Wafer level transfer structure and transfer method thereof

By forming MEMS chips on wafers and utilizing the fracture transfer technology of connecting pillars, the problems of low integration and large parasitic effects in MEMS integrated packaging are solved, achieving efficient MEMS chip integration and reducing process complexity.

CN118723911APending Publication Date: 2024-10-01SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310314056.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing MEMS integrated packaging technology has problems such as low integration and large parasitic effects, resulting in long R&D cycles, high costs and low manufacturing efficiency.

Method used

Using the wafer-level transfer structure and transfer method, by forming the MEMS chip on the first wafer and setting the connecting pillars to deform the suspended part until it breaks, the MEMS chip is transferred to the second wafer to achieve face-to-face bonding. Avoid wire bonding parasitics and reduce process complexity through temperature differences and applied stresses.

Benefits of technology

It improves the integration of MEMS chips on the wafer, avoids parasitic effects caused by wire bonding, improves the preparation efficiency of MEMS integrated circuits, and reduces process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723911A_ABST
    Figure CN118723911A_ABST
Patent Text Reader

Abstract

The invention provides a wafer level transfer structure and a transfer method thereof, and the method comprises the steps: preparing an MEMS chip on a first wafer, and enabling the MEMS chip to be connected with the first wafer only through a connecting column; the second wafer and the first wafer are bonded through the MEMS chip; and applying a transverse shear force or a temperature difference to the surfaces of the first wafer and the second wafer, so that the suspended part of the connecting column is deformed to be fractured, and the MEMS chip is transferred from the first wafer to the second wafer. According to the method, the MEMS chip is prepared and then transferred to the wafer for integration, so that the integration level of the MEMS chip on the wafer can be improved; meanwhile, the MEMS chip is transferred in a face-to-face bonding mode, so that the parasitic effect generated by lead bonding is avoided; in addition, the MEMS chip is directly prepared on the wafer, so that the preparation efficiency of the MEMS integrated circuit is improved; and finally, in cooperation with a temperature difference and stress application method, the process complexity is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor integrated circuit manufacturing, and in particular relates to a wafer-level transfer structure and a transfer method thereof. Background Art

[0002] Micro-Electro-Mechanical System (MEMS) is a technology that goes beyond Moore's Law by integrating electromechanical sensitive structures with execution structures and processing circuits to realize system-level chips that integrate information sensing, processing, storage, transmission and even execution. Realizing mechanical and electrical integration is the development goal of MEMS technology, but the development of integration technology is not smooth.

[0003] As early as the 1980s, MEMS products with monolithic integration of electromechanical sensors and processing circuits appeared, but in practice, a series of problems with monolithic integration technology were also found. First, in order to achieve monolithic integration, it is necessary to optimize processing technology and related materials to meet the needs of both electromechanical functional structures and integrated circuits. However, there are inconsistencies between the requirements of electromechanical functional structures and integrated circuits for processing technology. Compromise optimization will inevitably cause a slight decrease in the performance of both, while significantly increasing the complexity of the technology. Secondly, the development process of integrated circuits and MEMS technologies is different, and the cost of maintaining the advancement of monolithic integration process lines is extremely high. Integrated circuit technology is developing rapidly in accordance with Moore's Law. At present, the minimum line width is less than 5nm, and the frequency and other performance of CMOS devices also increase as the minimum line width decreases. On the other hand, the performance of many MEMS devices such as inertial sensors will decrease as the structural size decreases, and the development speed of MEMS processing technology in terms of minimum line width and other indicators is significantly slower than that of integrated circuit technology. While developing integrated circuit processing technology in accordance with Moore's Law, maintaining support for MEMS technology will undoubtedly significantly increase the R&D cost of the process line. In addition, the tape-out cycle of monolithic integrated MEMS products is significantly longer than that of discrete products, and the testing difficulty of monolithic integrated MEMS products is also significantly higher than that of discrete MEMS products. The R&D cycle of monolithic integrated MEMS products is long and the R&D cost is high.

