easily softened after heating;

[0015] Wherein, the resin is a polymer material with a low melting point and easily softened or decomposed upon heating;

[0016] Wherein, the paraffin wax is at least one of polyethylene wax, polytetrafluoroethylene wax, microcrystalline wax or semi-microcrystalline wax having a melting point of 60-120°C;

[0017] Wherein, the softening point of the glass is lower than the melting point of the metal material used for the straight-through microporous metal mesh.

[0018] Further, in S2, the binder is at least one of polyvinyl alcohol, epoxy resin, ethylene-vinyl acetate copolymer, stearic acid, polyoxymethylene or polyethyleneimine; wherein the mass fraction of the binder in the metal slurry is 3%-15%;

[0019] The metal powder is at least one of pure metal powder, alloy powder, reinforcement and mixed powder composed of pure metal or alloy.

[0020] Further, in S2, the stirring method is at least one of magnetic stirring, ultrasonic stirring or mechanical stirring;

[0021] Wherein, the stirring speed of the magnetic stirring is 200-1000r / min, and the stirring time is 10-40min.

[0022] Furthermore, in S3, the metal slurry is poured into the microcolumn mold and then pressed or leveled;

[0023] Wherein, the leveling is at least one of scraping with a scraper, cutting with a cutter, ultrasonic vibration or pressing with a pad.

[0024] Furthermore, in S4, the heating temperature of the drying and degreasing is increased from room temperature to 60-130°C at 0.5-3°C / min, and the drying time is 2-5h; the heating temperature of the demoulding is increased from room temperature to 60-400°C at 2-5°C / min, and the insulation time is 1-5h.

[0025] Further, in S5, the protective gas is at least one of nitrogen, reducing gas or inert gas;

[0026] Among them, the sintering temperature of the first sintering in S5 is increased from room temperature to 200-480°C at 0.5-5°C / min, and the sintering time is 1-5h; the sintering temperature of the second sintering is increased from the highest sintering temperature of the first sintering to 500-1500°C at 5-10°C / min, and the sintering time is 0.5-5h.

[0027] Furthermore, the method also includes surface treatment of the straight-through microporous metal mesh.

[0028] According to a second aspect of the technical solution of the present invention, a through-microporous metal mesh is provided, wherein the through-microporous metal mesh is prepared by the preparation method according to any one of the above aspects.

[0029] The beneficial effects of the present invention are:

[0030] (1) The technical solution of the present invention uses binder and metal powder as raw materials, combines the template method with the investment method, takes advantage of the characteristics of easily separable materials, and adopts powder metallurgy technology to prepare straight-through microporous metal mesh. The method for preparing straight-through microporous metal mesh has the advantages of short process flow, low equipment requirements, convenient operation, unlimited product size, low production cost, high efficiency, and the ability to meet different shape, size and performance requirements. It is particularly suitable for the preparation of straight-through microporous metal mesh with ultra-thin pore walls (size ≤ 1mm), thin thickness, variable thickness, special-shaped micropores, special-shaped structures, non-periodic pore distribution or layered composite, and reinforced composite.

[0031] (2) The preparation method of the present invention can accurately control the shape and size of the straight-through microporous metal mesh, as well as the form of the holes, the hole diameter, the hole wall size and the hole distribution density, etc., with low equipment investment, simple operation, high production efficiency, high material utilization rate, low production cost, and easy to realize automated mass production. It is particularly suitable for the preparation of straight-through microporous metal mesh with ultra-thin hole wall (size ≤ 1mm), thin thickness, variable thickness, special-shaped micropores, special-shaped structures, non-periodic hole distribution or layered composite, reinforced composite.

[0032] (3) The straight through microporous metal mesh of the present invention has high internal and surface quality, good hole size accuracy, excellent performance, a variety of varieties and specifications, and a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a process flow chart of the preparation of the straight-through microporous metal mesh of the present invention. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with specific embodiments, which should not be construed as limiting the scope of protection of the present invention. Professional and technical personnel in the field can make non-essential improvements and adjustments based on the contents of the present invention.

[0035] The technical solution of the present invention provides a method for preparing a straight-through microporous metal mesh.

