Laminate, display device comprising same, and adhesive layer

By optimizing the relationship between the stress reduction rate and thickness of the adhesive layer in the laminate structure, the deficiencies in thermal shock and low-temperature bending of the laminate in the prior art are solved, significantly improving the performance when the front panel side is on the inside. Thermal shock bending and low temperature bending.

CN118721877APending Publication Date: 2024-10-01SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410297611.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing laminates have deficiencies in thermal shock bending and low-temperature bending. Especially when the front panel side is bent inward, the thermal shock bending and low-temperature bending are not ideal.

Method used

A laminated body structure was designed, including a front panel, a first adhesive layer, a polarizer layer, a second adhesive layer, and a back panel. By optimizing the relationship between the stress reduction rate and thickness of the adhesive layer, the first The stress reduction rate of the adhesive layer and the second adhesive layer is 40% or more and 70% or less, and the relationship between the stress reduction rate of the first adhesive layer and the stress reduction rate of the second adhesive layer Meet specific conditions to improve the thermal shock bending and low-temperature bending properties of the laminate.

Benefits of technology

It is realized that when the front panel side is on the inside, the thermal shock bending flexibility and low-temperature bending resistance of the laminate are significantly improved, reducing bubble generation and peeling, and improving durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721877A_ABST
    Figure CN118721877A_ABST
Patent Text Reader

Abstract

Provided is a laminate having excellent thermal shock bendability and low-temperature bendability when bent so that the front plate side is the inner side. This laminate comprises a front panel, a first adhesive layer, a polarizer layer, a second adhesive layer, and a back panel in this order, the stress reduction rate of the first adhesive layer as determined by formula (1) being 40-70%, and the stress reduction rate R1 of the first adhesive layer and the stress reduction rate R2 of the second adhesive layer satisfying the relationship of formula (2). Stress reduction rate = 100-{(RB / RA * 100} (1) R1 < = R2 (2) [In formula (1), RA represents the stress (unit: Pa) when 400% deformation is initially applied to the adhesive layer at-20 DEG C after the start of the repeated deformation application test, and RB represents the stress (unit: Pa) when 400% deformation is finally applied at 60 DEG C in the tenth cycle of the repeated deformation application test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminate, a display device including the laminate, and an adhesive layer for a flexible display device. Background Art

[0002] Patent Document 1 describes a laminate including a front plate, a first pressure-sensitive adhesive layer, a polarizer layer, a second pressure-sensitive adhesive layer, and a back plate in this order.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-154308 Summary of the invention

[0006] Problems to be solved by the invention

[0007] Conventional laminates such as those described in Patent Document 1 have good bendability. However, the thermal shock bendability and low-temperature bendability of conventional laminates are not necessarily sufficient, and there is room for improvement.

[0008] In addition, the laminate may be bent with the front panel side facing inward depending on the application. In such applications, the laminate is required to have improved thermal shock bendability and low temperature bendability when bent with the front panel side facing inward.

[0009] Therefore, an object of the present invention is to provide a laminate having excellent thermal shock bendability and low-temperature bendability when bent with the front panel side facing inward, a display device including the laminate, and an adhesive layer for a flexible display device.

[0010] Means for solving problems

[0011] The present invention provides the following laminated body, display device, and adhesive layer.

[0012] [1] A laminate comprising, in sequence, a front panel, a first adhesive layer, a polarizer layer, a second adhesive layer and a back panel, wherein the stress reduction rate of the first adhesive layer calculated using the following formula (1) is greater than 40% and less than 70%, and the stress reduction rate R1 of the first adhesive layer and the stress reduction rate R2 of the second adhesive layer satisfy the relationship of the following formula (2).

[0013] Stress reduction rate = 100-{(RB / RA)×100}...(1)

[0014] R1≤R2...(2)

[0015] [In formula (1), RA represents the stress (unit: Pa) when a 400% deformation is applied to the adhesive layer at -20°C for the first time after the start of the repeated deformation test, and RB represents the stress (unit: Pa) when a 400% deformation is applied to the adhesive layer at 60°C for the last time in the 10th cycle of the repeated deformation test.]

[0016] [Repeated deformation test]

[0017] The repeated deformation test is carried out by the following operation, i.e., an adhesive layer adjusted to a thickness of 150 μm is bonded to a measuring chip of a viscoelasticity measuring device, and 0% deformation and 400% deformation are repeatedly applied under the conditions of no force (Normal Force Free) and a frequency of 1 Hz. The temperature is maintained at -20°C for 2 minutes, and then the temperature is increased to 60°C at a heating rate of 10°C / min and maintained for 2 minutes. This operation is set as one cycle, and the operation is repeated for a total of 10 cycles.

[0018] [2] The laminate according to [1] above, wherein the flexural rigidity of the laminate at a temperature of -20°C is 1000 gf·m or more and 2000 gf·m or less.

[0019] [3] The laminate according to [1] or [2], wherein the thickness of the first adhesive layer and the second adhesive layer are both 10 μm or more and 100 μm or less.

[0020] [4] The laminate according to any one of [1] to [3], wherein the first adhesive layer and the second adhesive layer are both layers formed from an adhesive composition containing a (meth)acrylic polymer.

[0021] [5] The laminate according to [4], wherein the (meth)acrylic polymer contains 20% by mass or more and 30% by mass or less of structural units derived from nitrogen atom-containing monomers based on the total amount of structural units.

[0022] [6] A laminate according to any one of [1] to [5] above, wherein the first adhesive layer is a layer formed by a first adhesive composition comprising a fluorine atom-containing compound, and the content of the fluorine atom-containing compound is 5% by weight or less based on the total solid content of the first adhesive composition.

[0023] [7] The laminate according to any one of [1] to [6], wherein the stress reduction rate R1 of the first adhesive layer and the stress reduction rate R2 of the second adhesive layer satisfy the relationship of the following formula (3).

[0024] 0Pa≤(R2-R1)≤20Pa...(3)

[0025] [8] The laminate according to any one of [1] to [7], wherein the stress reduction rate of the second adhesive layer is 40% to 70%.

[0026] [9] The laminate according to any one of [1] to [8], wherein the thickness T1 of the first adhesive layer and the thickness T2 of the second adhesive layer satisfy the relationship of the following formula (4).

[0027] 0.1≤(T1 / T2)≤4...(4)

[0028]

[10] A display device comprising the laminate according to any one of [1] to [9] above.

[0029]

[11] An adhesive layer disposed between a front panel and a polarizing layer of a flexible display device, wherein the stress reduction rate calculated by the following formula (1) is 40% to 70%.

[0030] Stress reduction rate = 100-{(RB / RA)×100}...(1)

[0031] [In formula (1), RA represents the stress (unit: Pa) when a 400% deformation is applied to the adhesive layer at -20°C for the first time after the start of the repeated deformation test, and RB represents the stress (unit: Pa) when a 400% deformation is applied to the adhesive layer at 60°C for the last time in the 10th cycle of the repeated deformation test.]

[0032] [Repeated deformation test]

[0033] The repeated deformation test is carried out by the following operation, i.e., an adhesive layer adjusted to a thickness of 150 μm is bonded to a measuring chip of a viscoelasticity measuring device, and 0% deformation and 400% deformation are repeatedly applied under the conditions of no force (Normal Force Free) and a frequency of 1 Hz. The temperature is maintained at -20°C for 2 minutes, and then the temperature is increased to 60°C at a heating rate of 10°C / min and maintained for 2 minutes. This operation is set as one cycle, and the operation is repeated for a total of 10 cycles.

[0034] Effects of the Invention

[0035] According to the present invention, it is possible to provide a laminate having excellent thermal shock bendability and low-temperature bendability when bent with the front panel side facing inward, a display device including the laminate, and a pressure-sensitive adhesive layer for a flexible display device. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic cross-sectional view showing one embodiment of the laminated body of the present invention.

[0037] Figure 2 This is a schematic cross-sectional view showing another embodiment of the laminated body of the present invention.

[0038] Description of Reference Numerals

[0039] 100, 200 laminated body, 101 front plate, 102 first adhesive layer, 103 polarizing plate layer, 104 second adhesive layer, 105 back plate, 106 first phase difference layer, 107 second phase difference layer, 108, 109 bonding layers. DETAILED DESCRIPTION

[0040] Hereinafter, a laminated body (hereinafter also simply referred to as a “laminated body”) according to one embodiment of the present invention will be described with reference to the drawings.

[0041] <Laminate>

[0042] Figure 1 1 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention. The laminate 100 sequentially includes a front panel 101, a first adhesive layer 102, a polarizer layer 103, a second adhesive layer 104, and a back panel 105. Hereinafter, the first adhesive layer 102 and the second adhesive layer 104 are sometimes collectively referred to as "adhesive layers".

[0043] The laminate 100 of the present embodiment preferably has a bending stiffness S1 of 1000 gf·m or more and 2000 gf·m or less at -20°C. If the bending stiffness at -20°C is 1000 gf·m or more and 2000 gf·m or less, the laminate 100 becomes a laminate having excellent flexibility and durability as well as moderate hardness. For example, when the laminate 100 is applied to a flexible display, the display can be easily bent even in a low temperature environment. In the present embodiment, the bending stiffness of the laminate 100 is more preferably 1200 gf·m or more and 1800 gf·m or less, and further preferably 1400 gf·m or more and 1600 gf·m or less. It should be noted that the bending stiffness is a value measured according to the method described in the examples.

[0044] The bending rigidity of the laminate 100 can be adjusted to a desired range by controlling the thickness of each layer constituting the laminate 100, the stress reduction rate of the adhesive layer, etc. Specifically, the bending rigidity can be increased by increasing the thickness of the adhesive layer or the stress reduction rate.

[0045] The thickness of the stack 100 varies depending on the function required for the stack and the application of the stack, and is not particularly limited, but is, for example, 30 μm to 1500 μm, preferably 40 μm to 1000 μm, and more preferably 50 μm to 500 μm.

[0046] The top view shape of the stack 100 can be, for example, a square shape, preferably a square shape with long sides and short sides, and more preferably a rectangle. In the case where the shape of the face direction of the stack 100 is a rectangle, the length of the long side can be, for example, 10 mm or more and 1400 mm or less, preferably 50 mm or more and 600 mm or less. The length of the short side can be, for example, 5 mm or more and 800 mm or less, preferably 30 mm or more and 500 mm or less, and more preferably 50 mm or more and 300 mm or less. In each layer constituting the stack, the corners can be R-processed, the ends can be grooved, or the holes can be opened.

