Preparation method of polytetrafluoroethylene sealing ring with double sealing lips

By drying the semi-finished product when preparing the polytetrafluoroethylene double sealing lip seal ring, and combining the process flow of the hot press and high-temperature furnace, the problem of bubbles and holes caused by moisture residue during the sintering process is solved, and the density of the product is improved. and strength, enhancing the durability and reliability of the seal.

CN118721831APending Publication Date: 2024-10-01XIAN KERIS NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095947.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When preparing a polytetrafluoroethylene double sealing lip seal ring in the prior art, residual moisture in the preform during the sintering process causes bubbles and holes inside the product, affecting product quality.

Method used

Before sintering, the semi-finished products are dried to reduce the moisture content and sintered in a high-temperature furnace. A process combining a hot press and a high-temperature furnace is used, including pretreatment, hot press preforming, sintering, processing and reprocessing to ensure The density and strength of the product.

Benefits of technology

The drying process reduces the expansion and deformation during the sintering process, ensures product dimensional accuracy, shortens the sintering time, improves the density and strength of the material, reduces the formation of bubbles and voids, and enhances the durability and reliability of the sealing ring. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721831A_ABST
    Figure CN118721831A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a polytetrafluoroethylene sealing ring with double sealing lips, and relates to the technical field of production of sealing rings. The preparation method of the polytetrafluoroethylene sealing ring with the double sealing lips comprises the following steps: S1, preparing raw materials, and pretreating the raw materials; s2, the raw materials pretreated in the step S1 are put into a hot press to be subjected to hot-pressing preforming; s3, putting a semi-finished product subjected to hot-pressing pre-forming in the step S2 into a high-temperature furnace for sintering; s4, processing a product sintered and molded in the step S3; and S5, reprocessing the processed product, drying the semi-finished product, then sintering, and reducing the moisture content, so that expansion and deformation in the sintering process are reduced, the dimensional accuracy of the final product is ensured, meanwhile, the sintering time can be shortened, the sintering efficiency can be improved, and the formation of bubbles and gaps is reduced, so that the microstructure of the preformed part is improved, and the product quality is improved. A more uniform crystal structure is formed in the sintering process, and the compactness and strength of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing ring production, in particular to a method for preparing a polytetrafluoroethylene double sealing lip sealing ring. Background Art

[0002] The selection of sealing ring materials is of great significance to its sealing performance and service life. The performance of the material directly affects the performance of the sealing ring. With the increasing development of products and the expansion of application fields, higher requirements are placed on the application of sealing products. As a result, the requirements for sealing rings are getting higher and higher. A single lip (or a pair of lips) can no longer adapt to the current form. Therefore, the double sealing lip sealing structure is a new structure designed for this demand. Polytetrafluoroethylene is a very excellent engineering plastic with excellent chemical resistance, low friction coefficient and good temperature resistance. When polytetrafluoroethylene is used to make a sealing ring with double sealing lips, it can resist the erosion of most acids, alkalis, solvents and other chemicals, thereby maintaining its performance for a long time in a harsh chemical environment. When using the existing preparation method to produce polytetrafluoroethylene double sealing lip sealing rings, it is easy to have bubbles and holes inside the product due to residual moisture in the preform during the sintering process, affecting the product quality. For example, when using a rubber sealing ring preparation method disclosed in the publication number CN112894953B to prepare a polytetrafluoroethylene double sealing lip sealing ring, it is easy to have bubbles and holes inside the product due to insufficient removal of residual moisture in the preform, affecting the product quality. Therefore, a preparation method for a polytetrafluoroethylene double sealing lip sealing ring is proposed. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a method for preparing a polytetrafluoroethylene double sealing lip sealing ring, which solves the problem that when producing a polytetrafluoroethylene double sealing lip sealing ring in the prior art, bubbles and holes may appear inside the product due to residual moisture in the preform during the sintering process, thereby affecting the product quality.

[0004] To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for preparing a polytetrafluoroethylene double sealing lip sealing ring comprises the following steps:

[0005] S1, preparing raw materials and pre-treating the raw materials;

[0006] S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming;

[0007] S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering;

[0008] S4, processing the product sintered in step S3;

[0009] S5, reprocessing the product processed in step S4;

[0010] S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

[0011] Preferably, the raw materials include PTFE powder, glass fiber and carbon fiber, and the weight proportions of the raw materials are 30-50 of PTFE powder, 5-12 of glass fiber and 4-11 of carbon fiber.

[0012] Preferably, the temperature of the hot press during hot pressing is between 150° C. and 230° C., the pressure of the hot press is between 12 MPa and 19 MPa, and the heating time of the hot press is between 7 min and 18 min.