[0004] Since the 1990s, mainstream MEMS products have generally adopted a technical route of discrete processing and then achieving system-level integration with processing circuits in the packaging stage. However, the use of system-level packaging technology to integrate MEMS and integrated circuits can optimize MEMS and integrated circuits independently, and has significant advantages in terms of R&D cycle and R&D cost. However, this type of technical route will inevitably sacrifice integration and volume, and the preparation efficiency is also low. In addition, the parasitic effects introduced by system-level packaging technology are also significantly greater than monolithic integration technology. Obviously, the development direction of system-level packaging integration technology is to improve integration and preparation efficiency, reduce volume and parasitic effects while maintaining performance and cost advantages.

[0005] It should be noted that the above introduction to the technical background is only for the convenience of providing a clear and complete description of the technical solutions of the present application and for the convenience of understanding by those skilled in the art. It cannot be considered that the above technical solutions are well known to those skilled in the art simply because these solutions are described in the background technology part of the present application. Summary of the invention

[0006] In view of the above shortcomings of the prior art, an object of the present invention is to provide a wafer-level transfer structure and a transfer method thereof, so as to solve the problems of integration and parasitic effects of MEMS integrated packaging in the prior art.

[0007] To achieve the above object, the present invention provides a wafer-level transfer method, the method comprising:

[0008] providing a first wafer;

[0009] Forming a MEMS chip on the first wafer, and providing connecting pillars so that the first wafer and the MEMS chip are connected only through the connecting pillars, and a suspended portion of the connecting pillars is exposed between the first wafer and the MEMS chip;

[0010] Bonding the first wafer to the second wafer via the MEMS chip, so that an effective electrical connection is formed between the MEMS chip and the second wafer;

[0011] The suspended portion of the connecting column is deformed until it breaks, so that the MEMS chip is transferred from the first wafer to the second wafer.

[0012] Optionally, the absolute value of the positive stress generated along the axial direction of the connecting column when the first wafer is bonded to the second wafer is less than the absolute value of the fracture stress of the connecting column, and the fracture stress is the maximum compressive stress that the cross section of the connecting column can withstand without breaking; the absolute value of the positive stress generated along the axial direction of the connecting column when the first wafer is bonded to the second wafer is less than the absolute value of the buckling stress of the connecting column, and the buckling stress is the positive stress that causes the resonant frequency of the connecting column to drop to 0 and causes buckling; the absolute value of the positive stress generated along the axial direction of the connecting column when the first wafer is bonded to the second wafer is less than the absolute value of the yield stress of the connecting column at the bonding temperature, and the yield stress is the minimum positive stress that causes the connecting column to yield.

[0013] Optionally, when the first wafer is bonded to the second wafer, the process temperature of the first wafer is T1, the process temperature of the second wafer is T2, ɑ is the thermal expansion coefficient of the connecting column, R is the radius of the first wafer, and w s is the minimum displacement of the MEMS chip relative to the first wafer when the connecting column is broken, and the first wafer and the second wafer are bonded to each other when:

[0014] Optionally, the method for deforming the suspended portion of the connecting column to break is: applying lateral shear forces to the surfaces of the first wafer and the second wafer connected to the connecting column respectively, and the two lateral shear forces are opposite in direction and equal in magnitude.

[0015] Optionally, the absolute value of the maximum surface stress of the connecting column caused by the transverse shear force is greater than the absolute value of the fracture stress of the connecting column.

[0016] Optionally, the method for deforming the suspended portion of the connecting column to the point of fracture is: setting the surface temperature of the first wafer connected to the connecting column to T3, and the surface temperature of the second wafer to T4, and then setting The connecting pillars that are more than R1 away from the center of the first wafer are all broken; and then forces of equal magnitude and opposite directions are applied to the first wafer and the second wafer at the same time, so that the other connecting pillars are all broken.

[0017] Optionally, the connecting column includes a chip portion H located in the MEMS chip, a suspended portion L between the first wafer and the MEMS chip, and a wafer portion L located in the first wafer. a , L a is 1-50 microns, and L is 5-80 microns.

[0018] Optionally, a first pad is provided on a surface of the connecting column on the MEMS chip away from the first wafer, a second pad is provided on a surface of the second wafer close to the connecting column, and the MEMS chip is connected to the second pad on the second wafer via the first pad.