[0036] In a preferred embodiment, Figure 1 As shown, the preparation method of the straight-through microporous metal mesh includes the following steps:

[0037] S1, preparation of micro-column mold: using a straight-through microporous mesh template to imprint or cut a liquid, semi-solid or solid easily separable material, and separating the straight-through microporous mesh template from the micro-column mold after solidification to obtain a micro-column mold whose horizontal cross section is precisely matched with the straight-through microporous mesh template.

[0038] Among them, the material of the straight-through microporous mesh template is one of metal materials, ceramic materials, polymer materials or composite materials, and there are no impurities in the holes of the straight-through microporous mesh template; the easily separable material is at least one of resin, paraffin or glass that is easy to melt, decompose or soften after heating; the resin is a polymer material with a low melting point and is easy to soften or decompose when heated, the paraffin is at least one of polyethylene wax, polytetrafluoroethylene wax, microcrystalline wax or semi-microcrystalline wax with a melting point of 60-120°C, and the softening point of the glass is lower than the melting point of the metal material used for the straight-through microporous metal mesh.

[0039] S2, metal slurry preparation: the binder solution is mixed with the metal powder and stirred evenly to obtain metal slurry.

[0040] Wherein, the binder is at least one of polyvinyl alcohol, epoxy resin, ethylene-vinyl acetate copolymer, stearic acid, polyoxymethylene or polyethyleneimine, the metal powder is at least one of pure metal powder, alloy powder, reinforcement and mixed powder of pure metal or alloy, and the mass fraction of the binder in the metal slurry is 3%-15%; the stirring method is at least one of magnetic stirring, ultrasonic stirring or mechanical stirring, the stirring speed of the magnetic stirring is 200-1000r / min, and the stirring time is 10-40min.

[0041] S3, metal blank preparation: pouring the metal slurry into the gap of the micro-column mold, and then pressing and flattening to obtain a metal blank, the horizontal cross section of which has the same shape and size as the straight-through microporous mesh template.

[0042] The metal slurry is poured into the microcolumn mold and then pressed or leveled. The leveling is performed by at least one of scraping with a scraper, cutting with a cutter, ultrasonic vibration or pressing with a pad.

[0043] S4, drying and demoulding: drying and degreasing the integral part composed of the metal blank and the micro-column mold, and separating the metal blank and the micro-column mold by melting, decomposing or softening the easily separable material, thereby achieving demoulding and obtaining a straight-through microporous metal mesh preform.

[0044] The heating temperature of the drying and degreasing is increased from room temperature to 60-130°C at 0.5-3°C / min, and the drying time is 2-5h; the heating temperature of the demoulding is increased from room temperature to 60-400°C at 2-5°C / min, and the insulation time is 1-5h.

[0045] S5, sintering: the straight microporous metal mesh preform is subjected to a first (low temperature) sintering and a second (high temperature) sintering in sequence under a protective gas atmosphere, and then cooled to room temperature in a furnace to obtain a straight microporous metal mesh.

[0046] Wherein, the protective gas is at least one of nitrogen, reducing gas or inert gas; the sintering temperature of the low-temperature sintering is increased from room temperature to 200-480°C at 0.5-5°C / min, and the sintering time is 1-5h; the sintering temperature of the high-temperature sintering is increased from the highest sintering temperature of the low-temperature sintering to 500-1500°C at 5-10°C / min, and the sintering time is 0.5-5h.

[0047] In another preferred embodiment, the straight-through microporous metal mesh may be surface treated.

[0048] The technical solution of the present invention also provides a straight-through microporous metal mesh, which is prepared by the preparation method described above.

[0049] Example 1: A resin microcolumn mold was prepared using a straight microporous 304L stainless steel mesh with a pore size of 0.3 mm, a pore spacing and a mesh thickness of 1 mm as a template, and then filled with pure copper slurry, dried, demoulded and sintered to prepare a straight microporous copper mesh.