[0013] Preferably, the high temperature furnace is a continuous tunnel furnace, the heating rate of the high temperature furnace is between 1°C / min-3°C / min, the insulation time of the high temperature furnace is between 10min-20min, and the preheating temperature of the high temperature furnace is between 260°C-300°C.

[0014] Preferably, the sintering temperature of the high temperature furnace is between 370° C. and 385° C., the conveying speed of the high temperature furnace is between 0.5 m / min and 0.8 m / min, and the cooling rate of the high temperature furnace is between 3° C. and 4° C. per minute.

[0015] Preferably, the processing in step S4 includes turning, the turning speed is between 9m / min-22m / min, the cutting depth of the turning is between 0.1mm-0.3mm, and the reprocessing in step S5 includes polishing, the polishing pressure is between 0.4kg / m 3 -1.1kg / m 3 During polishing, the rotation speed of the polishing wheel is between 900rpm and 1600rpm.

[0016] Preferably, in step S3, the semi-finished product is dried before sintering, the drying temperature is between 65°C and 80°C, the drying time is between 1h and 2h, and after drying, the semi-finished product is placed on a matching supporting component, and then the supporting component is placed in a high-temperature furnace for sintering.

[0017] Preferably, in step S3, the semi-finished product is dried, tested, cooled to room temperature, and then placed on a matching support component and placed in a high-temperature furnace for sintering, and the size of the support component is adjustable.

[0018] The present invention provides a method for preparing a polytetrafluoroethylene double sealing lip sealing ring. Compared with the prior art, it has the following beneficial effects:

[0019] (1) The method for preparing a polytetrafluoroethylene double sealing lip sealing ring reduces the moisture content by drying the semi-finished product before sintering, thereby reducing expansion and deformation during the sintering process, ensuring the dimensional accuracy of the final product, and at the same time shortening the sintering time and improving the sintering efficiency. Reducing the formation of bubbles and voids helps to improve the microstructure of the preform, so that it forms a more uniform crystal structure during the sintering process, thereby improving the density and strength of the material.

[0020] (2) The method for preparing a polytetrafluoroethylene double sealing lip sealing ring can maintain stability within a temperature range of -200°C to 260°C by using polytetrafluoroethylene to prepare a double sealing lip sealing ring. This wide temperature range enables the sealing ring to work under extreme temperature conditions, whether in extremely cold or high temperature environments, increasing the application scenarios of the sealing ring and having a wide range of application potential. In addition, due to its very low friction coefficient, it can reduce friction between moving parts and extend its service life. The double sealing lip design can provide double protection. Even if one of the lips fails, the other lip can still maintain the sealing effect, thereby improving the reliability and safety of the sealing ring and reducing the risk of leakage. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] See also Figure 1 , the present invention provides the following technical solutions:

[0024] Embodiment 1: A method for preparing a polytetrafluoroethylene double sealing lip sealing ring, comprising the following steps:

[0025] S1, preparing raw materials and pre-treating the raw materials;

[0026] S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming;

[0027] S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering;

[0028] S4, processing the product sintered in step S3;

[0029] S5, reprocessing the product processed in step S4;

[0030] S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

[0031] The raw materials include PTFE powder and glass fiber, and the weight proportion of the raw materials is 30 parts of PTFE powder and 5 parts of glass fiber.

[0032] The temperature during hot pressing of the hot press is 150°C, the pressure of the hot press is 12MPa, and the heating time of the hot press is 7min.

[0033] The high temperature furnace is a continuous tunnel furnace. The heating rate of the high temperature furnace is 1°C / min, the insulation time of the high temperature furnace is 10min, the preheating temperature of the high temperature furnace is 260°C, the sintering temperature of the high temperature furnace is 370°C, the conveying speed of the high temperature furnace is 0.5m / min, and the cooling rate of the high temperature furnace is 3°C / min.

[0034] The processing in step S4 includes turning, the turning speed is 9m / min, the cutting depth of turning is 0.1mm, and the reprocessing in step S5 includes polishing, the polishing pressure is 0.4kg / m 3 , the polishing wheel speed during polishing is 900rpm.

[0035] In step S3, the semi-finished product is dried before sintering, the drying temperature is 65°C, the drying time is 1 hour, and after drying, the semi-finished product is placed on a matching support component, and then the support component is placed in a high-temperature furnace for sintering.

[0036] Furthermore, in step S3, after the semi-finished product is dried, it is tested and cooled to room temperature before being placed on a matching support component and placed in a high-temperature furnace for sintering. The size of the support component is designed to be adjustable.

[0037] Embodiment 2: A method for preparing a polytetrafluoroethylene double sealing lip sealing ring, comprising the following steps:

[0038] S1, preparing raw materials and pre-treating the raw materials;

[0039] S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming;

[0040] S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering;

[0041] S4, processing the product sintered in step S3;

[0042] S5, reprocessing the product processed in step S4;

[0043] S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

[0044] The raw materials include PTFE powder and glass fiber, and the weight proportion of the raw materials is 40 parts of PTFE powder and 8 parts of glass fiber.

