Polypropylene pre-coating film and multi-layer co-extrusion film blowing stretching preparation equipment thereof

Through the multi-layer co-extrusion blown film stretching technology of polypropylene pre-coated films, the problems of high cost and complex process of traditional pre-coated films are solved, efficient production is achieved, product quality and stability are improved, and mechanical strength and gloss are enhanced. Spend.

CN118721920APending Publication Date: 2024-10-01YANTAI FENGFULAI FILM TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410764293.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In order to improve the bonding fastness of traditional pre-coated films, a primer needs to be applied on the surface of the pre-coated film, resulting in high costs and complicated processes, and at the same time adversely affecting product quality.

Method used

It adopts multi-layer co-extrusion blown film stretching technology of polypropylene pre-coated film, and is designed from the outside to the inside, including the outer layer of polyolefin copolymer, the sub-outer layer of copolymerized polypropylene and polyolefin copolymer blend materials, and the middle layer. and sub-inner layer homopolypropylene It is a blend of ethylene and binary or ternary copolymerized polypropylene, and the inner layer is homopolymerized polypropylene, combined with co-extrusion blown film unidirectional stretching technology, eliminating the need for glue coating and drying steps, and using quartz heating tubes and bevel gear transmission mechanisms. Precisely control raw material heating and flow.

Benefits of technology

It reduces the gluing process, improves product quality and stability, enhances mechanical strength, transparency and gloss, reduces costs, and improves the composite fastness to printed products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721920A_ABST
    Figure CN118721920A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of multi-layer co-extrusion film blowing stretching, in particular to a polypropylene pre-coating film and multi-layer co-extrusion film blowing stretching preparation equipment thereof.The polypropylene pre-coating film comprises the pre-coating film, the pre-coating film sequentially comprises an outer layer, a secondary outer layer, a middle layer, a secondary inner layer and an inner layer from outside to inside, the outer layer is prepared from polyolefin copolymer, and the middle layer is prepared from polypropylene; and the secondary outer layer is prepared from co-polypropylene and polyolefin copolymer blending materials. A co-extrusion film blowing uniaxial stretching technology is adopted for production, and compared with a traditional manufacturing method, the steps of gluing, drying, ozone adding and the like are omitted. Therefore, the gluing link is reduced, the problems of unstable adhesion fastness, demolding, degumming and the like caused by non-uniform gluing are avoided, and the drying link is reduced, so that the working efficiency is improved to a certain extent, and the cost is saved. And compared with the original product with the prime coat, the product without the prime coat does not yellow after being placed for a long time, and the phenomena of roll sticking and the like in the use process are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of multi-layer co-extrusion blown film stretching, in particular to a polypropylene pre-coated film and a multi-layer co-extrusion blown film stretching preparation device. Background Art

[0002] Pre-coating refers to the process of pre-gluing and rewinding plastic film before laminating it with printed paper. Pre-coating factories first apply adhesive to the film according to the specifications and format, then rewind it for the manufacturer to choose. Lamination is then laminated with the printed matter. Lamination, also known as film application, involves coating plastic film with adhesive and bonding it to the printed matter through heating and pressurization to create a paper-plastic hybrid product. Laminated printed matter has a thin, transparent layer of plastic film, resulting in a smoother, brighter surface, improved gloss and durability, and more vivid colors and a more three-dimensional effect. It also provides waterproofing, anti-fouling, abrasion resistance, fold resistance, and chemical resistance. The traditional process for pre-coating involves extrusion-cast lamination of biaxially oriented polypropylene (BOPP) or biaxially oriented polyester (BOPET) film with an ethylene-vinyl acetate copolymer (EVA) film. The film is then slit to produce the pre-coating. Traditional pre-coated films typically require a primer coating to improve their bonding strength, which is costly, complex, and can negatively impact product quality. Therefore, the present invention provides a polypropylene pre-coated film and a multi-layer co-extrusion blown film stretching device for producing the same. Summary of the Invention

[0003] The main purpose of the present invention is to provide a polypropylene pre-coated film and a multi-layer co-extrusion blown film stretching preparation device thereof, so as to solve the problem proposed in the related art that in order to improve the bonding strength of the traditional pre-coated film, it is usually necessary to coat the surface of the pre-coated film with a primer, which has the problems of high cost and complicated process, and also has an adverse effect on product quality.