[0050] The semi-solidified resin is printed using a straight-through microporous 304L stainless steel mesh, so that the resin can fully flow into the micropores of the straight-through microporous 304L stainless steel mesh template to form, and the excess resin overflowing the surface is removed. After the resin is solidified to form a microcolumn, the straight-through microporous 304L stainless steel mesh template is taken out, and the resin microcolumn mold is obtained after the semi-solidified resin is completely solidified.

[0051] Pure copper powder was added into 6% polyvinyl alcohol binder solution, mixed and stirred evenly to obtain pure copper slurry. The mass fraction of polyvinyl alcohol in the pure copper slurry was 5.5%. The magnetic stirring time was 10 min and the stirring speed was 400 r / min.

[0052] Pour the evenly mixed pure copper slurry into the gap of the resin micro-column mold in small amounts and multiple times, then use a scraper to scrape it in one direction multiple times to prevent the pure copper slurry from mixing with gas and producing tiny holes when flowing into the resin micro-column mold. Then quickly perform ultrasonic vibration for 5 minutes to make the pure copper slurry completely fill the resin micro-column mold.

[0053] The resin microcolumn mold filled with pure copper slurry was heated from room temperature to 80°C at 2°C / min and kept for 1 hour for drying and degreasing, then heated to 100°C at the same heating rate for 2 hours for further drying and degreasing, and then heated to 350°C at 5°C / min and kept for 3 hours to complete demolding, thereby obtaining a straight-through microporous copper mesh preform.

[0054] The straight-through microporous copper mesh preform was subjected to low-temperature sintering and high-temperature sintering in sequence under NH3 atmosphere and gas flow rate of 0.3-2L / min. The low-temperature sintering was carried out from room temperature to 450°C at a rate of 5°C / min and the sintering time was 2h. The high-temperature sintering was carried out from 450°C to 1000°C at a rate of 10°C / min and the sintering time was 2h. Then it was cooled to room temperature in the furnace to obtain the straight-through microporous copper mesh.

[0055] Example 2: A paraffin microcolumn mold was prepared using a straight microporous 316L stainless steel mesh with a pore size of 0.5 mm, a pore spacing of 0.6 mm, and a mesh thickness of 1.5 mm as a template, and then filled with copper-tin alloy (CuSn10) slurry, dried, demolded, and sintered to prepare a straight microporous copper-tin alloy mesh.

[0056] Heat the solid block paraffin to 100°C to completely melt the solid paraffin into liquid. After standing at room temperature for 2 minutes, pour the liquid paraffin into a container to level it. Place the straight-through microporous 316L stainless steel mesh template on the surface of the liquid paraffin for embossing, so that the paraffin fully flows into the micropores of the straight-through microporous 316L stainless steel mesh template to form, and remove the excess paraffin that overflows the surface to avoid the paraffin microcolumn from breaking during demolding. After the paraffin solidifies to form the microcolumn, use the lubricity of the paraffin to smoothly remove the straight-through microporous 316L stainless steel mesh template, and obtain the paraffin microcolumn mold after the liquid paraffin is completely solidified.

[0057] The copper-tin alloy powder was added into a 5% polyvinyl alcohol binder solution, mixed and stirred evenly to obtain a copper-tin alloy slurry. The mass fraction of polyvinyl alcohol in the copper-tin alloy slurry was 6.25%. The magnetic stirring time was 10 minutes and the stirring speed was 400 r / min.

[0058] Pour the evenly mixed copper-tin alloy slurry into the gap of the paraffin microcolumn mold in small amounts and multiple times, and then use a scraper to scrape it in one direction multiple times to prevent the copper-tin alloy slurry from mixing with gas and producing tiny holes when flowing into the paraffin microcolumn mold. Then quickly perform ultrasonic vibration for 5 minutes to make the copper-tin alloy slurry completely fill the paraffin microcolumn mold.

[0059] The paraffin microcolumn mold filled with copper-tin alloy slurry was heated from room temperature to 80°C at 2°C / min and kept warm for 1 hour for drying and dewaxing, then heated to 100°C at the same heating rate for 1 hour for further drying and dewaxing, and then heated to 120°C at 3°C / min and kept warm for 2 hours to complete demolding, thereby obtaining a straight-through microporous copper-tin alloy mesh preform.