[0045] The temperature during hot pressing of the hot press is 170°C, the pressure of the hot press is 15MPa, and the heating time of the hot press is 9min.

[0046] The high temperature furnace is a continuous tunnel furnace. The heating rate of the high temperature furnace is 2°C / min, the insulation time of the high temperature furnace is 16min, the preheating temperature of the high temperature furnace is 275°C, the sintering temperature of the high temperature furnace is 375°C, the conveying speed of the high temperature furnace is 0.7m / min, and the cooling rate of the high temperature furnace is 3.5°C / min.

[0047] The processing in step S4 includes turning, the turning speed is 14m / min, the cutting depth of turning is 0.2mm, and the reprocessing in step S5 includes polishing, the polishing pressure is 0.7kg / m 3 , the polishing wheel speed during polishing is 980rpm.

[0048] In step S3, the semi-finished product is dried before sintering. The drying temperature is 67° C. and the drying time is 1.5 hours. After drying, the semi-finished product is placed on a matching support component, and then the support component is placed in a high-temperature furnace for sintering.

[0049] Furthermore, in step S3, after the semi-finished product is dried, it is tested and cooled to room temperature before being placed on a matching support component and placed in a high-temperature furnace for sintering. The size of the support component is designed to be adjustable.

[0050] Embodiment 3: A method for preparing a polytetrafluoroethylene double sealing lip sealing ring, comprising the following steps:

[0051] S1, preparing raw materials and pre-treating the raw materials;

[0052] S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming;

[0053] S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering;

[0054] S4, processing the product sintered in step S3;

[0055] S5, reprocessing the product processed in step S4;

[0056] S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

[0057] The raw materials include PTFE powder and glass fiber, and the weight proportion of the raw materials is 50 parts of PTFE powder and 12 parts of glass fiber.

[0058] The temperature during hot pressing of the hot press is 200°C, the pressure of the hot press is 14MPa, and the heating time of the hot press is 11min.

[0059] The high temperature furnace is a continuous tunnel furnace. The heating rate of the high temperature furnace is 1.5℃ / min, the insulation time of the high temperature furnace is 16min, the preheating temperature of the high temperature furnace is 290℃, the sintering temperature of the high temperature furnace is 380℃, the conveying speed of the high temperature furnace is 0.8m / min, and the cooling rate of the high temperature furnace is 3.5℃ / min.

[0060] The processing in step S4 includes turning, the turning speed is 9m / min, the cutting depth of turning is 0.25mm, and the reprocessing in step S5 includes polishing, the polishing pressure is 0.6kg / m 3 , the polishing wheel speed during polishing is 1100rpm.

[0061] In step S3, the semi-finished product is dried before sintering, the drying temperature is 75°C, the drying time is 1.2 hours, and after drying, the semi-finished product is placed on a matching support component, and then the support component is placed in a high-temperature furnace for sintering.

[0062] Furthermore, in step S3, after the semi-finished product is dried, it is tested and cooled to room temperature before being placed on a matching support component and placed in a high-temperature furnace for sintering. The size of the support component is designed to be adjustable.

[0063] Embodiment 4: A method for preparing a polytetrafluoroethylene double sealing lip sealing ring, comprising the following steps:

[0064] S1, preparing raw materials and pre-treating the raw materials;

[0065] S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming;

[0066] S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering;

[0067] S4, processing the product sintered in step S3;

[0068] S5, reprocessing the product processed in step S4;

[0069] S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

[0070] The raw materials include PTFE powder and carbon fiber, and the weight proportions of the raw materials are 50 parts of PTFE powder and 11 parts of carbon fiber.

[0071] The temperature during hot pressing of the hot press is 210°C, the pressure of the hot press is 13MPa, and the heating time of the hot press is 10min.

[0072] The high temperature furnace is a continuous tunnel furnace. The heating rate of the high temperature furnace is 2°C / min, the insulation time of the high temperature furnace is 15min, the preheating temperature of the high temperature furnace is 295°C, the sintering temperature of the high temperature furnace is 385°C, the conveying speed of the high temperature furnace is 0.7m / min, and the cooling rate of the high temperature furnace is 3.8°C / min.

[0073] The processing in step S4 includes turning, the turning speed is 9m / min, the cutting depth of turning is 0.3mm, and the reprocessing in step S5 includes polishing, the polishing pressure is 0.9kg / m 3 , the polishing wheel speed during polishing is 1300rpm.

[0074] In step S3, the semi-finished product is dried before sintering, the drying temperature is 78°C, the drying time is 1.8 hours, and after drying, the semi-finished product is placed on a matching support component, and then the support component is placed in a high-temperature furnace for sintering.