[0047] The laminate 100 can be applied to, for example, a display device, etc. The display device is not particularly limited, and examples thereof include an organic electroluminescent (organic EL) display device, an inorganic electroluminescent (inorganic EL) display device, a liquid crystal display device, and an electroluminescent display device (Japanese: electric field light display device). The display device can have a touch panel function. In addition, a display device using the laminate 100 can be used as a flexible display that can be bent or rolled up. The display device is preferably capable of being bent with the front panel 101 side as the inner side. The display device having the laminate 100 of the present embodiment is particularly excellent in thermal shock bendability and low-temperature bendability when being bent with the front panel 101 side as the inner side. However, the laminate 100 can also be bent with the front panel 101 side as the outer side.

[0048] <Adhesive Layer (First Adhesive Layer and Second Adhesive Layer)>

[0049] As described above, the laminated body 100 includes the first adhesive layer 102 and the second adhesive layer 104 .

[0050] In the laminated body 100 , the stress reduction rate of the first adhesive layer 102 is 40% or more and 70% or less. The stress reduction rate is represented by the following formula (1).

[0051] Stress reduction rate = 100-{(RB / RA)×100}...(1)

[0052] In formula (1), RA represents the stress (unit: Pa) when a 400% deformation is initially applied to the adhesive layer at -20°C after the start of the repeated deformation test, and RB represents the stress (unit: Pa) when a 400% deformation is finally applied at 60°C in the 10th cycle of the repeated deformation test.

[0053] In the laminated body 100 , the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the following formula (2).

[0054] R1≤R2...(2)

[0055] The repeated deformation test is performed by bonding an adhesive layer adjusted to a thickness of 150 μm to a measuring chip of a viscoelasticity measuring device, repeatedly applying 0% deformation and 400% deformation under the conditions of no force and a frequency of 1 Hz, and keeping the temperature at -20°C for 2 minutes, then heating to 60°C at a heating rate of 10°C / min and keeping it for 2 minutes, setting this operation as 1 cycle, and repeating this operation for a total of 10 cycles. The above temperature represents the temperature of the adhesive layer. Stress RA and stress RB can be obtained according to the measurement method described in the embodiment column described later.

[0056] When the stress reduction rate of the first adhesive layer 102 is greater than 40% and less than 70%, and the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above-mentioned formula (2), the generation of bubbles in the first adhesive layer 102 can be suppressed in the environment of a thermal shock test (thermal shock bending test) when the laminate 100 is bent with the front panel 101 side facing inside, thereby improving the durability. Specifically, as shown in the embodiments described later, the laminate 100 is wound around a mandrel in such a manner that the front panel 101, which becomes the inner side when bent, is on the inner side. After being placed at -20°C for 2 minutes, it is placed at 25°C for 2 minutes and then at 60°C for 2 minutes. This is set as one cycle. After a total of 10 cycles, it is taken out to an environment of 25°C. Even in this case, the generation of bubbles in the first adhesive layer 102 and the generation of peeling between the first adhesive layer 102 and the front panel 101 can be suppressed (hereinafter, this performance is also referred to as "excellent bending durability in a thermal shock test environment"). It should be noted that when the stacked body 100 is bent with the front panel 101 side facing inward and subjected to heat shock, bubbles are easily generated in the first adhesive layer 102 located on the inner side (the side close to the core rod) relative to the second adhesive layer 104 and the peeling of the adjacent layers is more likely to occur than in the second adhesive layer 104. However, by satisfying the above conditions, the generation of bubbles in the first adhesive layer 102 and the peeling of the adjacent layers can be suppressed.

[0057] In addition, when the stress reduction rate of the first adhesive layer 102 is 40% or more and 70% or less, and the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2), the generation of bubbles in the first adhesive layer 102 can be suppressed in a low-temperature bending test when the laminate 100 is bent in a manner with the front panel 101 side being the inner side, thereby improving durability. Specifically, as shown in the embodiments described later, the laminate 100 is wound around a mandrel in a manner with the front panel 101 being the inner side when bent, placed in an environment of -20°C for 24 hours, and taken out to an environment of 25°C. Even in this case, the generation of bubbles in the first adhesive layer 102 and the generation of peeling between the first adhesive layer 102 and the front panel 101 can be suppressed (hereinafter, this performance is also referred to as "excellent low-temperature bending"). It should be noted that when the stacked body 100 is bent with the front panel 101 side facing inside and placed in a low-temperature environment, bubbles are easily generated in the first adhesive layer 102 located on the inside (the side close to the core rod) relative to the second adhesive layer 104 and the peeling of the adjacent layers is more likely to occur than in the second adhesive layer 104. However, by satisfying the above conditions, the generation of bubbles in the first adhesive layer 102 and the peeling of the adjacent layers can be suppressed.

[0058] In the present embodiment, the stress reduction rate of the first adhesive layer 102 is more preferably 45% to 65%, and further preferably 50% to 60%, from the viewpoint of further improving the thermal shock bendability and low-temperature bendability when bending with the front panel 101 side as the inner side.

[0059] In this embodiment, the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 preferably satisfy the relationship of the following formula (3). By making R1 and R2 satisfy the relationship of the following formula (3), the thermal shock bendability and low temperature bendability when bending with the front panel 101 side as the inner side can be further improved. From the viewpoint of further improving the above-mentioned effect, the value of R2-R1 can be 18Pa or less, or 16Pa or less.

[0060] 0Pa≤(R2-R1)≤20Pa...(3)

[0061] In the laminate 100, the stress reduction rate of the second adhesive layer 104 is not particularly limited as long as it satisfies the condition of the above formula (2), but is preferably 40% or more and 70% or less, more preferably 45% or more and 70% or less, and further preferably 50% or more and 70% or less. By setting the stress reduction rate of the second adhesive layer 104 to be within the above range, the generation of bubbles in the first adhesive layer 102 and the peeling from the adjacent layer can be further suppressed in the above thermal shock test and the above low-temperature bending test.

[0062] Here, the term "bend" in this specification includes a bent form in which a curved surface is formed in the bent portion. In the bent form, the radius of curvature of the inner surface of the bent portion is not limited unless otherwise specified. In addition, unless otherwise specified, "bend" includes a bent form in which the bending angle of the inner surface is greater than 0 degrees and less than 180 degrees, and includes a folded form in which the radius of curvature of the inner surface is approximately zero or the bending angle of the inner surface is 0 degrees.

[0063] The laminate 100 can be used for a laminate that is bent with the front panel 101 side as the inner side (so-called inward folding mode) and a display device (flexible display device) including the laminate. It should be noted that the laminate 100 can also be bent with the front panel 101 side as the outer side. Therefore, the laminate 100 can also be applied to a laminate that is bent not only with the front panel 101 side as the inner side but also with the front panel 101 side as the outer side, and a display device including the laminate.

[0064] The gel fraction of the pressure-sensitive adhesive layer may be 40 to 90%, or 50 to 80%.

[0065] The thickness of the adhesive layer is not particularly limited, but is preferably 10 μm to 150 μm, more preferably 10 μm to 100 μm, further preferably 15 μm to 80 μm, and particularly preferably 20 μm to 75 μm.

[0066] The thickness T1 of the first adhesive layer 102 and the thickness T2 of the second adhesive layer 104 preferably satisfy the relationship of the following formula (4). By making T1 and T2 satisfy the relationship of the following formula (4), the thermal shock bendability and low temperature bendability when bending with the front panel 101 side as the inner side can be further improved. From the viewpoint of further improving the above effects, the value of T1 / T2 can be greater than 0.5 and less than 3.5.

[0067] 0.1≤(T1 / T2)≤4...(4)

[0068] Here, as a method for preparing the first adhesive composition and the second adhesive composition constituting the first adhesive layer and the second adhesive layer of the present embodiment, for example, these compositions include the adhesive composition A described later, or the type of monomer constituting the (meth)acrylic polymer A described later is changed, or the molecular weight of the (meth)acrylic polymer A is adjusted. The adhesive composition is described in detail below.

[0069] <Adhesive Composition A>

[0070] In the first adhesive layer 102 and the second adhesive layer 104, the compositions of the two may be the same or different, but both may be formed in one mode by an adhesive composition (hereinafter also referred to as "adhesive composition A") containing a (meth) acrylic polymer. Adhesive composition A may be an active energy ray-curable type or a thermosetting type. The so-called "(meth) acrylic polymer" in this specification means at least one selected from acrylic polymers and methacrylic polymers. The same also applies to other terms with "(meth)". For the first adhesive composition forming the first adhesive layer and the second adhesive composition forming the second adhesive layer, when both contain (meth) acrylic polymers, their (meth) acrylic polymers may be the same or different. Hereinafter, the (meth) acrylic polymer contained in adhesive composition A will also be referred to as "(meth) acrylic polymer A".

[0071] The (meth) acrylic polymer A of the present embodiment may contain a nitrogen atom-containing monomer as a monomer unit constituting the polymer. Examples of nitrogen atom-containing monomers include monomers having an amino group, monomers having an amide group, monomers having a nitrogen-containing heterocycle, and the like. Among them, from the viewpoint of the bending durability of the resulting adhesive layer, monomers having an amide group (amide-containing monomers) are preferred. They may be used alone or in combination of two or more. It should be noted that the monomers containing reactive functional groups described later are excluded from the nitrogen atom-containing monomers mentioned here.

[0072] Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-dodecyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide; alkoxyalkyl(meth)acrylamide such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide, etc. Among them, N-dodecyl(meth)acrylamide is preferred from the viewpoint of the bending durability of the obtained adhesive layer.

[0073] In the case where (meth) acrylic polymer A contains a nitrogen-containing monomer (particularly an amide-containing monomer) as a monomer unit constituting the polymer, its content is preferably 20% by mass or more and 30% by mass or less relative to 100% by mass of all structural units, more preferably 22% by mass or more and 28% by mass or less, and further preferably 24% by mass or more and 26% by mass or less. By controlling the content of the structural unit from the nitrogen-containing monomer, the stress reduction rate of the adhesive layer can be adjusted to a desired range. Specifically, by increasing the content of the structural unit from the nitrogen-containing monomer, the flexibility of the adhesive layer can be reduced and the stress reduction rate can be increased.

[0074] The adhesive composition A preferably further comprises a fluorine atom-containing compound as an additive in addition to the (meth)acrylic polymer A. Examples of the fluorine atom-containing compound include 2,2,2-trifluoroethyl (meth)acrylate and 2,2,3,3-tetrafluoropropyl (meth)acrylate, wherein 2,2,2-trifluoroethyl methacrylate and 2,2,3,3-tetrafluoropropyl acrylate are preferred from the viewpoint of improving the heat resistance of the obtained adhesive layer. These may be used alone or in combination of two or more.