[0004] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a polypropylene pre-coating film, comprising a pre-coating film, wherein the pre-coating film comprises, from the outside to the inside, an outer layer, a sub-outer layer, a middle layer, a sub-inner layer and an inner layer, the outer layer being made of a polyolefin copolymer, the sub-outer layer being made of a copolymerized polypropylene and a polyolefin copolymer blend, the middle layer and the sub-inner layer being both made of a homopolymerized polypropylene and a binary or ternary copolymerized polypropylene blend, the inner layer being made of a homopolymerized polypropylene, the polyolefin copolymer material having a melt index of 7.5 g·(10 min)-1 and a density of 0.902 g.(Cm3)-1, and the polyolefin copolymer material being compatible with polypropylene.

[0005] Furthermore, the melt index of the copolymerized polypropylene and polyolefin copolymer blend is 2g·(10min)-1 to 8g·(10min)-1, the mass of the polypropylene accounts for 1 to 60% of the total mass of the blend, and the melt index of the homopolypropylene and binary or ternary copolymerized polypropylene blend is 1g·(10min)-1, the mass of the homopolypropylene accounts for 0 to 50% of the total mass of the blend, and the mass of the binary or ternary copolymerized polypropylene accounts for 0 to 50% of the total mass of the blend.

[0006] According to another aspect of the present invention, a multi-layer co-extrusion blown film stretching preparation device for polypropylene pre-coated film is provided, comprising a fixed box, an extruder is provided at one end of the fixed box, the extruder comprises an extrusion box, a die head is provided on one side of the extrusion box, a feeding device is provided at the top of the extrusion box near the center of one end, a winding device is provided at the other end of the fixed box, the winding device comprises a mounting column, a second motor is provided at one end of the mounting column, a cooling device is provided on one side of the winding device, an annealing device is provided on one side of the cooling device, and a stretching device is provided on one side of the annealing device.

[0007] Furthermore, a slot is provided at the center of the top of the fixed box, a fixing seat is fixedly installed at one end of the bottom of the slot, several extrusion boxes are fixedly installed on the top of the fixing seat, and the first motor is fixedly installed at the center of one end of several extrusion boxes.

[0008] Furthermore, the feeding device includes an installation box, a cavity is opened in the installation box, a threaded tube is fixedly installed at the center of the top of the installation box, a feeding column is fixedly installed on the top of the threaded tube, an inner cavity is opened in the feeding column, and a quartz heating tube is fixedly installed around the inner cavity.

[0009] Furthermore, the cavity is provided with small grooves on both sides near the bottom, and baffles are rotatably installed on the two small grooves near the top. Mounting rods are rotatably installed on both ends of the cavity near the bottom. The two mounting rods are located below one side of the two baffles. Support rods are fixedly installed at the centers of both ends of one side of the mounting rod. Bevel gears are fixedly installed at the center and both ends of the mounting rod. Rotating rods are rotatably installed at the center and both ends of both sides of the mounting box near the bottom. One end of the rotating rod is located in the cavity, and the other end of the rotating rod is higher than both sides of the mounting box.

[0010] Furthermore, the bevel gear includes a first bevel gear and a second bevel gear, the first bevel gear is fixedly mounted on one end of the rotating rod, and the second bevel gear is fixedly mounted at the center and both ends of the mounting rod.

[0011] Furthermore, support plates are provided on both sides of the mounting column, and the bottoms of the two support plates are respectively fixedly mounted on both sides of the other end of the slot, and second rotating shafts are fixedly mounted at the centers of both ends of the mounting column, one end of one of the second rotating shafts is rotatably mounted on one side of one of the support plates near the top center, the second motor is fixedly mounted on the other side of the other support plate near the top center, and one end of the other second rotating shaft passes through the other side of the other support plate near the top center and is coaxially connected to the output shaft of the second motor.

[0012] Furthermore, the cooling device includes a cooling box, a second trough body is opened through one side of the cooling box near the bottom, and second fixed plates are fixedly installed at both ends of the bottom of the cooling box; the annealing device includes an annealing box, a first trough body is opened through one side of the annealing box near the bottom, and first fixed plates are fixedly installed at both ends of the bottom of the annealing box.

