Solid wood preservative as well as preparation method and application thereof
Nanoscale zinc borate solid wood preservatives are prepared by combining zinc acetate, borax and surfactants, which solves the problems of odor residue and mechanical properties of existing wood preservatives, achieves effective inhibition of white rot, brown rot fungi and termites, and improves Compressive strength and anti-corrosion properties of wood.
Patent Information
- Application Number
- CN202410966921.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing copper-based ACQ wood preservative has problems such as odor residue, wood color change, and poor resistance to copper fungi during use. It also has adverse effects on the mechanical properties of the wood, making it difficult to effectively prevent termite infestation.
A combination of zinc acetate, borax and surfactants (such as didecyldimethylammonium chloride, polyethylene glycol or sodium stearate) is used to prepare nanoscale zinc borate solid wood preservatives through metathesis reaction to improve its performance in wood. dispersion and anti-corrosion properties.
Significantly inhibits the attack of white rot, brown rot fungi and termites, improves the compressive strength and dimensional stability of wood, reduces the loss of preservative components, enhances anti-corrosion and anti-termite properties, and improves mechanical properties.
Smart Images

Figure CN118721349A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wood preservatives, and in particular to a solid wood preservative and a preparation method and application thereof. Background Art
[0002] Wood is extremely vulnerable to microorganisms and insects (termites) during storage, transportation, processing and use. Microorganisms can destroy the cell walls of wood, and insects such as termites can also feed on the lignin inside the wood, accelerating the decay of the wood, causing holes, mold, decay, color change, etc., and ultimately causing a significant reduction in mechanical properties, seriously affecting the service life of the wood, and even causing a series of safety accidents.
[0003] In order to prevent wood from corroding, wood products are usually placed in a ventilated and dry environment. However, the use of wood products cannot be completely avoided in high temperature, high humidity and low temperature areas. Therefore, wood preservatives are often used to extend the service life of wood and reduce the cultural and economic losses caused by wood decay. At present, copper-based ACQ wood preservatives are mostly used to treat wood, but the use of this preservative not only has problems such as odor residue, change of wood color and poor effect on copper-resistant fungi, but also has an adverse effect on the mechanical properties of wood, so it is necessary to find new wood preservatives. Summary of the invention
[0004] The purpose of the present invention is to provide a wood preservative and a preparation method and application thereof to achieve wood antiseptic properties.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] A solid wood preservative, comprising the following raw materials in parts by mass:
[0007] Zinc acetate 35.2~36.1 parts
[0008] Borax 61.2~62.7 parts
[0009] 1.2 to 3.6 parts of surfactant;
[0010] The surfactant comprises didecyldimethylammonium chloride, polyethylene glycol or sodium stearate.
[0011] The present invention provides a method for preparing the solid wood preservative, comprising the following steps:
[0012] 1) mixing zinc acetate, a surfactant and water to obtain a first mixed solution;
[0013] 2) mixing borax and water to obtain a second mixed solution;
[0014] 3) The first mixed solution and the second mixed solution are mixed to undergo double decomposition reaction, and the solid wood preservative is obtained by drying.
[0015] Optionally, when preparing the solid wood preservative, the mixing temperature in step 1) is 65-75° C.; and the mass fraction of zinc acetate in the first mixed solution is 2.1-2.2%.
[0016] Optionally, when preparing the solid wood preservative, the mixing temperature in step 2) is 65-75° C.; and the mass fraction of borax in the second mixed solution is 2.4-2.5%.
[0017] Optionally, when preparing the solid wood preservative, the temperature of the double decomposition reaction in step 3) is 65 to 75° C. and the time is 12 to 36 hours.
[0018] The invention also provides application of the solid wood preservative in wood preservation.
[0019] The wood preservative provided by the present invention contains nano-sized zinc borate, which has a small particle size and can better enter and disperse inside the wood, and has a relatively obvious inhibitory effect on white rot and brown rot fungi, and the treated preservative wood has strong anticorrosion and insect resistance. The surfactant can change the surface morphology and phase composition of nano zinc borate, improve the compatibility of nano zinc borate with water, improve its impregnation performance, and reduce the loss of preservative components, thereby strengthening its anticorrosion and anti-termite performance.