[0075] When the adhesive composition A contains a fluorine atom-containing compound, the content thereof is preferably 5% by mass or less, more preferably 4% by mass or less, and further preferably 3% by mass or less relative to 100% by mass of the solid content of the adhesive composition A. In addition, the content of the fluorine atom-containing compound is preferably 1% by mass or more relative to 100% by mass of the solid content of the adhesive composition A. By controlling the content of the fluorine atom-containing compound, the heat resistance of the adhesive layer can be adjusted and the bending durability of the laminate under the thermal shock test environment can be improved.

[0076] (Active energy ray-curable adhesive composition)

[0077] In the case where the adhesive composition A is an active energy ray-curable adhesive composition, in the (meth) acrylic polymer A contained in the adhesive composition A, the content of the structural unit from the monomer with reactive functional groups is preferably less than 1% by mass based on the total mass of the (meth) acrylic polymer A. As reactive functional groups, for example, hydroxyl, carboxyl and epoxy groups can be cited. Thus, the flexibility of the adhesive layer is improved, and there is a trend of easily suppressing the generation of bubbles in the adhesive layer under the thermal shock test environment. In the (meth) acrylic polymer A, about the content of the structural unit from the monomer with reactive functional groups, from the viewpoint of suppressing the generation of bubbles during bending, it is more preferably less than 0.01% by mass based on the total mass of the (meth) acrylic polymer A, and it is further preferred that there is no structural unit from the monomer with reactive functional groups, and it is particularly preferred that there is no hydroxyl, carboxyl and epoxy group.

[0078] The (meth)acrylic polymer A may contain a structural unit derived from a (meth)acrylic monomer having a linear or branched alkyl group with 1 to 24 carbon atoms. As the (meth)acrylic monomer having a linear or branched alkyl group with 1 to 24 carbon atoms, for example, an alkyl (meth)acrylate may be used, and examples thereof include butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, and the like. The (meth)acrylic polymer A may be a polymer or copolymer having one or more of the above-mentioned alkyl (meth)acrylates as monomers.

[0079] The content of the (meth)acrylic polymer A in the adhesive composition A is, for example, 50% to 100% by mass, preferably 80% to 99.5% by mass, and more preferably 90% to 99% by mass, relative to 100% by mass of the solid content of the adhesive composition A.

[0080] The weight average molecular weight (Mw) of the (meth)acrylic polymer A can be, for example, 100,000 to 2,000,000, and is preferably 500,000 to 1,500,000 from the viewpoint of suppressing bubbles during bending. The weight average molecular weight in this specification can be obtained based on the value converted to standard polystyrene measured by gel permeation chromatography (GPC) as described in the Examples column described later.

[0081] The adhesive composition A may contain one or more (meth) acrylic polymers A. In addition, the adhesive composition A may contain only the (meth) acrylic polymer A as its constituent component, or may further contain a crosslinking agent. As a crosslinking agent, there may be cited divalent or more metal ions that form carboxylic acid metal salts with carboxyl groups; polyamine compounds that form amide bonds with carboxyl groups; polyepoxide compounds or polyols that form ester bonds with carboxyl groups; polyisocyanate compounds that form amide bonds with carboxyl groups, etc., as polyisocyanate compounds. Among them, polyisocyanate compounds are preferred. In the case where the adhesive composition A contains a crosslinking agent, the content of the crosslinking agent can be, for example, 5 parts by mass or less, preferably 3 parts by mass or less, more preferably 1 part by mass or less, and further preferably 0.5 parts by mass or less relative to 100 parts by mass of the (meth) acrylic polymer A. The adhesive composition A may also not contain a crosslinking agent.

[0082] The so-called active energy ray-curable adhesive composition is an adhesive composition having the following properties, that is, having the property of being cured by irradiation with active energy rays such as ultraviolet rays or electron beams, having adhesiveness before irradiation with active energy rays and being able to adhere to an adherend such as a film, and being able to adjust the adhesion by curing due to irradiation with active energy rays. The active energy ray-curable adhesive composition is preferably an ultraviolet curable type.

[0083] When the pressure-sensitive adhesive composition A is an active energy ray-curable pressure-sensitive adhesive composition, the pressure-sensitive adhesive composition A may further contain an active energy ray-polymerizable compound, a photopolymerization initiator, a photosensitizer, and the like.

[0084] Examples of active energy ray polymerizable compounds include (meth)acrylic compounds such as compounds containing (meth)acryloyloxy groups. Examples of compounds containing (meth)acryloyloxy groups include (meth)acrylate monomers having at least one (meth)acryloyloxy group in the molecule; (meth)acrylate oligomers having at least two (meth)acryloyloxy groups in the molecule obtained by reacting two or more functional group-containing compounds; and the like. The adhesive composition A may contain 0.1% by mass or more and 10% by mass or less of active energy ray polymerizable compounds relative to 100% by mass of the solid content of the adhesive composition A.

[0085] As the photopolymerization initiator, for example, benzophenone, benzyldimethylketal, 1-hydroxycyclohexyl ketone, etc. can be mentioned. When the adhesive composition A contains a photopolymerization initiator, it can contain one or more kinds. When the adhesive composition A contains a photopolymerization initiator, the total content thereof can be, for example, 0.01% by mass or more and 1.0% by mass or less relative to 100% by mass of the solid content of the adhesive composition A.

[0086] The adhesive composition A may contain additives such as fine particles, beads (resin beads, glass beads, etc.), glass fibers, resins other than the base polymer, tackifiers, fillers (metal powders or other inorganic powders, etc.), antioxidants, ultraviolet absorbers, dyes, pigments, colorants, defoamers, and anticorrosives for imparting light scattering properties. From the viewpoint of preventing the problem of reduced durability due to residual solvents, the adhesive composition A preferably does not contain an organic solvent.

[0087] When the adhesive layer is formed of the adhesive composition A, the adhesive layer can be formed by applying the adhesive composition A to a substrate. When an active energy ray-curable adhesive composition is used, a cured product having a desired degree of curing can be prepared by irradiating the formed adhesive layer with active energy rays.

[0088] (Thermosetting Adhesive Composition)

[0089] When the adhesive composition A is a thermosetting adhesive composition, the (meth)acrylic polymer A preferably contains an alkyl (meth)acrylate having an alkyl group with 2 to 20 carbon atoms and a monomer having a reactive functional group in the molecule (a monomer containing a reactive functional group) as monomer units constituting the polymer. When the adhesive composition A is a thermosetting adhesive composition, it preferably further contains a thermal crosslinking agent.

[0090] By making the (meth)acrylic polymer A contain a (meth)acrylic acid alkyl ester having an alkyl group with 2 to 20 carbon atoms as a monomer unit constituting the polymer, preferred adhesiveness can be exhibited. When the (meth)acrylic acid alkyl ester having an alkyl group with 2 to 20 carbon atoms forms a homopolymer, for example, it is preferable to contain a (meth)acrylic acid alkyl ester having a Tg of -40°C or less (hereinafter sometimes referred to as "low Tg alkyl acrylate"). By containing the above-mentioned low Tg alkyl acrylate as a constituent monomer unit, the flexibility of the adhesive layer is improved, and the generation of bubbles during bending can be more easily suppressed.

[0091] As low Tg alkyl acrylate, for example, n-butyl acrylate (Tg-54°C), n-octyl acrylate (Tg-65°C), isooctyl acrylate (Tg-58°C), 2-ethylhexyl acrylate (Tg-70°C), isononyl acrylate (Tg-58°C), isodecyl acrylate (Tg-60°C), isodecyl methacrylate (Tg-41°C), n-lauryl methacrylate (Tg-65°C), tridecyl acrylate (Tg-55°C), tridecyl methacrylate (Tg-40°C), etc. are preferably mentioned. Among them, as low Tg alkyl acrylate, compounds having a homopolymer Tg of -45°C or less are more preferred, and compounds having a Tg of -50°C or less are particularly preferred. Specifically, n-butyl acrylate and 2-ethylhexyl acrylate are particularly preferred. These may be used alone or in combination of two or more.

[0092] The (meth)acrylic polymer A preferably contains 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more of a low Tg alkyl acrylate as a monomer unit constituting the polymer, as the lower limit.

[0093] In addition, the (meth)acrylic polymer A preferably contains 99.9% by mass or less of the above-mentioned low Tg alkyl acrylate as a monomer unit constituting the polymer, more preferably 99.5% by mass or less, and further preferably 99% by mass or less. By containing 99.9% by mass or less of the above-mentioned low Tg alkyl acrylate, an appropriate amount of other monomer components (particularly a monomer containing a reactive functional group) can be introduced into the (meth)acrylic polymer A.

[0094] From the viewpoint of further exerting the effect of the present invention, the content of the monomer having a glass transition temperature (Tg) of greater than 0°C as a homopolymer (hereinafter sometimes referred to as "hard monomer") in the (meth)acrylic polymer A is preferably reduced as much as possible. Specifically, the content of the hard monomer as a monomer unit constituting the polymer in the (meth)acrylic polymer A is preferably set to 15% by mass or less, more preferably 10% by mass or less, and further preferably 5% by mass or less in terms of the upper limit. The hard monomer also includes the monomer containing a reactive functional group described later.

[0095] Examples of the hard monomer include methyl acrylate (Tg 10°C), methyl methacrylate (Tg 105°C), ethyl methacrylate (Tg 65°C), n-butyl methacrylate (Tg 20°C), isobutyl methacrylate (Tg 48°C), tert-butyl methacrylate (Tg 107°C), n-stearyl acrylate (Tg 30°C), n-stearyl methacrylate (Tg 38°C), cyclohexyl acrylate (Tg 15°C), cyclohexyl methacrylate (Tg 66°C), phenoxyethyl acrylate (Tg 5°C), methyl Acrylic monomers such as phenoxyethyl acrylate (Tg54℃), benzyl methacrylate (Tg54℃), isobornyl acrylate (Tg94℃), isobornyl methacrylate (Tg180℃), acryloylmorpholine (Tg145℃), adamantyl acrylate (Tg115℃), adamantyl methacrylate (Tg141℃), acrylic acid (Tg105℃), dimethylacrylamide (Tg89℃), acrylamide (Tg165℃), vinyl acetate (Tg32℃), styrene (Tg80℃), etc.

[0096] Since the (meth)acrylic polymer A contains a monomer containing a reactive functional group as a monomer unit constituting the polymer, the reactive functional group from the monomer containing the reactive functional group reacts with the thermal crosslinking agent described later. Thus, a crosslinked structure (three-dimensional network structure) is formed as a whole, thereby obtaining an adhesive having a desired cohesive force.