[0060] The straight-through microporous copper-tin alloy mesh preform was subjected to low-temperature sintering and high-temperature sintering in sequence under Ar atmosphere and gas flow rate of 1.5L / min. The low-temperature sintering was heated from room temperature to 450°C at a rate of 3°C / min and the sintering time was 1h. The high-temperature sintering was heated to 850°C at a rate of 10°C / min and the sintering time was 1.5h. It was then cooled to room temperature in the furnace to obtain a straight-through microporous copper-tin alloy mesh.

[0061] Example 3: A resin / paraffin microcolumn mold was prepared using a straight microporous Q235 carbon steel mesh with a pore size and pore spacing of 0.9 mm and a mesh thickness of 0.6 mm as a template, and then filled with pure titanium slurry, dried, demolded, and sintered to prepare a straight microporous titanium mesh.

[0062] Put 15% paraffin wax by mass into the resin solution, mix and stir evenly at 70°C, pour the evenly stirred resin / paraffin mixture into a container, let it flow and stand still at room temperature to a semi-solidified state, use a straight-through microporous Q235 carbon steel mesh template to imprint the semi-solidified resin / paraffin mixture, so that the resin / paraffin mixture fully flows into the micropores of the straight-through microporous Q235 carbon steel mesh template to form, and remove the excess resin / paraffin mixture overflowing the surface to ensure smooth subsequent demolding, and after the resin / paraffin mixture forms a microcolumn, take out the straight-through microporous Q235 carbon steel mesh template, and obtain a resin / paraffin microcolumn mold after the semi-solidified resin / paraffin mixture is completely cured.

[0063] Pure titanium powder was added into 5% polyvinyl alcohol binder solution, mixed and stirred evenly to obtain pure titanium slurry. The mass fraction of polyvinyl alcohol in the pure titanium slurry was 5.5%. The magnetic stirring time was 10 min and the stirring speed was 400 r / min.

[0064] Pour the evenly mixed pure titanium slurry into the gap of the resin / paraffin microcolumn mold in small amounts and multiple times, then use a scraper to scrape it in one direction multiple times to prevent the pure titanium slurry from mixing with gas and producing tiny holes when flowing into the resin / paraffin microcolumn mold. Then quickly perform ultrasonic vibration for 5 minutes to make the pure titanium slurry completely fill the resin / paraffin microcolumn mold.

[0065] The resin / paraffin microcolumn mold filled with pure titanium slurry was heated from room temperature to 80°C at 2°C / min and kept warm for 2 hours for drying and degreasing. The resin and paraffin in the resin / paraffin microcolumn mold were partially removed. The mold was then heated to 100°C at the same heating rate and kept warm for 1 hour to further remove the resin and paraffin. The mold was then heated to 120°C and kept warm for 2 hours to complete demolding and obtain a straight-through microporous titanium mesh preform.

[0066] The straight-through microporous titanium mesh preform was subjected to low-temperature sintering and high-temperature sintering in sequence under N2 atmosphere and gas flow rate of 1L / min. The low-temperature sintering was carried out from room temperature to 450°C at a rate of 2°C / min and the sintering time was 1h. The high-temperature sintering was carried out from 450°C to 1250°C at a rate of 10°C / min and the sintering time was 2h. It was then cooled to room temperature in the furnace to obtain the straight-through microporous titanium mesh.

[0067] In summary, the present invention provides a straight-through microporous metal mesh and a preparation method thereof, which combines the template method with the investment method, utilizes the characteristics of easily separable materials, and adopts powder metallurgy technology to prepare the straight-through microporous metal mesh. The advantages of the present invention are that the shape and size of the straight-through microporous metal mesh, the form of the holes, the aperture size, the hole wall size and the hole distribution density can be accurately controlled, the equipment investment is small, the operation is simple, the material utilization rate and production efficiency are high, the production cost is low, and it is easy to realize automated mass production; the straight-through microporous metal mesh has high internal and surface quality, good hole size accuracy, excellent performance, a variety of varieties and specifications, and a wide range of applications. It is particularly suitable for the preparation of straight-through microporous metal meshes with ultra-thin hole walls, thin thickness, variable thickness, special-shaped micropores, special-shaped structures, non-periodic hole distribution or layered composites, and reinforced composites.