[0020] The wood preservative prepared by the invention promotes the compressive strength parallel to the grain and the dimensional stability, and improves the problem of high loss of the current borate wood preservatives. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The XRD patterns of the solid wood preservatives prepared in Example 1(a), Example 2(b), Example 3(c) and Comparative Example 1(d);
[0022] Figure 2 The SEM images of the solid wood preservatives prepared in Example 1(a), Example 2(b), Example 3(c) and Comparative Example 1(d) are shown. DETAILED DESCRIPTION
[0023] The present invention provides a solid wood preservative, which comprises the following raw materials in parts by mass:
[0024] Zinc acetate 35.2~36.1 parts
[0025] Borax 61.2~62.7 parts
[0026] 1.2 to 3.6 parts of surfactant;
[0027] The surfactant comprises didecyldimethylammonium chloride, polyethylene glycol or sodium stearate.
[0028] In the present invention, the weight fraction of zinc acetate is preferably 35.6 parts.
[0029] In the present invention, the mass fraction of the borax is preferably 62.0 parts; the borax is preferably sodium tetraborate decahydrate.
[0030] In the present invention, the amount of the surfactant is preferably 2.4 parts.
[0031] The present invention provides a method for preparing the solid wood preservative, comprising the following steps:
[0032] 1) mixing zinc acetate, a surfactant and water to obtain a first mixed solution;
[0033] 2) mixing borax and water to obtain a second mixed solution;
[0034] 3) The first mixed solution and the second mixed solution are mixed to undergo double decomposition reaction, and the solid wood preservative is obtained by drying.
[0035] In the present invention, when preparing a solid wood preservative, the mixing temperature in step 1) is preferably 65-75° C., more preferably 70-72° C.; the mass fraction of zinc acetate in the first mixed solution is preferably 2.1-2.2%, more preferably 2.1-2.15%.
[0036] In the present invention, when preparing a solid wood preservative, the mixing temperature in step 2) is preferably 65-75° C., more preferably 70-72° C.; the mass fraction of borax in the second mixed solution is preferably 2.4-2.5%, more preferably 2.4-2.45%.
[0037] In the present invention, when preparing the solid wood preservative, the temperature of the double decomposition reaction in step 3) is preferably 65-75° C., more preferably 70-72° C., and the time is preferably 12-36 h, more preferably 24-30 h.
[0038] In the present invention, when preparing the solid wood preservative, the mixing in step 3) is preferably stirred for 30 minutes, the stirring rate is preferably 300 r / min, and the temperature is preferably 70°C.
[0039] In the present invention, when preparing the solid wood preservative, after the double decomposition reaction is completed, washing is preferably performed, and the washing solution is preferably anhydrous ethanol or deionized water;
[0040] The drying conditions are not particularly limited, and any conditions that can achieve drying are acceptable.
[0041] The invention also provides application of the solid wood preservative in wood preservation.
[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] Example 1
[0044] 2.1 parts of zinc acetate, 0.15 parts of didecyldimethylammonium chloride and 97.75 parts of water are mixed, wherein the mass fraction of zinc acetate is 2.1%, and the mixture is heated to 70° C. to obtain a first mixed solution;
[0045] 2.4 parts of borax (sodium tetraborate decahydrate) are mixed with 97.6 parts of water, wherein the mass fraction of borax in the mixture is 2.4%, and the mixture is heated to 70° C. to obtain a second mixed solution;
[0046] The obtained first mixed solution and the second mixed solution are mixed in a volume ratio of 2:3; stirred at a stirring rate of 300 r / min at 70°C for 30 minutes, and then reacted at a constant temperature of 70°C for 24 hours. After the reaction is completed, washed with anhydrous ethanol and deionized water for several times in sequence, centrifuged, and vacuum dried at 45°C to obtain the solid wood preservative.