[0097] Preferred examples of the monomer containing a reactive functional group contained in the (meth)acrylic polymer A as a monomer unit constituting the polymer include a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. Among them, a hydroxyl group-containing monomer is particularly preferred because there are many monomers having a glass transition temperature (Tg) of 0° C. or less.

[0098] Examples of hydroxyl-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among them, from the perspective of glass transition temperature (Tg), the reactivity of the hydroxyl group in the obtained (meth)acrylic polymer A with a thermal crosslinking agent, and copolymerizability with other monomers, at least one of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, and 4-hydroxybutyl acrylate is preferred. These may be used alone or in combination of two or more.

[0099] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. These may be used alone or in combination of two or more.

[0100] Examples of the amino group-containing monomer include aminoethyl (meth)acrylate, n-butylaminoethyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0101] The (meth)acrylic polymer A preferably contains 0.1% by mass or more of a monomer containing a reactive functional group as a monomer unit constituting the polymer, with respect to the lower limit, preferably 0.5% by mass or more, and more preferably 1% by mass or more. The (meth)acrylic polymer A preferably contains 10% by mass or less of the above-mentioned monomer containing a reactive functional group, with respect to the upper limit, preferably 8% by mass or less, and more preferably 5% by mass or less. This tends to make it easier to suppress the generation of bubbles during bending.

[0102] The (meth)acrylic acid polymer A may not contain a carboxyl group-containing monomer, particularly acrylic acid, which is also a hard monomer, as a monomer unit constituting the polymer. Since the carboxyl group is an acid component, the absence of the carboxyl group-containing monomer can suppress the occurrence of adverse conditions caused by the acid on the object to which the adhesive is attached. For example, in the presence of a transparent conductive film such as tin-doped indium oxide (ITO), a metal film or a metal mesh, these adverse conditions (corrosion, resistance value change, etc.) caused by the acid can also be suppressed.

[0103] The (meth)acrylic polymer A may contain other monomers as monomer units constituting the polymer as required. As other monomers, in order not to hinder the action of the monomer containing a reactive functional group, it is also preferred that the monomer not contain a reactive functional group. As the above-mentioned other monomers, for example, (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, and monomers having a glass transition temperature (Tg) greater than -40°C and below 0°C as a homopolymer (hereinafter sometimes referred to as "medium Tg alkyl acrylates"), etc. As medium Tg alkyl acrylates, for example, ethyl acrylate (Tg-20°C), isobutyl acrylate (Tg-26°C), 2-ethylhexyl methacrylate (Tg-10°C), n-lauryl acrylate (Tg-23°C), isostearyl acrylate (Tg-18°C), etc. can be mentioned. They can be used alone or in combination of two or more.

[0104] The polymerization form of the (meth)acrylic polymer A may be a random copolymer or a block copolymer.

[0105] The lower limit of the weight average molecular weight of the (meth)acrylic polymer A is preferably 200,000 or more, particularly preferably 300,000 or more, and further preferably 400,000 or more. If the lower limit of the weight average molecular weight of the (meth)acrylic polymer A is above, undesirable conditions such as oozing of the adhesive are suppressed. The weight average molecular weight in this specification can be obtained based on the value converted to standard polystyrene measured by gel permeation chromatography (GPC) as described in the Examples column described later.

[0106] The upper limit of the weight average molecular weight of the (meth)acrylic polymer A is preferably 2 million or less, particularly preferably 1.5 million or less, and further preferably 1.3 million or less. If the upper limit of the weight average molecular weight of the (meth)acrylate polymer (A) is below the above, the flexibility of the adhesive layer can be ensured, and the effect of the present invention can be easily exerted.

[0107] In the pressure-sensitive adhesive composition A, the (meth)acrylic polymer A may be used alone or in combination of two or more.

[0108] When the adhesive composition A containing a thermal crosslinking agent is heated, the thermal crosslinking agent crosslinks the (meth)acrylic polymer A to form a three-dimensional network structure. This can improve the cohesive force while ensuring the flexibility of the adhesive, and when applied to a laminate, a hardness that can improve the surface hardness of the laminate can be obtained.

[0109] As the above-mentioned thermal crosslinking agent, any crosslinking agent that reacts with the reactive group possessed by the (meth) acrylic polymer A may be used, for example, isocyanate crosslinking agents, epoxy crosslinking agents, amine crosslinking agents, melamine crosslinking agents, aziridine crosslinking agents, hydrazine crosslinking agents, aldehyde crosslinking agents, oxazoline crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, ammonium salt crosslinking agents, etc. Among the above, when the reactive group possessed by the (meth) acrylic polymer A is a hydroxyl group, it is preferred to use an isocyanate crosslinking agent that has excellent reactivity with the hydroxyl group. The thermal crosslinking agent may be used alone or in combination of two or more.

[0110] The isocyanate crosslinking agent contains at least a polyisocyanate compound. As the polyisocyanate compound, for example, aromatic polyisocyanates such as toluene diisocyanate, diphenylmethane diisocyanate, and xylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, alicyclic polyisocyanates such as hydrogenated diphenylmethane diisocyanate, and the like, and their biuret bodies, isocyanurate bodies, and adducts as reactants with low molecular weight active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil, etc. Among them, from the viewpoint of reactivity with hydroxyl groups, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified toluene diisocyanate and trimethylolpropane-modified xylene diisocyanate are preferred.

[0111] Examples of epoxy crosslinking agents include 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidyl aniline, and diglycidyl amine.

[0112] The content of the thermal crosslinking agent in the adhesive composition A is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and further preferably 0.1 parts by mass or more relative to 100 parts by mass of the (meth) acrylic polymer A. In addition, the content is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and further preferably 0.5 parts by mass or less. By making the content of the thermal crosslinking agent within the above range, it is possible to more easily obtain a moderate hardness due to an increase in cohesive force.

[0113] The adhesive composition A may contain a silane coupling agent. This improves the adhesion between the obtained adhesive layer and each member in the laminated body serving as an adherend, and further improves the durability against bending.

[0114] The silane coupling (SC) agent is an organic silicon compound having at least one alkoxysilyl group in the molecule, and preferably a compound having good compatibility with the (meth)acrylic polymer A and having light transparency.

[0115] Examples of the silane coupling agent include silicon compounds containing a polymerizable unsaturated group such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane, silicon compounds having an epoxy structure such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and mercapto groups such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane. Silicon compounds, amino-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, or condensates of at least one of these with alkyl-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane, etc. These may be used alone or in combination of two or more.

[0116] The content of the silane coupling agent in the adhesive composition A is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and further preferably 0.1 parts by mass or more relative to 100 parts by mass of the (meth) acrylic polymer A. In addition, the content is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and further preferably 0.3 parts by mass or less. By making the content of the silane coupling agent within the above range, the adhesion with each member in the laminate can be further improved.

[0117] Various additives may be added to the adhesive composition A as needed. In the present specification, the polymerization solvent and the dilution solvent are solvents not included in the additives constituting the adhesive composition A.

[0118] The (meth)acrylic acid polymer A can be produced by polymerizing a mixture of monomers constituting the polymer using a conventional free radical polymerization method. The polymerization of the (meth)acrylic acid polymer A is preferably carried out using a polymerization initiator as required and using a solution polymerization method. Examples of the polymerization solvent include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, methyl ethyl ketone, and the like, and two or more thereof may be used in combination.

[0119] Examples of the polymerization initiator include azo compounds and organic peroxides, and two or more of them may be used in combination. Examples of the azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane 1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].

[0120] Examples of the organic peroxide include benzoyl peroxide, tert-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl) peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, (3,5,5-trimethylhexanoyl) peroxide, dipropionyl peroxide, and diacetyl peroxide.

[0121] In the above-mentioned polymerization step, by adding a chain transfer agent such as 2-mercaptoethanol, the weight average molecular weight of the obtained polymer can be adjusted.

[0122] After obtaining the (meth) acrylic polymer A, a thermal crosslinking agent, a silane coupling agent, and additives and a diluting solvent as needed are added to the solution of the (meth) acrylic polymer A, and the mixture is fully mixed to obtain an adhesive composition A (coating solution) diluted with a solvent. The adhesive composition A can be prepared by utilizing a known method, for example, by mixing the components at one time using a mixer. In addition, the first adhesive composition and the second adhesive composition can be prepared from the adhesive composition A obtained as described above.

[0123] When any of the above components is used in a solid form, or when precipitation occurs when mixed with other components in an undiluted state, the component may be dissolved in a dilution solvent alone or diluted before mixing with other components.

[0124] As the above-mentioned diluting solvent, for example, aliphatic hydrocarbons such as hexane, heptane, and cyclohexane, aromatic hydrocarbons such as toluene and xylene, halogenated hydrocarbons such as dichloromethane and vinyl chloride, alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol, ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone, esters such as ethyl acetate and butyl acetate, and cellosolve-based solvents such as ethyl cellosolve can be used.

[0125] The concentration and viscosity of the adhesive composition A (coating solution) prepared as described above are not particularly limited as long as they are within the range that can be applied, and can be appropriately selected according to the situation. For example, the concentration of the adhesive composition A can be prepared in a manner that reaches 10 to 60% by mass in the solution. When obtaining the coating solution, the addition of a diluting solvent or the like is not a necessary condition, and as long as the viscosity of the adhesive composition A can be applied, the diluting solvent may not be added. In this case, the adhesive composition A becomes a coating solution directly using the polymerization solvent of the (meth) acrylic polymer A as the diluting solvent.

[0126] The adhesive layer can be obtained by crosslinking the adhesive composition A. The crosslinking of the adhesive composition A can be performed by heat treatment. The heat treatment can also serve as a drying treatment when the dilution solvent or the like is volatilized from the coating film of the adhesive composition A applied to the desired object.

[0127] The heating temperature in the heat treatment is preferably 50 to 150° C., and more preferably 70 to 120° C. The heating time in the heat treatment is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.

[0128] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23° C., 50% RH) as required. If such a curing period is required, the adhesive layer may be formed after the curing period. If a curing period is not required, the adhesive layer may be formed after the above-mentioned heat treatment is completed.

[0129] By the above-mentioned heat treatment (and curing), the (meth)acrylic polymer A is sufficiently crosslinked via the crosslinking agent to form a crosslinked structure, thereby obtaining the adhesive layer (the first adhesive layer 102 and the second adhesive layer 104 ).