[0068] The above are only specific embodiments of the present invention, but the protection of the present invention is not limited thereto. Any equivalent changes or substitutions of the features of the present technical solution that can be thought of by a person skilled in the art are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A method for preparing a straight-through microporous metal mesh, characterized in that: The steps include: S1, preparation of micro-column mold: using a straight-through microporous mesh template to imprint or cut the easily separable material, and separating the two after solidification and forming, to obtain a micro-column mold whose horizontal cross section is precisely matched with the straight-through microporous mesh template; S2, metal slurry preparation: mixing the binder solution and the metal powder and stirring them evenly to obtain metal slurry; S3, metal blank preparation: pouring the metal slurry into the gap of the microcolumn mold, and then pressing and leveling to obtain a metal blank; S4, drying and demoulding: drying and degreasing the integral part composed of the metal blank and the micro-column mold, and then separating the two to achieve demoulding, so as to obtain a straight-through microporous metal mesh preform; S5, sintering: sintering the straight microporous metal mesh preform in a protective gas atmosphere for the first time and the second time in sequence, and then cooling the preform to room temperature in a furnace to obtain the straight microporous metal mesh.

2. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: In S1, the material of the straight-through microporous mesh template is one of metal material, ceramic material, polymer material or composite material; Wherein, there are no impurities in the pores of the straight-through microporous mesh template.

3. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: In S1, the easily separable material is at least one of a resin, paraffin or glass that is easily melted, easily decomposed or easily softened after heating; Wherein, the resin is a polymer material with a low melting point and easily softened or decomposed upon heating; Wherein, the paraffin wax is at least one of polyethylene wax, polytetrafluoroethylene wax, microcrystalline wax or semi-microcrystalline wax having a melting point of 60-120°C; Wherein, the softening point of the glass is lower than the melting point of the metal material used for the straight-through microporous metal mesh.

4. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: In S2, the binder is at least one of polyvinyl alcohol, epoxy resin, ethylene-vinyl acetate copolymer, stearic acid, polyoxymethylene or polyethyleneimine; wherein the mass fraction of the binder in the metal slurry is 3%-15%; The metal powder is at least one of pure metal powder, alloy powder, reinforcement and mixed powder composed of pure metal or alloy.

5. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: In S2, the stirring method is at least one of magnetic stirring, ultrasonic stirring or mechanical stirring; Wherein, the stirring speed of the magnetic stirring is 200-1000r / min, and the stirring time is 10-40min.

6. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: In S3, the metal slurry is poured into the microcolumn mold and then pressed or leveled; Wherein, the leveling is at least one of scraping with a scraper, cutting with a cutter, ultrasonic vibration or pressing with a pad.

7. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: In S4, the heating temperature of the drying and degreasing is increased from room temperature to 60-130°C at 0.5-3°C / min, and the drying time is 2-5h; the heating temperature of the demoulding is increased from room temperature to 60-400°C at 2-5°C / min, and the insulation time is 1-5h.

8. The method for preparing a straight microporous metal mesh according to claim 1, characterized in that: In S5, the protective gas is at least one of nitrogen, reducing gas or inert gas; Among them, the sintering temperature of the first sintering in S5 is increased from room temperature to 200-480°C at 0.5-5°C / min, and the sintering time is 1-5h; the sintering temperature of the second sintering is increased from the highest sintering temperature of the first sintering to 500-1500°C at 5-10°C / min, and the sintering time is 0.5-5h.

9. The method for preparing a straight through microporous metal mesh according to claim 1, characterized in that: The method also includes surface treatment of the straight-through microporous metal mesh.

10. A straight-through microporous metal mesh, characterized in that: The straight-through microporous metal mesh is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Ultrathin diamond dicing blade with microporous structure and preparation method of ultrathin diamond dicing blade

    CN120984885A

  • An ultrathin diamond dicing blade with a microporous structure and a preparation method thereof