[0013] Furthermore, the stretching device includes a mounting plate, which is fixedly mounted on both ends of the bottom of the slot, and a rotating column is provided at the center between the two mounting plates.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] 1. The present invention utilizes co-extrusion blown film uniaxial stretching technology for production. Compared to traditional production methods, it eliminates steps such as gluing, drying, and adding ozone. This not only reduces the gluing process, avoiding problems such as unstable adhesion, demolding, and degumming caused by uneven gluing, but also reduces the drying process, thereby improving work efficiency and saving costs to a certain extent. Compared to existing products with primers, primer-free products will not yellow due to prolonged storage, nor will they stick to the roller during use. This significantly improves product quality and stability.

[0016] 2. The present invention improves the mechanical strength, transparency and glossiness of the blown film by adopting a production method of online longitudinal stretching during co-extrusion blown film, through four steps of preheating, longitudinal stretching, annealing and cooling.

[0017] 3. The present invention uses co-extrusion blown film and adds polyolefin copolymer to the outer layer, thereby improving the composite fastness of the pre-coated film to the printed product.

[0018] 4. The present invention heats the raw materials in the inner cavity through a quartz heating tube to ensure that the raw materials reach a predetermined temperature before entering the extruder, so that they are in a suitable flow state, thereby improving the extrusion effect and product quality. By opening and closing the baffle, the flow rate of the raw materials entering the cavity from the feed column can be accurately controlled to avoid problems caused by too much or too little raw materials, such as blockage or low production efficiency.

[0019] 5. The present invention ensures stable and reliable transmission between the rotating rod and the mounting rod by using a combination of a bevel gear transmission mechanism, a sprocket and a chain, thereby ensuring smooth operation of the baffle. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the cross section of the practical pre-coating film;

[0021] Figure 2 A schematic diagram of the present invention as a whole;

[0022] Figure 3 A schematic diagram of the present invention is cut away as a whole;

[0023] Figure 4 It is a schematic diagram of the overall cross-section of the feeding device of the present invention;

[0024] Figure 5 It is a schematic diagram of a cutaway installation box of the present invention;

[0025] Figure 6 A schematic diagram of the entire A of the present invention;

[0026] Figure 7 Schematic diagram of the winding device of the present invention.

[0027] Illustration:

[0028] 1. Fixing box; 11. Slotting; 12. Fixing seat; 2. Extruder; 21. Extrusion box; 22. First motor; 3. Die head; 31. Extrusion hole; 32. Fixing rod; 33. First support rod; 34. Second support rod; 41. Mounting plate; 42. Rotating column; 421. First rotating shaft; 5. Annealing device; 51. Annealing box; 52. First trough; 53. First fixing plate; 6. Cooling device; 61. Cooling box; 62. Second trough; 63. Second fixing plate; 7. Winding device; 71. Support plate; 72. Mounting column; 721. Groove; 73. Second rotating shaft; 74. Second Motor; 75, fixed plate; 76, cutter; 8, feeding device; 81, mounting box; 811, threaded hole; 812, cavity; 813, small groove; 82, feeding column; 821, inner cavity; 822, threaded tube; 83, quartz heating tube; 84, baffle; 841, first small plate; 842, second small plate; 843, rotating rod; 844, supporting groove; 9, rotating device; 91, first bevel gear; 92, mounting rod; 93, second bevel gear; 94, supporting rod; 95, sprocket; 96, chain; 97, plate; 971, vertical plate; 972, rotating rod; 973, positioning rod;

[0029] 101, outer layer; 102, inner layer; 103, sub-inner layer; 104, middle layer; 105, sub-outer layer. DETAILED DESCRIPTION

[0030] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the specific implementation methods, structures, features and effects of the present invention are described in detail below in conjunction with the accompanying drawings and preferred embodiments.

[0031] See also Figure 1 The present embodiment provides a polypropylene pre-coating film, including a pre-coating film, which includes an outer layer 101, a sub-outer layer 105, a middle layer 104, a sub-inner layer 103 and an inner layer 102 from the outside to the inside. The outer layer 101 is made of a polyolefin copolymer, the sub-outer layer 105 is made of a blend of copolymerized polypropylene and a polyolefin copolymer, the middle layer 104 and the sub-inner layer 103 are both made of a blend of homopolypropylene and a binary or ternary copolymerized polypropylene, and the inner layer 102 is made of homopolypropylene. The polyolefin copolymer material has a melt index of 7.5 g·10 min-1 and a density of 0.902 g.cm3-1, and the polyolefin copolymer material is compatible with polypropylene.