[0130] <Adhesive Sheet>

[0131] The adhesive sheet may include an adhesive layer formed by the above-mentioned adhesive composition A. The adhesive layer can be formed by applying the adhesive composition A to a substrate. When an active energy ray-curable adhesive composition is used as the adhesive composition A, a cured product having a desired degree of cure can be prepared by irradiating the formed adhesive layer with active energy rays. When a thermosetting adhesive composition is used as the adhesive composition, a cured product having a desired degree of cure can be prepared by heat treating (and curing) the formed adhesive layer.

[0132] The substrate may be a release film subjected to a release treatment. The PSA sheet can be produced by applying the PSA composition A onto a release film to form a PSA layer in a sheet form, and further laminating another release film onto the PSA layer.

[0133] Examples of a method for applying the coating liquid of the pressure-sensitive adhesive composition A include bar coating, knife coating, roll coating, blade coating, die coating, and gravure coating.

[0134] <Front Panel>

[0135] As long as the front panel 101 is a plate-like body capable of transmitting light, the material and thickness are not limited, and it can be composed of only one layer or more than two layers. As examples thereof, a plate-like body made of resin (such as a resin plate, a resin sheet, a resin film, etc.), a plate-like body made of glass (such as a glass plate, a glass film, etc.), and a touch sensor panel described later can be cited. The front panel can be the outermost panel constituting the display device.

[0136] The thickness of front panel 101 may be, for example, 10 μm to 1000 μm, preferably 20 μm to 500 μm, and more preferably 30 μm to 300 μm. In the present invention, the thickness of each layer can be measured by the thickness measurement method described in the following examples.

[0137] When the front panel 101 is a plate-like body made of resin, the plate-like body made of resin is not limited as long as it is a plate-like body that can transmit light. As the resin constituting the plate-like body made of resin such as resin film, for example, films formed by macromolecules such as triacetyl cellulose, acetyl cellulose butyrate, ethylene-vinyl acetate copolymer, propionyl cellulose, butyryl cellulose, acetyl cellulose propionyl cellulose, polyester, polystyrene, polyamide, polyetherimide, poly(methyl) acrylic acid, polyimide, polyether sulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyether ether ketone, polyether sulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyamide-imide, and polyamide-imide can be cited. These macromolecules can be used alone or in combination with more than two kinds. From the viewpoint of improving strength and transparency, a resin film formed of a polymer such as polyimide, polyamide, or polyamideimide is preferred.

[0138] From the viewpoint of hardness, the front panel 101 is preferably a film having a hard coating layer on at least one surface of the substrate film. As the substrate film, a film formed by the above-mentioned resin can be used. The hard coating layer can be formed on one surface of the substrate film or on both surfaces. By providing the hard coating layer, a resin film having improved hardness and scratch resistance can be made. The hard coating layer is, for example, a cured layer of an ultraviolet curable resin. As the ultraviolet curable resin, for example, acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, epoxy resins, etc. can be cited. In order to increase the strength, the hard coating layer can include additives. The additives are not limited, and inorganic particles, organic particles, or mixtures thereof can be cited.

[0139] When the front panel 101 is a glass plate, the glass plate is preferably tempered glass for display. The thickness of the glass plate can be, for example, 10 μm to 1000 μm, or 50 μm to 500 μm. By using a glass plate, the front panel 101 having excellent mechanical strength and surface hardness can be formed.

[0140] When the stack 100 is used in a display device, the front panel 101 can not only have the function of protecting the front (screen) of the display device (as a window film), but also have the function of serving as a touch sensor, anti-blue light function, viewing angle adjustment function, etc.

[0141] <First Adhesive Layer>

[0142] The first adhesive layer 102 is a layer sandwiched between the front panel 101 and the polarizer layer 103 and pasted together, for example, it can be a layer containing an adhesive or a bonding agent or a layer formed by applying some treatment to the layer. The first adhesive layer 102 can be an adhesive layer configured at the position closest to the front panel 101 among the adhesive layers constituting the laminate 100. Here, the so-called "adhesive" in this specification is also referred to as a pressure-sensitive adhesive. In addition, the so-called "adhesive" in this specification refers to an adhesive other than an adhesive (pressure-sensitive adhesive), which is clearly distinguished from an adhesive. The first adhesive layer 102 can be 1 layer, or it can be a layer containing more than 2 layers, but preferably 1 layer.

[0143] The first adhesive layer 102 is formed using the first adhesive composition as described above. The first adhesive composition can be formed using the adhesive composition A as described above. The first adhesive layer 102 is a layer having a stress reduction rate of 40% or more and 70% or less obtained using the above formula (1), and is a layer formed in such a way that the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2). As long as the first adhesive composition satisfies the above conditions, it is not limited to the adhesive composition A, and can be directly formed from any adhesive composition, or can be formed using an adhesive sheet having an adhesive layer formed using any adhesive composition. However, the first adhesive composition is preferably formed from the above-mentioned adhesive composition A, or is also preferably formed using an adhesive sheet formed by applying the above-mentioned adhesive composition A to a substrate.

[0144] That is, in the first adhesive layer 102, the composition and compounding components of the first adhesive composition constituting it, the type of the first adhesive composition (active energy ray-curing type, thermosetting type, etc.), the additives that can be compounded into the first adhesive composition, the method for preparing the first adhesive layer and the thickness of the first adhesive layer, etc., can be set as described in the above-mentioned <Adhesive layer (first adhesive layer and second adhesive layer)> column.

[0145] <Polarizing Plate Layer>

[0146] As the polarizer layer 103, there can be cited a stretched film or stretched layer adsorbed with a dichroic pigment, a layer formed by coating a composition containing a dichroic pigment and a polymerizable compound and curing it, etc. As the dichroic pigment, specifically, iodine or a dichroic organic dye is used. The dichroic organic dye includes a dichroic direct dye containing a disazo compound such as CIDIRECT RED 39, and a dichroic direct dye containing a compound such as triazo or tetrakis azo.

[0147] As the polarizer layer formed by coating and curing a composition containing a dichroic dye and a polymerizable compound, there can be cited a polarizer layer containing a cured product of a polymerizable liquid crystal compound, such as a layer obtained by coating and curing a composition containing a dichroic dye having liquid crystal properties or a composition containing a dichroic dye and a polymerizable liquid crystal. The polarizer layer formed by coating and curing a composition containing a dichroic dye and a polymerizable compound is preferred because it has no restrictions on the bending direction compared to a stretched film or stretched layer adsorbed with a dichroic dye.

[0148] In the laminate 100 , the polarizer layer 103 can function as a circular polarization plate by, for example, combining with a retardation layer described later.

[0149] (Polarizer layer as stretched film or stretched layer)

[0150] The polarizer layer as a stretched film adsorbed with a dichroic dye can be generally manufactured through the following steps, namely, a step of uniaxially stretching a polyvinyl alcohol resin film, a step of dyeing the polyvinyl alcohol resin film with a dichroic dye to adsorb the dichroic dye, a step of treating the polyvinyl alcohol resin film adsorbed with a boric acid aqueous solution, and a step of washing with water after the treatment with the boric acid aqueous solution. The thickness of the polarizer layer 103 is, for example, 2 μm or more and 40 μm or less. The thickness of the polarizer layer 103 can be 5 μm or more, and can be 20 μm or less, further can be 15 μm or less, and further can be 10 μm or less.

[0151] The polyvinyl alcohol resin is obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, polyvinyl acetate, which is a homopolymer of vinyl acetate, can be used, and copolymers of vinyl acetate and other monomers copolymerizable therewith can also be used. As other monomers copolymerizable with vinyl acetate, for example, unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, (meth)acrylamides having an ammonium group, and the like can be cited.

[0152] The saponification degree of the polyvinyl alcohol resin is usually 85 mol% or more and 100 mol% or less, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, for example, polyvinyl formal or polyvinyl acetal modified by aldehydes may be used. The degree of polymerization of the polyvinyl alcohol resin is usually 1000 or more and 10000 or less, preferably 1500 or more and 5000 or less.

[0153] The polarizer layer as a stretched layer adsorbed with a dichroic pigment can usually be manufactured through the following steps, that is, a step of applying a coating liquid containing the above-mentioned polyvinyl alcohol resin on a substrate film, a step of uniaxially stretching the obtained laminated film, a step of dyeing the polyvinyl alcohol resin layer of the uniaxially stretched laminated film with a dichroic pigment to adsorb the dichroic pigment, and a step of making a polarizer layer, a step of treating the film adsorbed with the dichroic pigment with an aqueous boric acid solution, and a step of washing with water after the treatment with the aqueous boric acid solution. The polarizer layer as a stretched layer adsorbed with a dichroic pigment can be stripped and removed from the substrate film as needed. The material and thickness of the substrate film can be the same as the material and thickness of the thermoplastic resin film described later.

[0154] The polarizer layer as a stretched film or stretched layer can be assembled into a laminate in the form of a thermoplastic resin film attached to one or both sides thereof. The thermoplastic resin film can function as a protective film for the polarizer layer 103 or a phase difference film. The thermoplastic resin film can be, for example, a polyolefin resin including a chain polyolefin resin (polypropylene resin, etc.), a cyclic polyolefin resin (norbornene resin, etc.); a cellulose resin such as triacetyl cellulose; a polyester resin such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate; a polycarbonate resin; a (meth) acrylic resin; or a film of a mixture thereof.

[0155] The thermoplastic resin film may or may not have a phase difference. The thickness of the thermoplastic resin film is generally 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less, further preferably 80 μm or less, and further preferably 60 μm or less from the viewpoint of thinning. The thickness of the thermoplastic resin film is generally 5 μm or more, preferably 20 μm or more. The thermoplastic resin film can be bonded to the polarizer layer 103 using an adhesive layer, for example.

[0156] (Polarizing layer formed by applying and curing a composition containing a dichroic dye and a polymerizable compound)

[0157] Examples of polarizer layers formed by coating and curing a composition containing a dichroic dye and a polymerizable compound include a layer obtained by coating a composition containing a polymerizable dichroic dye having liquid crystal properties or a composition containing a dichroic dye and a polymerizable liquid crystal on a substrate film and curing the composition.

[0158] The polarizer layer formed by coating and curing the composition comprising a dichroic pigment and a polymerizable compound can be peeled off from the polarizer layer as needed. The material and thickness of the substrate film can be the same as the material and thickness of the above-mentioned thermoplastic resin film. The polarizer layer can have an alignment film. The alignment film can be peeled off.