[0019] Optionally, the bonding method between the first wafer and the second wafer includes one or any combination of gold-gold hot pressure welding, gold-silicon eutectic welding, gold-tin solder bonding, copper-tin solder bonding, and copper-copper hot pressure welding.

[0020] The present invention also provides a wafer-level transfer structure, and the wafer-level transfer structure is obtained using any one of the wafer-level transfer methods described above.

[0021] As described above, the wafer-level transfer structure and transfer method of the present invention have the following beneficial effects:

[0022] The present invention improves the integration degree of the MEMS chip on the wafer by preparing the MEMS chip and then transferring it to the wafer for integration;

[0023] The present invention utilizes face-to-face bonding to transfer the MEMS chip, thereby avoiding the parasitic effects caused by wire bonding;

[0024] The present invention improves the preparation efficiency of MEMS integrated circuits by directly preparing MEMS chips on wafers;

[0025] The invention combines the temperature difference with the method of applying stress, thereby reducing the complexity of the process. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic structural diagram of forming a MEMS chip on a first wafer in step 2 of the first embodiment of the present invention.

[0027] Figure 2 It is a schematic diagram of the structure presented by forming deep holes on the first wafer in step 2.1 in the first embodiment of the present invention.

[0028] Figure 3 It is a schematic diagram of the structure presented by setting the first barrier layer and low stress polysilicon in step 2.2 in the first embodiment of the present invention.

[0029] Figure 4 It is a schematic diagram of the structure presented by planarizing the surface of the first wafer in step 2.3 in the first embodiment of the present invention.

[0030] Figure 5 It is a schematic diagram of the structure presented by setting the second barrier layer and the MEMS structure in step 2.4 in the first embodiment of the present invention.

[0031] Figure 6 It is a schematic diagram of the structure presented by forming a deep groove in step 2.5 in the first embodiment of the present invention.

[0032] Figure 7 It is a schematic diagram of the structure presented by growing the third barrier layer in step 2.6 in the first embodiment of the present invention.

[0033] Figure 8 It is a schematic diagram of the structure presented by etching the bottom of the deep groove in step 2.7 in the first embodiment of the present invention.

[0034] Fig. 9 It is a schematic diagram of the structure presented by removing the silicon under the MEMS chip in step 2.8 in the first embodiment of the present invention.

[0035] Fig.10 It is a schematic diagram showing the structure of the metal electrode prepared in step 2.9 of the first embodiment of the present invention.

[0036] Fig.11 It shows an enlarged schematic diagram of the structure of the connecting column in the first embodiment of the present invention.

[0037] Fig.12 It is a schematic diagram of the structure presented by the bonding of the first wafer and the second wafer in step 3 in the first embodiment of the present invention.

[0038] Fig.13 It is a schematic diagram of the structure of forming a second pad on a second wafer in the first embodiment of the present invention.

[0039] Fig.14 It is a schematic diagram of the structure presented by bonding the second wafer with the second pad in the first embodiment of the present invention.

[0040] Fig.15 It is a schematic diagram of the structure presented by the broken connecting column after the second wafer with the second pad is bonded in the first embodiment of the present invention.

[0041] Fig.16 It is a schematic structural diagram showing the deformation of the suspended portion of the connecting column in step 4 in the first embodiment of the present invention.

[0042] Fig.17 It is a schematic diagram showing an enlarged structure of the deformation of the suspended portion of the connecting column in step 4 in the first embodiment of the present invention.

[0043] Fig.18 It is a schematic diagram of the structure presented when the suspended part of the connecting column is broken in step 4 in the first embodiment of the present invention.

[0044] Component number description

[0045] 11. First wafer; 12. MEMS chip; 13. Connecting column; 131. Chip part; 132. Suspended part; 133. Wafer part; 14. First pad; 15. Second pad; 151. Chromium layer; 152. Platinum layer; 153. First gold layer; 154. Amorphous silicon layer; 155. Titanium layer; 156. Second gold layer; 16. Second wafer;

[0046] 21. deep hole; 22. first barrier layer; 23. low stress polysilicon; 24. second barrier layer; 25. MEMS structure; 26. deep trench; 261. bottom of deep trench; 27. third barrier layer; 28. metal electrode. DETAILED DESCRIPTION

[0047] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0048] For example, when describing the embodiments of the present invention in detail, for the sake of convenience, the schematic diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.