[0047] Example 2
[0048] 2.1 parts of zinc acetate, 0.15 parts of polyethylene glycol (polymerization degree of 300) and 97.75 parts of water are mixed, wherein the mass fraction of zinc acetate is 2.1%, and the mixture is kept warm to 70° C. to obtain a first mixed solution;
[0049] 2.4 parts of borax (sodium tetraborate decahydrate) are mixed with 97.6 parts of water, wherein the mass fraction of borax in the mixture is 2.4%, and the mixture is heated to 70° C. to obtain a second mixed solution;
[0050] The obtained first mixed solution and the second mixed solution are mixed in a volume ratio of 2:3; stirred at a stirring rate of 300 r / min at 70°C for 30 minutes, and then reacted at a constant temperature of 70°C for 24 hours. After the reaction is completed, the mixture is washed several times with anhydrous ethanol and deionized water in sequence, centrifuged, and vacuum dried at 45°C to obtain the solid wood preservative.
[0051] Example 3
[0052] 2.1 parts of zinc acetate, 0.15 parts of sodium stearate and 97.75 parts of water are mixed, wherein the mass fraction of zinc acetate is 2.1%, and the mixture is kept at 70° C. to obtain a first mixed solution;
[0053] 2.4 parts of borax (sodium tetraborate decahydrate) are mixed with 97.6 parts of water, wherein the mass fraction of borax in the mixture is 2.4%, and the mixture is heated to 70° C. to obtain a second mixed solution;
[0054] The obtained first mixed solution and the second mixed solution are mixed in a volume ratio of 2:3; stirred at a stirring rate of 300 r / min at 70°C for 30 minutes, and then reacted at a constant temperature of 70°C for 24 hours. After the reaction is completed, the mixture is washed several times with anhydrous ethanol and deionized water in sequence, centrifuged, and vacuum dried at 45°C to obtain the solid wood preservative.
[0055] Comparative Example 1
[0056] 2.1 parts of zinc acetate are mixed with 97.9 parts of water, wherein the mass fraction of zinc acetate is 2.1%, and the mixture is heated to 70° C. to obtain a first mixed solution;
[0057] 2.4 parts of borax are mixed with 97.6 parts of water, wherein the mass fraction of borax in the mixture is 2.4%, and the mixture is heated to 70° C. to obtain a second mixed solution;
[0058] The obtained first mixed solution and the second mixed solution are mixed in a volume ratio of 2:3; stirred at a stirring rate of 300 r / min at 70°C for 30 minutes, and then reacted at a constant temperature of 70°C for 24 hours. After the reaction is completed, washed several times with anhydrous ethanol and deionized water in sequence, centrifuged, and vacuum dried at 45°C to obtain the wood preservative.
[0059] Experimental example
[0060] The nano wood preservatives prepared in Examples 1 to 3 and Comparative Example 1 were subjected to ICP testing, and the results are shown in Table 1;
[0061] Table 1 ICP results of wood preservatives prepared in Examples 1 to 3 and Comparative Example 1
[0062] project Example 1 Example 2 Example 3 Comparative Example 1 Boron content / % 2.95 4.14 3.99 9.88 Zinc content / % 37.41 63.97 52.99 48.18
[0063] From Table 1, it can be found that the prepared product contains two elements, boron and zinc, and the addition of different modifiers has an effect on the content of boron and zinc in the product;
[0064] The nano wood preservatives prepared in Example 1 (a), Example 2 (b), Example 3 (c) and Comparative Example 1 (d) were subjected to XRD tests. The results are as follows: Figure 1 As shown;
[0065] pass Figure 1It can be found that the modified products are all composed of several hydrated zinc borates. The addition and type of surfactants will affect the phase composition of the products. The phase compositions of the products modified by didecyl dimethyl ammonium chloride and PEG-300 are basically the same.
[0066] The nano wood preservatives prepared in Example 1 (a), Example 2 (b), Example 3 (c) and Comparative Example 1 (d) were subjected to SEM testing. The results are as follows: Figure 2 As shown;
[0067] pass Figure 2 It can be found that the modified products of didecyl dimethyl ammonium chloride and PEG-300 are roughly spherical in shape, and the spheres are stacked by thin sheet structures, while the microscopic morphology of the modified product of sodium stearate is flaky and the particle size is relatively small.
[0068] Therefore, Table 1 and Figure 1 , Figure 2 The comprehensive results show that the main component of the wood preservative is zinc borate, which reaches nanometer level.