[0032] The melt index of the copolymerized polypropylene and polyolefin copolymer blend is 2 g·10 min-1 to 8 g·10 min-1, with the mass of polypropylene accounting for 1 to 60% of the total mass of the blend. The melt index of the homopolypropylene and binary or ternary copolymerized polypropylene blend is 1 g·10 min-1, with the mass of homopolypropylene accounting for 0 to 50% of the total mass of the blend, and the mass of binary or ternary copolymerized polypropylene accounting for 0 to 50% of the total mass of the blend. It should be added that the melt index of the homopolypropylene is 1 g·(10 min)-1 to 6 g·(10 min)-1, and the total thickness of the polypropylene pre-coating film is 29 μm to 80 μm; the outer layer thickness is 10 μm to 30 μm, the sub-outer layer thickness is 5 μm to 10 μm, the middle layer thickness is 2 μm to 10 μm, the sub-inner layer thickness is 2 μm to 10 μm, and the inner layer thickness is 10 μm to 20 μm.

[0033] See also Figures 2 to 7 The present embodiment provides a multi-layer co-extrusion blown film stretching preparation equipment for a polypropylene pre-coated film, comprising a fixed box 1, an extruder 2 is provided at one end of the fixed box 1, the extruder 2 comprises an extrusion box 21, a die head 3 is provided on one side of the extrusion box 21, a feeding device 8 is provided at the top of the extrusion box 21 near the center of one end, a winding device 7 is provided at the other end of the fixed box 1, the winding device 7 comprises a mounting column 72, a second motor 74 is provided at one end of the mounting column 72, a cooling device 6 is provided on one side of the winding device 7, an annealing device 5 is provided on one side of the cooling device 6, and a stretching device is provided on one side of the annealing device 5.

[0034] A slot 11 is provided at the center of the top of the fixed box 1, a fixed base 12 is fixedly installed at one end of the bottom of the slot 11, several extrusion boxes 21 are fixedly installed on the top of the fixed base 12, and a first motor 22 is fixedly installed at the center of one end of the several extrusion boxes 21. It should be supplemented that: a fixed rod 32 is provided at the center of one side near the fixed base 12, the bottom end of the fixed rod 32 is fixedly installed at the center of the bottom of the slot 11, the bottom center of the die head 3 is fixedly installed at the top of the fixed rod 32, an outlet hole 31 is provided at the center of the top of the die head 3, and a first support rod 33 is fixedly connected to the center of the bottom of the two ends of the die head 3 near the center of the bottom, two second support rods 34 are fixedly connected to one side of the two first support rods 33, and a second support rod 34 is fixedly connected to the center of one side of the die head 3. Five extrusion boxes 21 are provided, and one end of the five second support rods 34 is fixedly connected to the center of the other end of the extrusion box 21.

[0035] The temperature inside the die 3 is 190°C to 220°C.

[0036] The feeding device 8 includes an installation box 81, which defines a cavity 812. A threaded tube 822 is fixedly mounted at the top center of the installation box 81. A feed column 82 is fixedly mounted on top of the threaded tube 822. The feed column 82 defines an inner cavity 821, and a quartz heating tube 83 is fixedly mounted around the inner cavity 821. It should be noted that a threaded hole 811 is formed through the top center of the installation box 81, communicating with the cavity 812. The threaded tube 822 is threadedly mounted within the threaded hole 811. The threaded hole 811 and the threaded tube 822 have the same diameter.

[0037] The quartz heating tube 83 is used to heat the feed column 82 .