[0049] For convenience of description, spatially relative terms such as "under", "below", "below", "below", "above", "on", etc. may be used herein to describe the relationship of one element or feature shown in the drawings to other elements or features. It will be understood that these spatially relative terms are intended to encompass other orientations of the device in use or operation in addition to the orientation depicted in the drawings.

[0050] In the context of the present application, a structure in which a first feature is described as being "above" a second feature may include embodiments in which the first and second features are in direct contact, and may also include embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.

[0051] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and therefore the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0052] The present invention provides a wafer-level transfer method, the method comprising:

[0053] Step 1: providing a first wafer 11;

[0054] Step 2: forming a MEMS chip 12 on the first wafer 11, and providing a connecting column 13, so that the first wafer 11 and the MEMS chip 12 are connected only through the connecting column 13, and a suspended portion 132 of the connecting column 13 is exposed between the first wafer 11 and the MEMS chip 12;

[0055] Step 3: Bonding the first wafer 11 to the second wafer 16 via the MEMS chip 12 to form an effective electrical connection between the MEMS chip 12 and the second wafer 16;

[0056] Step 4: Deform the suspended portion 132 of the connection pillar 13 until it breaks, so that the MEMS chip 12 is transferred from the first wafer 11 to the second wafer 16 .

[0057] The wafer-level transfer method of the present invention will be described in detail below in conjunction with the accompanying drawings. It should be noted that the above sequence does not strictly represent the sequence of the wafer-level transfer method protected by the present invention, and those skilled in the art may change it according to the actual preparation steps.

[0058] First, step 1 is performed to provide a first wafer 11 .

[0059] Then, if Figure 1 As shown, step 2 is performed to form a MEMS chip 12 on the first wafer 11, and to set a connecting column 13 so that the first wafer 11 and the MEMS chip 12 are connected only through the connecting column 13, and a suspended portion 132 of the connecting column 13 is exposed between the first wafer 11 and the MEMS chip 12.

[0060] In one embodiment, the step of forming the MEMS chip 12 supported by the connecting pillars 13 on the first wafer 11 by the (111) silicon wafer processing process includes:

[0061] Step 2.1: Figure 2 As shown, a deep hole 21 is formed on the first wafer 11;

[0062] Step 2.2: If Figure 3 As shown, a first barrier layer 22 is provided to cover the surface of the first wafer 11 and the deep hole 21, and a low-stress polysilicon 23 is provided to completely fill the deep hole 21;

[0063] Step 2.3: If Figure 4 As shown, the surface of the first wafer 11 is planarized, and the connection pillars 13 and the first barrier layer 22 are manufactured;

[0064] Step 2.4: If Figure 5 As shown, a second barrier layer 24 is fabricated on the surface of the first wafer 11, and a MEMS structure 25 is fabricated using a (111) processing technique;

[0065] Step 2.5: If Figure 6 As shown, a deep groove 26 is formed by photolithography and etching, and the deep groove 26 surrounds the MEMS structure 25 to form a closed pattern;

[0066] Step 2.6: If Figure 7 As shown, a third barrier layer 27 is grown on the surface of the deep trench 26;

[0067] Step 2.7: If Figure 8 As shown, the third barrier layer 27 on the surface of the second barrier layer 24 and the bottom 261 of the deep groove is removed, and the bottom 261 of the deep groove is etched;

[0068] Step 2.8: If Fig. 9 As shown, the first wafer 11 is corroded to remove the silicon under the MEMS chip 12, so that the MEMS chip 12 is supported only by the connecting pillars 13;

[0069] Step 2.9: If Fig.10 As shown, lead holes and metal electrodes 28 are prepared.

[0070] Specifically, in step 2.1, a deep hole 21 is formed on the first wafer 11 by photolithography and / or DRIE (deep reactive ion etching) process.

[0071] Specifically, in step 2.1, the material of the first wafer 11 is (111) silicon, and the angle between the surface of the first wafer 11 and the (111) crystal plane is less than or equal to 1°.