[0159] The polarizer layer formed by coating and curing the composition comprising a dichroic pigment and a polymerizable compound can be loaded into the optical laminate in the form of a thermoplastic resin film bonded to one or both sides thereof. As the thermoplastic resin film, the same film as the thermoplastic resin film that can be used in the polarizer layer as a stretched film or a stretched layer can be used. The thermoplastic resin film can be bonded to the polarizer layer using, for example, an adhesive layer.

[0160] The polarizer layer formed by coating and curing a composition containing a dichroic pigment and a polymerizable compound may have an outer coating (OC) layer formed on one or both sides as a protective layer. As the OC layer, for example, a cured layer of a photocurable resin, a water-soluble polymer, etc. can be cited. As the photocurable resin, for example, (meth) acrylic resins, urethane resins, (meth) acrylic urethane resins, epoxy resins, silicone resins, etc. can be cited. As the water-soluble polymer, for example, poly (meth) acrylamide polymers; polyvinyl alcohol and ethylene-vinyl alcohol copolymers, ethylene-vinyl acetate copolymers, (meth) acrylic acid or its anhydride-vinyl alcohol copolymers and other vinyl alcohol polymers can be cited; carboxyvinyl polymers; polyvinyl pyrrolidone; starch; sodium alginate; polyethylene oxide polymers, etc. The thickness of the OC layer is preferably less than 20 μm, more preferably less than 15 μm, further preferably less than 10 μm, and can also be less than 5 μm. In addition, it is more than 0.05 μm, and can also be more than 0.5 μm.

[0161] The thickness of the polarizer layer formed by applying and curing the composition containing the dichroic dye and the polymerizable compound is usually 10 μm or less, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 5 μm.

[0162] <Second Adhesive Layer>

[0163] The second adhesive layer 104 is an adhesive layer disposed between the polarizer layer 103 and the back plate 105. The second adhesive layer may be an adhesive layer disposed closest to the back plate 105 among the adhesive layers constituting the laminate 100. The second adhesive layer 104 may be a single layer or may be a layer including two or more layers, but is preferably a single layer.

[0164] The second adhesive layer 104 is formed using the second adhesive composition as described above. The second adhesive composition can be formed using the adhesive composition A as described above. The second adhesive layer 104 is a layer formed in such a way that the stress reduction rate R1 of the first adhesive layer 102 and the stress reduction rate R2 of the second adhesive layer 104 satisfy the relationship of the above formula (2). As long as the second adhesive composition meets the above conditions, it is not limited to the adhesive composition A, and can be directly formed by any adhesive composition, or can be formed using an adhesive sheet having an adhesive layer formed using any adhesive composition. However, the second adhesive composition is preferably formed by the above-mentioned adhesive composition A, or is also preferably formed using an adhesive sheet formed by applying the above-mentioned adhesive composition A to a substrate.

[0165] That is, the second adhesive layer 104 may have the same composition as the first adhesive layer 102 or may be different, but they are the same in that they are preferably formed of the adhesive composition A. Therefore, in the second adhesive layer 104, the composition and compounding components of the second adhesive composition constituting it, the type of the second adhesive composition (active energy ray curing type or thermosetting type, etc.), the additives that can be compounded into the second adhesive composition, the method for preparing the second adhesive layer, the thickness of the second adhesive layer, etc., can be set as described in the above <Adhesive layer (first adhesive layer and second adhesive layer)> column.

[0166] <Back Panel>

[0167] As the rear panel 105 , a plate-like body capable of transmitting light, a component used in a general display device, or the like can be used.

[0168] The thickness of rear plate 105 may be, for example, not less than 5 μm and not more than 2000 μm, preferably not less than 10 μm and not more than 1000 μm, and more preferably not less than 15 μm and not more than 500 μm.

[0169] The plate-like body used in rear plate 105 may be composed of only one layer or may be composed of two or more layers, and the plate-like body exemplified for the plate-like body described in connection with front plate 101 may be used.

[0170] As the components used in the general display device used in the back panel 105, for example, a spacer, a touch sensor panel, an organic EL display element, etc. can be cited. As the stacking order of the components in the display device, for example, front panel / circular polarization plate / spacer, front panel / circular polarization plate / organic EL display device, front panel / circular polarization plate / touch sensor panel / organic EL display element, front panel / touch sensor panel / circular polarization plate / organic EL display element, etc. can be cited. The back panel 105 is preferably a touch sensor panel.

[0171] (Touch sensor panel)

[0172] As a touch sensor panel, as long as it is a sensor that can detect a touched position, the detection method is not limited, and examples thereof include touch sensor panels of a resistive film method, an electrostatic capacitance coupling method, an optical sensor method, an ultrasonic method, an electromagnetic induction coupling method, a surface elastic wave method, etc. From the perspective of low cost, touch sensor panels of a resistive film method and an electrostatic capacitance coupling method can be appropriately used.

[0173] An example of a touch sensor panel of a resistive film type includes a pair of substrates arranged opposite to each other, an insulating spacer sandwiched between the pair of substrates, a transparent conductive film provided as a resistive film on the entire inner side of each substrate, and a touch position detection circuit. In an image display device provided with a touch sensor panel of a resistive film type, when the surface of the front panel is touched, the resistive films facing each other are short-circuited, and current flows through the resistive films. The touch position detection circuit detects the change in voltage at this time and detects the touched position.

[0174] An example of a capacitive coupling touch sensor panel includes a substrate, a transparent electrode for position detection disposed on the entire surface of the substrate, and a touch position detection circuit. In an image display device provided with a capacitive coupling touch sensor panel, when the surface of the front panel is touched, the transparent electrode is grounded at the touched point via the electrostatic capacitance of the human body. The touch position detection circuit detects the grounding of the transparent electrode and detects the touched position.

[0175] The thickness of the touch sensor panel may be, for example, not less than 5 μm and not more than 2000 μm, or not less than 5 μm and not more than 100 μm.

[0176] <Phase difference layer>

[0177] The laminate 100 may have one or more phase difference layers between the polarizer layer 103 and the back plate 105. The phase difference layer may be laminated on other layers (including other phase difference layers) via the first adhesive layer 102, the second adhesive layer 104, or a layer containing an adhesive or a bonding agent other than these layers (hereinafter also referred to as a bonding layer).

[0178] As examples of phase difference layers, positive A plates and positive C plates such as λ / 4 plates and λ / 2 plates can be cited. The phase difference layer can be, for example, a phase difference film that can be formed by the above-mentioned thermoplastic resin film, or a layer formed by curing a polymerizable liquid crystal compound, that is, a layer containing a cured product of a polymerizable liquid crystal compound, preferably the latter. The thickness of the phase difference film can be the same as the thickness of the above-mentioned thermoplastic resin film. The thickness of the phase difference layer formed by curing the polymerizable liquid crystal compound is, for example, 0.1 μm or more and 10 μm or less, preferably 0.5 μm or more and 8 μm or less, and more preferably 1 μm or more and 6 μm or less.

[0179] The phase difference layer formed by curing the polymerizable liquid crystal compound can be formed by applying a composition containing the polymerizable liquid crystal compound to a substrate film and curing it. An orientation layer can be formed between the substrate film and the coating layer. The material and thickness of the substrate film can be the same as the material and thickness of the above-mentioned thermoplastic resin film. The phase difference layer formed by curing the polymerizable liquid crystal compound can be loaded into the stack 100 in the form of an orientation layer and / or a substrate film. The back panel 105 can be a substrate film coated with the above-mentioned composition.

[0180] <Lamination layer>

[0181] The laminating layer is a layer disposed between the first adhesive layer 102 and the second adhesive layer 104, and is a layer containing an adhesive or a bonding agent. The adhesive constituting the laminating layer may be the same adhesive as the adhesive composition exemplified for constituting the first adhesive layer 102 and the second adhesive layer 104, or may be other adhesives, such as (meth) acrylic adhesives, styrene adhesives, silicone adhesives, rubber adhesives, urethane adhesives, polyester adhesives, epoxy copolymer adhesives, etc.

[0182] As the adhesive constituting the laminating layer, for example, it can be one or a combination of two or more of a water-based adhesive, an active energy ray-curable adhesive, an adhesive, etc. As the water-based adhesive, for example, polyvinyl alcohol resin aqueous solution, water-based two-component urethane emulsion adhesive, etc. can be cited. As the active energy ray-curable adhesive, it is an adhesive that is cured by irradiating active energy rays such as ultraviolet rays, for example, an adhesive containing a polymerizable compound and a photopolymerization initiator, an adhesive containing a photoreactive resin, an adhesive containing a binder resin and a photoreactive crosslinking agent, etc. can be cited. As the above-mentioned polymerizable compound, photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, photocurable urethane monomers, and oligomers derived from these monomers can be cited. As the above-mentioned photopolymerization initiator, an initiator of a substance containing active species such as neutral free radicals, anionic free radicals, and cationic free radicals generated by irradiating active energy rays such as ultraviolet rays can be cited.

[0183] The thickness of the bonding layer may be, for example, 1 μm or more, preferably 1 μm or more and 25 μm or less, more preferably 2 μm or more and 15 μm or less, and further preferably 2.5 μm or more and 5 μm or less.

[0184] Another embodiment of the laminate 200 of the present invention is as follows, for example Figure 2 As shown, it includes a front plate 101 , a first adhesive layer 102 , a polarizer layer 103 , a second adhesive layer 104 , and a back plate 105 , and may further include a bonding layer 108 , a first retardation layer 106 , a bonding layer 109 , and a second retardation layer 107 .

[0185] <Method for producing laminated body>

[0186] The laminates 100 and 200 can be manufactured by a method including a step of laminating the layers constituting the laminates 100 and 200 via an adhesive layer or further via an adhesive layer. When the layers are laminated via an adhesive layer or an adhesive layer, it is preferred to apply a surface activation treatment such as a corona treatment to one or both of the laminating surfaces for the purpose of improving adhesion.

[0187] The polarizer layer 103 may be directly formed on a thermoplastic resin film or a base film, and the thermoplastic resin film or the base film may be incorporated into the laminate 100 or 200 , or may be separated from the polarizer layer 103 and not become a constituent element of the laminate.

[0188] <Display device>

[0189] A display device according to one embodiment of the present invention includes the above-mentioned laminated bodies 100 and 200. The display device is not particularly limited, and examples thereof include image display devices such as organic EL display devices, inorganic EL display devices, liquid crystal display devices, and electroluminescent display devices. The display device may have a touch panel function. The above-mentioned laminated bodies 100 and 200 are suitable for display devices with flexibility such as being able to be bent or folded because the generation of bubbles is suppressed in the adhesive layer to improve durability.