[0038] Small grooves 813 are provided on both sides near the bottom of the cavity 812, and baffles 84 are rotatably installed in the two small grooves 813 near the top. Mounting rods 92 are rotatably installed at both ends of the cavity 812 near the bottom. The two mounting rods 92 are located below one side of the two baffles 84. Support rods 94 are fixedly installed at the center of both ends of one side of the mounting rod 92. Bevel gears are fixedly installed at the center and both ends of the mounting rod 92. Rotating rods 972 are rotatably installed at the center and both ends of both sides of the mounting box 81. One end of the rotating rod 972 is located in the cavity 812, and the other end of the rotating rod 972 is higher than both sides of the mounting box 81. It should be added that: a second small plate 842 is fixedly installed at the center and both sides of one side of the two baffles 84, and a first small plate 841 is fixedly installed near the top center and both sides of the two small grooves 813. The second small plate 842 and the first small plate 841 are rotatably connected together by a rotating rod 843. The other ends of the three rotating rods 972 are respectively fixedly installed with sprockets 95, and chains 96 are meshed and installed between the three sprockets 85. Plates 97 are fixedly installed at the centers of both sides of the installation box 81, and the plate 97 is located just below the rotating rod 972 at the center. On the other hand, vertical plates 971 are fixedly installed on both sides of the top of the plate 97 near one end, and a rotating rod 972 at the center is located between the two vertical plates 971. An opening is opened on one side of the two vertical plates 971 near the center of the top, and small holes are opened on both sides of the rotating rod 972 at the center near the other end. The diameter of the small hole is the same as that of the opening, and positioning rods 973 are installed with internal threads of the small hole and the opening. Support grooves 844 are respectively opened on both sides of the bottom of the two baffles 84, and one end of the two support rods 94 on both sides of the installation box 81 are respectively slidably installed in the support grooves 844.

[0039] The positioning rod 973 fixes the position of the rotating rod 972. The baffle 84 is set to allow the raw materials to be heated in the feed column 82. After heating to a certain temperature, the bevel gear rotates to make the support rod 94 leave the bottom of the baffle 84, so that the two baffles 84 are separated, and the raw materials enter the installation box 81 from the feed column 82.

[0040] The bevel gears include a first bevel gear 91 and a second bevel gear 93. The first bevel gear 91 is fixedly mounted on one end of the rotating rod 972, and the second bevel gear 93 is fixedly mounted at the center and both ends of the mounting rod 92. It should be added that the first bevel gear 91 and the second bevel gear 93 are vertically meshed with each other.

[0041] Support plates 71 are provided on both sides of the mounting column 72. The bottoms of the two support plates 71 are fixedly mounted on both sides of the other end of the slot 11. Second rotating shafts 73 are fixedly mounted at the centers of both ends of the mounting column 72. One end of the second rotating shaft 73 is rotatably mounted on one side of one of the support plates 71 near the top center. The second motor 74 is fixedly mounted on the other side of the other support plate 71 near the top center. One end of the other second rotating shaft 73 passes through the other side of the other support plate 71 near the top center and is coaxially connected to the output shaft of the second motor 74. It should be supplemented that a groove 721 is provided at the center of the outer wall of the mounting column 72. A fixed plate 75 is fixedly mounted on one end of the two support plates 71 near the top. One end of the fixed plate 75 is located obliquely below the mounting group 72. A cutter 76 is fixedly mounted on the top of the fixed plate 75 near the center of one end. The two cutters 76 are respectively on the same horizontal line with the two ends of the groove 721.

[0042] The cutter 76 is provided to remove irregularities from the edge of the cooled film.

[0043] The cooling device 6 includes a cooling box 61, a second trough 62 is provided on one side of the cooling box 61 near the bottom, and second fixing plates 63 are fixedly installed at both ends of the bottom of the cooling box 61. The annealing device 5 includes an annealing box 51, a first trough 52 is provided on one side of the annealing box 51 near the bottom, and first fixing plates 53 are fixedly installed at both ends of the bottom of the annealing box 51. It should be added that after the film is stretched, the film passes through the first trough 52 of the annealing box 51, and then the film passes through the second trough 62 of the cooling box 61. The bottoms of the two second fixing plates 63 are respectively fixedly installed on both sides of the bottom of the slot 11, and the bottoms of the two first fixing plates 53 are respectively fixedly installed on both sides of the bottom of the slot 11. The temperature of the annealing box 51 is 90-105°C, and the temperature of the cooling box 61 is 30-50°C.

[0044] The stretched film enters the annealing box 51 and is held at 90-105°C for a period of time. This helps eliminate internal stress in the film and improves the crystallization state, thereby increasing the film's transparency and gloss. The annealed film then enters the cooling box 61 for cooling and finalizing. During the cooling process, the film's temperature gradually drops to room temperature, solidifying its structure and properties.

[0045] The stretching device includes mounting plates 41, which are fixedly mounted at both ends of the bottom of the slot 11. A rotating column 42 is located at the center between the two mounting plates 41. It should be noted that the mounting plates 41 are L-shaped, and first rotating shafts 421 are rotatably mounted at the centers of both ends of the rotating column 42. One end of each first rotating shaft 421 is fixedly mounted within the two mounting plates 41. The rotating columns 42 are located between one end of each side of the two mounting plates 41, with three vertically downwardly mounted and one between the other ends of each side of the two mounting plates 41, and are aligned with the lowest vertically downward rotating column 42.