[0072] Specifically, in step 2.2, the depth of the deep hole 21 is equal to the total length of the connecting column 13, and the cross-sectional area of ​​the deep hole 21 is equal to the sum of the cross-sectional areas of the connecting column 13 and the first barrier layer 22 on its surface.

[0073] Specifically, the material and thickness of the first barrier layer 22 in step 2.2 must be able to withstand the subsequent anisotropic wet etching process for etching and releasing the MEMS chip 12.

[0074] Specifically, the material of the first barrier layer 22 in step 2.2 includes, but is not limited to, silicon dioxide generated by thermal oxidation, silicon dioxide produced by LPCVD (low pressure chemical vapor deposition) process, low stress silicon nitride and other thin film materials.

[0075] Specifically, in step 2.2, the low stress polysilicon 23 is filled by using LPCVD process or epitaxial process.

[0076] Specifically, the material of the second barrier layer 24 in step 2.4 needs to be able to withstand the subsequent (111) processing technology and the release process of the MEMS chip 12. The material of the second barrier layer 24 includes but is not limited to silicon dioxide and low-stress silicon nitride layers made by LPCVD process. The (111) processing technology for making the MEMS structure 25 includes but is not limited to MIS (minimally invasive surgery) process.

[0077] Specifically, in step 2.5, since the release corrosion process is lateral corrosion, the corrosion depth δ will be respectively increased and decreased based on the set etching width W0. Therefore, in order to ensure that the width W of the movable part of the connecting column 13 obtained by corrosion meets the expectation, the depth of the deep groove 26 is X, the thickness of the MEMS structure 25 is Y, and the structural dimensions are set to satisfy X=Y+δ.

[0078] Specifically, in step 2.6, the third barrier layer 27 can be made of but not limited to silicon dioxide, low stress silicon nitride, silicon carbide, etc., and can be prepared by processes such as but not limited to LPCVD, PECVD (plasma enhanced chemical vapor deposition), thermal oxidation, etc.

[0079] Specifically, in step 2.7, the third barrier layer 27 on the surface of the second barrier layer 24 and the bottom 261 of the deep trench is removed by reactive ion etching (RIE).

[0080] Specifically, in step 2.7, the deep groove bottom 261 is etched by DRIE method, and the depth of etching the deep groove bottom 261 is set to satisfy W0=W-2δ.

[0081] Specifically, in step 2.8, an anisotropic wet etching solution is used to etch the first wafer 11. The anisotropic wet etching solution may be, but is not limited to, TMAH (tetramethylammonium hydroxide) and KOH (potassium hydroxide).

[0082] Specifically, in step 2.9, the lead hole and the metal electrode 28 are prepared using a process that the mechanical strength of the structure in the previous step can withstand. The metal electrode 28 can be selected according to the requirements of the bonding process.

[0083] In one embodiment, the MEMS chip 12 has a length of 0.1-10 mm, a width of 0.1-10 mm, and a thickness of 1-50 mm.

[0084] In one embodiment, Fig.11 As shown, the connecting column 13 includes a chip portion 131H located in the MEMS chip 12, a suspended portion 132L between the first wafer 11 and the MEMS chip 12, and a wafer portion 133L located in the first wafer 11. a , L a is 1-50 microns, and L is 5-80 microns.

[0085] Specifically, the maximum radius of the connection column 13 is equal to the maximum thickness that can be achieved by the polysilicon filling process. In this embodiment, LPCVD is used to deposit polysilicon for filling. In the MEMS process, the thickness of LPCVD deposited polysilicon generally does not exceed 2 microns, so the radius of the silicon column generally does not exceed 2 microns.

[0086] Specifically, the maximum length of the connecting column 13 is determined by the maximum aspect ratio of deep reactive ion etching, and the ratio of the length of the connecting column 13 to the diameter radius of the connecting column 13 is less than or equal to the maximum aspect ratio.

[0087] Then, if Fig.12 As shown, step 3 is performed to bond the first wafer 11 to the second wafer 16 via the MEMS chip 12 , so that an effective electrical connection is formed between the MEMS chip 12 and the second wafer 16 .