[0075] Furthermore, in step S3, after the semi-finished product is dried, it is tested and cooled to room temperature before being placed on a matching support component and placed in a high-temperature furnace for sintering. The size of the support component is designed to be adjustable.

[0076] Embodiment 5: A method for preparing a polytetrafluoroethylene double sealing lip sealing ring, comprising the following steps:

[0077] S1, preparing raw materials and pre-treating the raw materials;

[0078] S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming;

[0079] S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering;

[0080] S4, processing the product sintered in step S3;

[0081] S5, reprocessing the product processed in step S4;

[0082] S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

[0083] The raw materials include PTFE powder and carbon fiber, and the weight proportion of the raw materials is 45 for PTFE powder and 8 for carbon fiber.

[0084] The temperature during hot pressing of the hot press is 230°C, the pressure of the hot press is 19 MPa, and the heating time of the hot press is 18 min.

[0085] The high temperature furnace is a continuous tunnel furnace. The heating rate of the high temperature furnace is 2°C / min, the insulation time of the high temperature furnace is 18min, the preheating temperature of the high temperature furnace is 300°C, the sintering temperature of the high temperature furnace is 372°C, the conveying speed of the high temperature furnace is 0.8m / min, and the cooling rate of the high temperature furnace is 4°C / min.

[0086] The processing in step S4 includes turning, the turning speed is 22m / min, the cutting depth of turning is 0.3mm, and the reprocessing in step S5 includes polishing, the polishing pressure is 1.1kg / m 3 , the polishing wheel speed during polishing is 1600rpm.

[0087] In step S3, the semi-finished product is dried before sintering, the drying temperature is 80°C, the drying time is 2 hours, and after drying, the semi-finished product is placed on a matching support component, and then the support component is placed in a high-temperature furnace for sintering.

[0088] Furthermore, in step S3, after the semi-finished product is dried, it is tested and cooled to room temperature before being placed on a matching support component and placed in a high-temperature furnace for sintering. The size of the support component is designed to be adjustable.

[0089] After C is performed according to all the schemes in the above embodiments,

[0090] The optimal high temperature furnace heating rate is 2°C / min;

[0091] The cooling rate of the optimal high-temperature furnace is 3.5°C / min;

[0092] The optimal drying temperature is 75°C;

[0093] The optimal drying time is 1.2h.

[0094] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0095] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0096] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a polytetrafluoroethylene double sealing lip sealing ring, characterized in that: The following steps are involved: S1, preparing raw materials and pre-treating the raw materials; S2, placing the raw material pretreated in step S1 into a hot press for hot pressing preforming; S3, placing the semi-finished product preformed by hot pressing in step S2 into a high temperature furnace for sintering; S4, processing the product sintered in step S3; S5, reprocessing the product processed in step S4; S6. The products that have been reprocessed in step S5 are sampled and inspected, and then packaged and stored.

2. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 1, characterized in that: The raw materials include PTFE powder, glass fiber and carbon fiber, and the weight proportions of the raw materials are 30-50 of PTFE powder, 5-12 of glass fiber and 4-11 of carbon fiber.

3. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 1, characterized in that: The temperature of the hot press during hot pressing is between 150° C. and 230° C., the pressure of the hot press is between 12 MPa and 19 MPa, and the heating time of the hot press is between 7 min and 18 min.

4. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 1, characterized in that: The high temperature furnace is a continuous tunnel furnace, the heating rate of the high temperature furnace is between 1°C / min-3°C / min, the insulation time of the high temperature furnace is between 10min-20min, and the preheating temperature of the high temperature furnace is between 260°C-300°C.

5. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 4, characterized in that: The sintering temperature of the high temperature furnace is between 370° C. and 385° C., the conveying speed of the high temperature furnace is between 0.5 m / min and 0.8 m / min, and the cooling rate of the high temperature furnace is between 3° C. and 4° C.

6. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 1, characterized in that: The processing in step S4 includes turning, the turning speed is between 9m / min-22m / min, the cutting depth of the turning is between 0.1mm-0.3mm, and the reprocessing in step S5 includes polishing, the polishing pressure is between 0.4kg / m 3 -1.1kg / m 3 During polishing, the rotation speed of the polishing wheel is between 900rpm and 1600rpm.

7. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 1, characterized in that: In step S3, the semi-finished product is dried before sintering, the drying temperature is between 65°C and 80°C, the drying time is between 1h and 2h, and after drying, the semi-finished product is placed on a matching support component, and then the support component is placed in a high-temperature furnace for sintering.

8. The method for preparing a polytetrafluoroethylene double sealing lip sealing ring according to claim 7, characterized in that: In step S3, the semi-finished product is dried, tested, cooled to room temperature, and then placed on a matching support component and placed in a high-temperature furnace for sintering. The size of the support component is adjustable.