[0046] The specific use of the present invention is as follows: first, the baffle 84 is in the closed position, closing the passage from the feed column 82 to the cavity 812, ensuring that the raw materials are fully heated in the inner cavity 821, starting the extruder 2, and placing the five raw materials into the feed columns 82 in the five extrusion boxes 21 respectively. The quartz heating tube 83 is started for heating. When the raw materials are heated to a predetermined temperature, the baffle 84 needs to be opened to allow the raw materials to enter the cavity 812, and the positioning rod 973 is rotated to take it out from the small hole on the center rotating rod 972 and the internal thread of the opening on the vertical plate 971, and then the rotating rod 972 at the center of the mounting box 81 starts to rotate. The rotation of the rotating rod 972 drives the other two rotating rods 972 to rotate synchronously through the sprocket 95 and the chain 96. The first bevel gear 91 on each rotating rod 972 is connected to the mounting rod 9 2 and 3. The second bevel gears 93 on the rotating rod 972 mesh with each other vertically, so the rotation of the rotating rod 972 is converted into the rotation of the mounting rod 92. The rotation of the mounting rod 92 causes the support rod 94 to move, so that the support rod 94 is removed from the support groove 844 of the baffle 84, so that the baffle 84 is opened, and the raw material can enter the cavity 812 through the opened small groove 813. The heated raw material is extruded into a film through the outlet hole 31 of the die head 3. At the same time, the second motor 74 is turned on, and the directional stretching of the film is controlled by the first rotating shaft 421 on the rotating column 42 to improve the physical properties of the film. The stretched film enters the annealing box 51 for annealing to eliminate internal stress and optimize the crystallization morphology. Subsequently, the film passes through the cooling box 61 and is cooled and shaped at a low temperature of 30-50°C. The film is automatically wound in the groove 721 in the mounting column 71.

[0047] The above description is merely a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as above in terms of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art can, without departing from the scope of the technical solution of the present invention, make some changes or modifications to equivalent embodiments using the technical contents disclosed above. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A polypropylene pre-coating film, comprising a pre-coating film, characterized in that: The pre-coated film comprises, from the outside to the inside, an outer layer (101), a sub-outer layer (105), a middle layer (104), a sub-inner layer (103) and an inner layer (102), wherein the outer layer (101) is made of a polyolefin copolymer, the sub-outer layer (105) is made of a copolymerized polypropylene and a polyolefin copolymer blend, the middle layer (104) and the sub-inner layer (103) are both made of a homopolymerized polypropylene and a binary or ternary copolymerized polypropylene blend, the inner layer (102) is made of a homopolymerized polypropylene, the polyolefin copolymer material has a melt index of 7.5 g·(10min)-1 and a density of 0.902 g.(cm3)-1, and the polyolefin copolymer material is compatible with polypropylene.

2. A polypropylene pre-coating film according to claim 1, characterized in that: The melt index of the copolymerized polypropylene and polyolefin copolymer blend is 2g·(10min)-1 to 8g·(10min)-1, the mass of the polypropylene accounts for 1 to 60% of the total mass of the blend, and the melt index of the homopolypropylene and binary or ternary copolymerized polypropylene blend is 1g·(10min)-1, the mass of the homopolypropylene accounts for 0 to 50% of the total mass of the blend, and the mass of the binary or ternary copolymerized polypropylene accounts for 0 to 50% of the total mass of the blend.

3. A multi-layer co-extrusion blown film stretching production equipment for polypropylene pre-coating film, used for preparing the polypropylene pre-coating film as claimed in claim 1, comprising a fixing box (1), characterized in that: An extruder (2) is provided at one end of the fixed box (1), the extruder (2) comprises an extrusion box (21), a die head (3) is provided on one side of the extrusion box (21), a feeding device (8) is provided at the top of the extrusion box (21) near the center of one end, a winding device (7) is provided at the other end of the fixed box (1), the winding device (7) comprises a mounting column (72), a second motor (74) is provided at one end of the mounting column (72), a cooling device (6) is provided on one side of the winding device (7), an annealing device (5) is provided on one side of the cooling device (6), and a stretching device is provided on one side of the annealing device (5).