[0190] In the display device, the stacked bodies 100 and 200 are arranged on the visible side of the display element of the display device with the front panel facing outward (the side opposite to the display element side, i.e., the visible side). The display device is preferably bendable with the front panel 101 side of the stacked bodies 100 and 200 as the inner side.

[0191] The display device of the present invention can be used as mobile devices such as smart phones and tablet computers, televisions, digital photo frames, electronic billboards, measuring instruments, metering instruments, office equipment, medical equipment, electronic computer equipment, etc.

[0192] Example

[0193] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples. In the present examples, "%" and "parts" mean "mass %" and "mass parts", respectively, unless otherwise specified.

[0194] [Measurement of weight average molecular weight (Mw)]

[0195] As the weight average molecular weight (Mw) converted to polystyrene, tetrahydrofuran was used as the mobile phase, and the weight average molecular weight (Mw) of the (meth) acrylic acid polymer described later was obtained by the following size exclusion chromatography (SEC). Specifically, the (meth) acrylic acid polymer to be measured was dissolved in tetrahydrofuran to a concentration of about 0.05% by mass, and 10 μL was injected into SEC. The mobile phase was passed at a flow rate of 1.0 mL / min. PLgel MIXED-B (manufactured by Polymer Laboratories) was used as a chromatographic column. A UV-VIS detector (trade name: Agilent GPC) was used as a detector.

[0196] [Measurement of thickness]

[0197] The thickness was measured using a contact-type film thickness measuring device (trade name "ZC-101", manufactured by Nikon Corporation).

[0198] [Measurement of bending rigidity]

[0199] The laminates obtained in each Example and each Comparative Example were left in an environment at a temperature of -20°C for 24 hours, taken out to an environment at 25°C, and within 5 minutes, the bending rigidity was measured under a load of 25 g using a bending rigidity evaluation device (Gurley Stiffness Tester, manufactured by Kumagai Riki Kogyo Co., Ltd.).

[0200] [Repeated deformation test]

[0201] The adhesive layer of the adhesive sheet described later is laminated to prepare a reference adhesive layer with a thickness of 150 μm. It should be noted that, for the adhesive layer of the adhesive sheet C7, since the thickness is 150 μm, it is not laminated and used directly as a reference adhesive layer. Then, the reference adhesive layer is cut into a width of 20 mm × a length of 20 mm and pasted on the carrier of the viscoelasticity measuring device (trade name "MCR-301", Anton Paar company), so that the surface of the reference adhesive layer is bonded to the measuring chip with a diameter of 8 mm. In this state, under the conditions of no force and a frequency of 1 Hz, 0% deformation and 400% deformation are repeatedly applied. The application of deformation is carried out under the following temperature conditions, that is, after the reference adhesive layer is cooled to -20 ° C, it is kept at -20 ° C for 2 minutes, and then the reference adhesive layer is heated to 60 ° C at a heating rate of 10 ° C / minute, and kept at 60 ° C for 2 minutes, and the operation is set as 1 cycle, and the operation is repeated for a total of 10 cycles. The temperature drop rate when shifting to the next cycle was set to 10° C. / min. From the stress measured in the test, the stress reduction rate (unit: %) was calculated based on the following formula (1).

[0202] Stress reduction rate = 100-{(RB / RA)×100}...(1)

[0203] [In formula (1), RA represents the stress (unit: Pa) when a 400% deformation is applied to the adhesive layer at -20°C for the first time after the start of the repeated deformation test, and RB represents the stress (unit: Pa) when a 400% deformation is applied to the adhesive layer at 60°C for the last time in the 10th cycle of the repeated deformation test.]

[0204] [Low temperature bendability test]

[0205] The laminate obtained in each embodiment and each comparative example was cut into a test piece with a width of 10 mm and a length of 100 mm using a super cutter. The test piece was wound around a cylindrical mandrel in such a way that the front panel side of the test piece was the inner side using a bending resistance tester (cylindrical mandrel method) manufactured by TP Giken Co., Ltd. In this state, the test piece was placed in an environment at a temperature of -20°C for 24 hours, and after being taken out to an environment at 25°C, the presence or absence of bubbles in the first adhesive layer and the second adhesive layer of the test piece, as well as the presence or absence of peeling between the first adhesive layer and the front layer and the peeling between the second adhesive layer and the back layer were confirmed within 5 minutes.

[0206] The above operation was performed by changing the diameter of the core rod between 30 mm, 20 mm, 15 mm, 10 mm, and 5 mm, and the minimum diameter of the core rod was determined when no bubbles were generated in the first adhesive layer and the second adhesive layer, and no peeling occurred between the first adhesive layer and the front layer and between the second adhesive layer and the back layer, and the evaluation was performed according to the following criteria. In the low-temperature bendability test, the smaller the minimum diameter of the core rod determined, the better the low-temperature bendability of the laminate. It should be noted that in any test piece, only the first adhesive layer generated bubbles or peeled off from the adjacent layer.

[0207] A: The minimum diameter of the mandrel is determined to be less than 10 mm.

[0208] B: The minimum diameter of the mandrel is determined to be 15 mm.

[0209] C: The minimum diameter of the determined mandrel is 20 mm or more.

[0210] [Heat shock bending test]

[0211] The laminate obtained in each embodiment and each comparative example was cut out with a width of 10 mm × a length of 100 mm using a super cutter to make a test piece. Using a bending resistance tester (cylindrical mandrel method) manufactured by TP Giken Co., Ltd., the test piece was wound around a cylindrical mandrel (mandrel) in such a way that the front panel side of the test piece was inside. In this state, the test piece was kept at a temperature of -20°C for 2 minutes, and then the ambient temperature was raised to 60°C at a heating rate of 10°C / min, and kept at 60°C for 2 minutes. This operation was set as 1 cycle, and the operation was repeated for a total of 10 cycles. The cooling rate when transferring to the next cycle was set to 10°C / min. After 10 cycles, the test piece was taken out of the environment at 25°C and the presence or absence of bubbles in the first adhesive layer and the second adhesive layer of the test piece, as well as the peeling between the first adhesive layer and the front layer and the peeling between the second adhesive layer and the back layer were confirmed within 5 minutes.

[0212] The above operation was performed by changing the diameter of the core rod between 30 mm, 20 mm, 15 mm, 10 mm, and 5 mm, and the minimum diameter of the core rod was determined when no bubbles were generated in the first adhesive layer and the second adhesive layer, and no peeling occurred between the first adhesive layer and the front layer and between the second adhesive layer and the back layer, and the evaluation was performed according to the following criteria. In the impact resistance bending test, the smaller the minimum diameter of the core rod determined, the better the thermal shock bending performance of the laminate. It should be noted that in any test piece, only the first adhesive layer generated bubbles or peeled off from the adjacent layer.

[0213] A: The minimum diameter of the mandrel is determined to be less than 10 mm.

[0214] B: The minimum diameter of the mandrel is determined to be 15 mm.

[0215] C: The minimum diameter of the determined mandrel is 20 mm or more.

[0216] <Preparation of (meth)acrylic acid polymers A1 to A10>

[0217] A 1L reactor equipped with a cooling device is prepared. Into the reactor, a mixture obtained by mixing the monomer components shown in Table 1 in the proportions shown in Table 1 is added while nitrogen is flowing. Then, while stirring the mixture, nitrogen is refluxed in the reactor for 1 hour to remove oxygen, and the temperature of the mixture is raised to 60°C. While maintaining the temperature at 60°C, the mixture is uniformly mixed, and then a polymerization initiator shown in Table 1 is added in the proportions shown in Table 1, and a polymerization reaction is carried out by irradiating a UV lamp (10 mW) while stirring to obtain (meth)acrylic polymers A1 to A10. The proportions shown in Table 1 represent the mass ratio (mass %) based on the total mass of the monomer components and the photopolymerization initiator. The weight average molecular weight (Mw) of the (meth)acrylic polymers A1 to A10 is shown in Table 1.

[0218] [Table 1]

[0219]

[0220] <Preparation of Adhesive Compositions B1 to B10>

[0221] The (meth)acrylic polymers A1 to A10, monomer components, fluorine-containing compounds and photopolymerization initiators shown in Table 2 were mixed in the amounts shown in Table 2 to obtain adhesive compositions B1 to B10. The amounts shown in Table 2 represent the mass ratios (mass %) based on the total mass of the (meth)acrylic polymers, monomer components, fluorine-containing compounds and photopolymerization initiators.

[0222] [Table 2]

[0223]

[0224] The abbreviations in Tables 1 and 2 are as follows.

[0225] (Monomer component)

[0226] BA: Butyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0227] n-DAM: N-dodecyl acrylamide (nitrogen-containing monomer, obtained from Tokyo Chemical Industry Co., Ltd.)

[0228] 4-HBA: 4-Hydroxybutyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0229] MA: Methyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0230] IBOA: Isobornyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0231] LA: Lauryl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0232] 2-PEA: 2-phenoxyethyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0233] C22A: Behenyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0234] n-OA: n-octyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0235] 2-EHA: 2-ethylhexyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0236] IDA: Isodecyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0237] (Fluorine-containing compounds)

[0238] TFEA: 2,2,2-trifluoroethyl acrylate (obtained from Tokyo Chemical Industry Co., Ltd.)

[0239] (Photopolymerization Initiator)

[0240] I-184: 1-Hydroxycyclohexylphenylketone (obtained from Tokyo Chemical Industry Co., Ltd.)

[0241] <Preparation of Adhesive Sheets C1 to C10>

[0242] The adhesive composition shown in Table 3 was applied to the release-treated surface of release film A (polyethylene terephthalate film coated with a release agent containing a silicone compound) so that the thickness of the adhesive layer was the thickness shown in Table 3. Release film B (polyethylene terephthalate film coated with a release agent containing a silicone compound) was laminated on the coating layer so that the release-treated surface side was the coating layer side, and then UV irradiation was performed to obtain adhesive sheets C1 to C10 having a layer structure of release film A / adhesive layer / release film B. The accumulated light intensity was 400 mJ / cm 2 , illumination is 1.8mW / cm 2 UV irradiation was performed in the manner of (UVV standard). The strain repetition test was performed using the obtained PSA layers of PSA sheets C1 to C10 to measure the stress reduction rate. The measurement results are shown in Table 3.

[0243] [Table 3]

[0244]

[0245] [Examples 1 and 2 and Comparative Example 2]

[0246] (Preparation of the front layer (1))

[0247] As the front layer (1), a front panel was prepared in which a hard coating layer (10 μm thick) was formed on one surface of a resin film (polyimide resin film, 40 μm thick) as a first substrate layer. The hard coating layer was a layer formed of a composition containing an acrylic compound having a dendritic polymer structure having a multifunctional acrylic group at the end.