[0069] The wood preservatives prepared in Examples 1 to 3 of the present invention and Comparative Example 1 were prepared into a suspension with a mass fraction of 2% for wood preservation, and the compressive strength along the grain of wood treated with the wood preservatives and untreated wood at a moisture content of 12% was tested with reference to GB / T 1935-2009; the dimensional stability (in terms of volume expansion coefficient) of wood treated with the preservatives and untreated wood was tested with reference to LY / T 2490-2015 using the method described in GB / T 4822-2015; the anti-loss property of the wood preservatives prepared in Examples 1 to 3 of the present invention and Comparative Example 1 was tested as the fixation rate with reference to GB / T29905-2013;
[0070] The results are shown in Table 2.
[0071] Table 2 Basic properties of wood preservatives prepared in Examples 1 to 3 and Comparative Example 1
[0072] project Example 1 Example 2 Example 3 Comparative Example Not treated with preservatives Compressive strength along the grain / MPa 15.3 15.1 14.6 15.0 14.3 Volume expansion coefficient / % 7.22 7.82 7.12 7.55 8.70 Fixation rate / % 70.18 69.16 68.69 54.17 ——
[0073] It can be seen from Table 2 that the nano wood preservatives prepared in Examples 1 to 3 of the present invention can improve the compressive strength along the grain, reduce the volume expansion coefficient, have a high fixation rate after the loss test, and can improve the basic properties of wood.
[0074] The anti-corrosion and anti-termite performance of the above-mentioned anti-corrosion treated wood and the un-anti-corrosion treated wood were tested in accordance with LY / T 1283-2011 and GB / T18260-2015, and compared with the un-anti-corrosion treated wood. The results are shown in Table 3.
[0075] Table 3 Comparison of anticorrosion and anti-termite performance of wood treated with wood preservatives prepared in Examples 1 to 3 and Comparative Example 1 and wood not treated with preservatives
[0076] project Example 1 Example 2 Example 3 Comparative Example 1 Not treated with preservatives White rot mass loss / % 4.20 4.47 5.18 9.98 20.71 Brown rot mass loss / % 6.55 3.33 2.88 7.61 24.50 Termite mass loss / % 7.30 4.20 11.20 11.40 23.00
[0077] It can be seen from Table 3 that the nano wood preservatives prepared in Examples 1 to 3 of the present invention can effectively reduce the mass loss of white rot, brown rot and termites, can significantly inhibit the erosion of decay fungi and termites, and have good anti-corrosion and anti-termite performance.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A solid wood preservative, characterized in that: The following raw materials are included in parts by mass: Zinc acetate 35.2~36.1 parts Borax 61.2~62.7 parts 1.2 to 3.6 parts of surfactant; The surfactant comprises didecyldimethylammonium chloride, polyethylene glycol or sodium stearate.
2. The method for preparing the solid wood preservative according to claim 1, characterized in that: The following steps are involved: 1) mixing zinc acetate, a surfactant and water to obtain a first mixed solution; 2) mixing borax and water to obtain a second mixed solution; 3) The first mixed solution and the second mixed solution are mixed to undergo double decomposition reaction, and the solid wood preservative is obtained by drying.
3. The preparation method according to claim 2, characterized in that: Step 1) The mixing temperature is 65-75° C.; the mass fraction of zinc acetate in the first mixed solution is 2.1-2.2%.
4. The preparation method according to claim 2, characterized in that: Step 2) The mixing temperature is 65-75° C.; the mass fraction of borax in the second mixed solution is 2.4-2.5%.
5. The preparation method according to claim 2, characterized in that: Step 3) The temperature of the double decomposition reaction is 65-75° C. and the time is 12-36 hours.
6. Use of the solid wood preservative according to claim 1 or the solid wood preservative prepared by the preparation method according to any one of claims 2 to 5 in wood preservation.
Citation Information
Patent Citations
Wood preservative composition, process for treating wood with the same, and wood treated with the same
CA2128983A1
Novel method for in situ preparing nano-zinc borate crystal whisker in normal pressure normal pressure liquid phase
CN101298694A
Method for preparing superfine zinc borate
CN102060306A
New hydrothermal synthesis method of zinc borate whisker
CN102226299A
Method for preparing sub-micron zinc borate by using glycerol
CN102502680A