4. The multi-layer co-extrusion blown film stretching preparation equipment for polypropylene pre-coated film according to claim 3, characterized in that: A slot (11) is provided at the center of the top of the fixed box (1), a fixed seat (12) is fixedly mounted at one end of the bottom of the slot (11), a plurality of extrusion boxes (21) are fixedly mounted on the top of the fixed seat (12), and a first motor (22) is fixedly mounted at the center of one end of a plurality of the extrusion boxes (21).

5. The multi-layer co-extrusion blown film stretching preparation equipment for polypropylene pre-coated film according to claim 4, characterized in that: The feeding device (8) comprises an installation box (81), a cavity (812) is provided in the installation box (81), a threaded tube (822) is fixedly installed at the top center of the installation box (81), a feeding column (82) is fixedly installed on the top of the threaded tube (822), an inner cavity (821) is provided in the feeding column (82), and a quartz heating tube (83) is fixedly installed around the inner cavity (821).

6. The multi-layer co-extrusion blown film stretching preparation equipment for polypropylene pre-coated film according to claim 5, characterized in that: The cavity (812) is provided with small grooves (813) on both sides near the bottom, and baffles (84) are rotatably installed near the top of the two small grooves (813). Mounting rods (92) are rotatably installed at both ends of the cavity (812) near the bottom. The two mounting rods (92) are located below one side of the two baffles (84). Support rods (94) are fixedly installed at the center of both ends of one side of the mounting rod (92). Bevel gears are fixedly installed at the center and both ends of the mounting rod (92). Rotating rods (972) are rotatably installed at the center and both ends of both sides of the mounting box (81). One end of the rotating rod (972) is located in the cavity (812), and the other end of the rotating rod (972) is higher than both sides of the mounting box (81).

7. The multi-layer co-extrusion blown film stretching preparation equipment of a polypropylene pre-coated film according to claim 6, characterized in that: The bevel gear comprises a first bevel gear (91) and a second bevel gear (93). The first bevel gear (91) is fixedly mounted on one end of the rotating rod (972), and the second bevel gear (93) is fixedly mounted at the center and both ends of the mounting rod (92).

8. The multi-layer co-extrusion blown film stretching preparation equipment for polypropylene pre-coated film according to claim 7, characterized in that: Support plates (71) are provided on both sides of the mounting column (72), and the bottoms of the two support plates (71) are respectively fixedly mounted on both sides of the other end of the slot (11), and second rotating shafts (73) are fixedly mounted at the centers of both ends of the mounting column (72), one end of one of the second rotating shafts (73) is rotatably mounted on one side of one of the support plates (71) near the top center, and the second motor (74) is fixedly mounted on the other side of the other support plate (71) near the top center, and one end of the other second rotating shaft (73) passes through the other side of the other support plate (71) near the top center and is coaxially connected to the output shaft of the second motor (74).

9. The multi-layer co-extrusion blown film stretching preparation equipment of polypropylene pre-coated film according to claim 8, characterized in that: The cooling device (6) comprises a cooling box (61), a second trough (62) is provided through one side of the cooling box (61) near the bottom, and second fixing plates (63) are fixedly installed at both ends of the bottom of the cooling box (61); the annealing device (5) comprises an annealing box (51), a first trough (52) is provided through one side of the annealing box (51) near the bottom, and first fixing plates (53) are fixedly installed at both ends of the bottom of the annealing box (51).

10. The multi-layer co-extrusion blown film stretching preparation equipment of polypropylene pre-coated film according to claim 9, characterized in that: The stretching device comprises a mounting plate (41), wherein the mounting plate (41) is fixedly mounted at two ends of the bottom of the slot (11), and a rotating column (42) is provided at the center between the two mounting plates (41).

Citation Information

Patent Citations

  • Polypropylene biaxially oriented film without primary coat and preparation method thereof

    CN102863919A

  • Pre-coating film without primer coating, two-way stretch polypropylene film thereof and preparation method of polypropylene film

    CN102873953A

  • BOPP pre-coated basement membrane without primer coatings and preparation method thereof

    CN104139592A

  • Biaxially oriented polypropylene lamination film base material as well as preparation method and application thereof

    CN105479884A

  • BOPP pre-coating film with high peel strength and preparation method of BOPP pre-coating film

    CN106273972A