[0248] (Preparation of circular polarizing plate (1))

[0249] A protective film (cycloolefin resin film, 18 μm thick) as a protective layer and a linear polarizing layer (8 μm thick) were bonded together using a water-based adhesive to obtain a linear polarizing plate (1) having a layer structure of protective layer / adhesive layer / linear polarizing layer.

[0250] Then, a phase difference laminate (1) is obtained in which a first phase difference layer (thickness 3 μm), an adhesive layer (thickness 1 μm) and a second phase difference layer (thickness 2 μm) are sequentially laminated. The first phase difference layer is a λ / 4 phase difference layer, which is a cured layer of a polymerizable liquid crystal compound. The adhesive layer is a cured layer of an epoxy adhesive as a photocurable adhesive composition. The second phase difference layer is a positive C layer, which is a cured layer of a polymerizable liquid crystal compound.

[0251] The linear polarizing layer side of the linear polarizing plate (1) obtained above and the first phase difference layer side of the phase difference laminate (1) are laminated using a laminating layer (adhesive layer using an acrylic adhesive, thickness 5 μm) to obtain a circular polarizing plate (1) as a polarizing plate. The layer structure of the circular polarizing plate (1) is linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / laminating layer / phase difference laminate (1) (first phase difference layer / adhesive layer / second phase difference layer).

[0252] (Production of Laminated Body)

[0253] The first substrate layer (resin film) side of the front layer (1) obtained above and the linear polarizing plate (1) side of the circular polarizing plate (1) are bonded using the first adhesive layer shown in Table 4, and the second adhesive layer shown in Table 4 and a spacer (50 μm) as a back layer are laminated on the phase difference laminate (1) side of the circular polarizing plate to prepare the laminates of Examples 1 to 2 and Comparative Example 2. The layer structure of these laminates is front layer (1) (hard coating layer / first substrate layer) / first adhesive layer / linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / laminating layer / phase difference laminate (1) (first phase difference layer / adhesive layer / second phase difference layer) / second adhesive layer / back layer. The obtained laminate was subjected to bending rigidity measurement, low temperature bending test and heat shock bending test. The results are shown in Table 4.

[0254] [Example 3 and Comparative Example 1]

[0255] (Preparation of circular polarizing plate (2))

[0256] A phase difference laminate (2) is obtained in which a first phase difference layer (thickness 2 μm), an adhesive layer (thickness 2 μm) and a second phase difference layer (thickness 1 μm) are sequentially laminated. The first phase difference layer is a λ / 2 phase difference layer, which is a cured layer of a polymerizable liquid crystal compound. The adhesive layer is a cured layer of an epoxy adhesive as a photocurable adhesive composition. The second phase difference layer is a λ / 4 phase difference layer, which is a cured layer of a polymerizable liquid crystal compound.

[0257] The linear polarizing layer side of the linear polarizing plate (1) obtained according to the steps described in Example 1 and the first phase difference layer side of the phase difference laminate (2) obtained above were laminated using a laminating layer (adhesive layer using an acrylic adhesive, thickness of 5 μm) to obtain a circular polarizing plate (2) as a polarizing plate. The layer structure of the circular polarizing plate (2) is linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / laminating layer / phase difference laminate (2) (first phase difference layer / adhesive layer / second phase difference layer).

[0258] (Production of Laminated Body)

[0259] The first substrate layer (resin film) side of the front layer (1) obtained according to the steps described in Example 1 is bonded to the linear polarizing plate (1) side of the circular polarizing plate (2) using the first adhesive layer shown in Table 4, and the second adhesive layer shown in Table 4 and a spacer (thickness 50 μm) as the back layer are laminated on the phase difference laminate (2) side of the circular polarizing plate to produce the laminates of Example 3 and Comparative Example 1. The layer structure of these laminates is front layer (1) (hard coating layer / first substrate layer) / first adhesive layer / linear polarizing plate (1) (protective layer / adhesive layer / linear polarizing layer) / laminating layer / phase difference laminate (2) (first phase difference layer / adhesive layer / second phase difference layer) / second adhesive layer / back layer. The obtained laminate was subjected to bending rigidity measurement, low temperature bending test and heat shock bending test. The results are shown in Table 4.

[0260] [Examples 4 to 6]

[0261] (Preparation of the front layer (2))

[0262] As the front layer (2), a front panel was prepared in which a hard coating layer (5 μm thick) was formed on one surface of a resin film (polyimide resin film, 40 μm thick) as a first substrate layer. The hard coating layer was a layer formed of a composition containing an acrylic compound having a dendritic polymer structure having a multifunctional acrylic group at the end.

[0263] (Preparation of circular polarizing plate (3))

[0264] According to the steps of [Preparation of Linear Polarizing Plate B] of the Example of Japanese Patent Publication No. 2022-185418, a linear polarizing plate (2) having a hard coating layer as a protective layer, a linear polarizing layer as a cured layer of a polymerizable liquid crystal compound, and an outer coating layer as a protective layer was prepared. The layer structure of the linear polarizing plate (2) is protective layer (hard coating layer) / aligned film / linear polarizing layer / protective layer (outer coating layer).

[0265] The protective layer (overcoat layer) side of the linear polarizing plate (2) obtained above and the first phase difference layer side of the phase difference laminate (1) obtained according to the steps described in Example 1 were laminated using a laminating layer (adhesive layer using an acrylic adhesive, thickness of 5 μm) to obtain a circular polarizing plate (3) as a polarizing plate. The layer structure of the circular polarizing plate (3) is linear polarizing plate (2) (protective layer (hard coat layer) / oriented film / linear polarizing layer / protective layer (overcoat layer)) / laminating layer / phase difference laminate (1) (first phase difference layer / adhesive layer / second phase difference layer).

[0266] (Production of Laminated Body)

[0267] The first substrate layer (resin film) side of the front layer (2) obtained above and the linear polarizing plate (2) side of the circular polarizing plate (3) were bonded together using the first adhesive layer shown in Table 4, and the second adhesive layer shown in Table 4 and a separator (thickness 50 μm) as a back layer were laminated on the phase difference laminate (1) side of the circular polarizing plate to prepare laminates of Examples 4 to 6. The layer structure of these laminates is front layer (2) (hard coating layer / first substrate layer) / first adhesive layer / linear polarizing plate (2) (protective layer (hard coating layer) / oriented film / linear polarizing layer / protective layer (outer coating layer)) / bonding layer / phase difference laminate (1) (first phase difference layer / adhesive layer / second phase difference layer) / second adhesive layer / back layer. The obtained laminates were subjected to measurement of bending rigidity, low temperature bending test and heat shock bending test.

[0268] Table 4 shows the results.

[0269] [Table 4]

[0270]

Claims

1. A laminate comprising, in order, a front panel, a first adhesive layer, a polarizer layer, a second adhesive layer and a back panel, The stress reduction rate of the first adhesive layer calculated by the following formula (1) is 40% or more and 70% or less, The stress reduction rate R1 of the first adhesive layer and the stress reduction rate R2 of the second adhesive layer satisfy the relationship of the following formula (2): Stress reduction rate = 100-{(RB / RA)×100}...(1) R1≤R2...(2) In formula (1), RA represents the stress when a 400% deformation is applied to the adhesive layer at -20°C after the start of the repeated deformation test, and RB represents the stress when a 400% deformation is applied to the adhesive layer at 60°C in the 10th cycle of the repeated deformation test, and the unit of the stress is Pa; Repeated deformation test: The repeated deformation test is carried out by the following operation, i.e., an adhesive layer adjusted to a thickness of 150 μm is bonded to a measuring chip of a viscoelasticity measuring device, and 0% deformation and 400% deformation are repeatedly applied under the conditions of no force and a frequency of 1 Hz. The temperature is maintained at -20°C for 2 minutes, and then the temperature is increased to 60°C at a heating rate of 10°C / min and maintained for 2 minutes. The above operation is set as 1 cycle, and the above operation is repeated for a total of 10 cycles.

2. The laminate according to claim 1, in, The laminate has a bending rigidity of 1000 gf·m or more and 2000 gf·m or less at a temperature of -20°C.

3. The laminate according to claim 1, in, The thickness of the first adhesive layer and the second adhesive layer are both 10 μm or more and 100 μm or less.

4. The laminate according to claim 1, in, The first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer are both layers formed of a pressure-sensitive adhesive composition containing a (meth)acrylic polymer.

5. The laminate according to claim 4, in, The (meth)acrylic polymer contains 20% by mass or more and 30% by mass or less of a structural unit derived from a nitrogen atom-containing monomer based on the total amount of the structural units.

6. The laminate according to claim 1, in, The first adhesive layer is a layer formed of a first adhesive composition containing a fluorine atom-containing compound. The content of the fluorine atom-containing compound is 5% by mass or less based on the total solid content of the first adhesive composition.

7. The laminate according to claim 1, in, The stress reduction rate R1 of the first adhesive layer and the stress reduction rate R2 of the second adhesive layer satisfy the relationship of the following formula (3). 0Pa≤(R2-R1)≤20Pa...(3).

8. The laminate according to claim 1, in, The stress reduction rate of the second adhesive layer is 40% to 70%.

9. The laminate according to claim 1, in, The thickness T1 of the first adhesive layer and the thickness T2 of the second adhesive layer satisfy the relationship of the following formula (4). 0.1≤(T1 / T2)≤4...(4). 10 . A display device comprising the laminate according to claim 1 .

11. An adhesive layer disposed between a front panel and a polarizing layer of a flexible display device, The stress reduction rate calculated by the following formula (1) is 40% or more and 70% or less; Stress reduction rate = 100-{(RB / RA)×100}...(1) In formula (1), RA represents the stress when a 400% deformation is applied to the adhesive layer at -20°C after the start of the repeated deformation test, and RB represents the stress when a 400% deformation is applied to the adhesive layer at 60°C in the 10th cycle of the repeated deformation test, and the unit of the stress is Pa; Repeated deformation test: The repeated deformation test is carried out by the following operation, i.e., an adhesive layer adjusted to a thickness of 150 μm is bonded to a measuring chip of a viscoelasticity measuring device, and 0% deformation and 400% deformation are repeatedly applied under the conditions of no force and a frequency of 1 Hz. The temperature is maintained at -20°C for 2 minutes, and then the temperature is increased to 60°C at a heating rate of 10°C / min and maintained for 2 minutes. The above operation is set as 1 cycle, and the above operation is repeated for a total of 10 cycles.