[0088] In one embodiment, the absolute value of the positive stress generated along the axial direction of the connecting column 13 when the first wafer 11 and the second wafer 16 are bonded is less than the absolute value of the fracture stress of the connecting column 13, and the fracture stress is the maximum compressive stress that the cross section of the connecting column 13 can withstand without breaking; the absolute value of the positive stress generated along the axial direction of the connecting column 13 when the first wafer 11 and the second wafer 16 are bonded is less than the absolute value of the buckling stress of the connecting column 13, and the buckling stress is the positive stress that causes the resonant frequency of the connecting column 13 to drop to 0 and causes buckling; the absolute value of the positive stress generated along the axial direction of the connecting column 13 when the first wafer 11 and the second wafer 16 are bonded is less than the absolute value of the yield stress of the connecting column 13 at the bonding temperature, and the yield stress is the minimum positive stress that causes the connecting column 13 to yield.

[0089] Specifically, when the first wafer 11 and the second wafer 16 are bonded, the average normal stress generated on each of the connecting pillars 13 along the axial direction of the connecting pillar 13 is T L , F b is the pressure applied to the connecting pillars 13 during bonding, N is the number of the connecting pillars 13, and A i is the cross-sectional area of ​​the i-th connecting column 13, then it needs to satisfy:

[0090]

[0091] When the bonding pressure is P and the area of ​​the MEMS chip 12 is A, F b =PA;

[0092] T s is the fracture stress, T bis the buckling stress, T y is the yield stress at bonding temperature, by setting N and A i Make T L Satisfies: |T L |<|T s |,|T L |<|T b | and|T L |<|T y |.

[0093] Specifically, when the material of the connecting column 13 is silicon, since silicon is a brittle material, its fracture stress is very sensitive to the defect density and structure within the material, and its measurement data is distributed in a wide range from several hundred MPa to several GPa. During preparation, the fracture stress can be taken as 500 MPa or the precise value can be obtained through experiments.

[0094] Specifically, for a homogeneous cylindrical silicon connecting column 13 with a radius of r and a length of L of the suspended portion 132, the buckling stress expression is: Where E is the Young's modulus of silicon. The buckling stress of the connecting column 13 of other cross sections can be obtained by calculating the axial stress when the resonant frequency drops to 0 through finite element simulation, or by experiment. The buckling stress can be greater than or less than the fracture stress, which is related to the size of the connecting column 13.

[0095] In one embodiment, the buckling stress is 3.37 GPa, and at a bonding temperature of 400° C., the yield stress of the connecting column 13 is 300 MPa.

[0096] In one embodiment, when the first wafer 11 is bonded to the second wafer 16, the process temperature of the first wafer 11 is T1, the process temperature of the second wafer 16 is T2, ɑ is the thermal expansion coefficient of the connecting column 13, R is the radius of the first wafer 11, and w s is the minimum displacement of the MEMS chip 12 relative to the first wafer 11 when the connecting pillar 13 is broken, and the first wafer 11 and the second wafer 16 are bonded to each other to satisfy:

[0097] Specifically, since the MEMS chip 12 is supported by the connecting pillars 13, and the cross-sectional area of ​​the connecting pillars 13 is significantly smaller than the cross-sectional area of ​​the MEMS chip 12, the heat dissipation capacity of the MEMS chip 12 is significantly reduced. During the bonding process, when the temperature of the MEMS chip 12 is different from that of the first wafer 11, the MEMS chip 12 except the center of the first wafer 11 will be displaced relative to the first wafer 11 due to thermal expansion and contraction, thereby causing the connecting pillars 13 to deform. The present invention designs the process temperature of the first wafer 11 and the second wafer 16 to ensure that any connecting pillar 13 will not break due to temperature difference during the bonding process.

[0098] In one embodiment, for a wafer with a diameter of 100 mm, the temperature difference between the first wafer 11 and the second wafer 16 during bonding is less than 5° C.

[0099] Specifically, when the cross section is a simple geometric shape and the length L is much greater than When s It can be obtained by analytical formula. For example, for a homogeneous silicon column with a cylindrical cross section, it satisfies: For silicon columns with complex cross-sections and materials, the finite element method is used to calculate w s , and design it.

[0100] In one embodiment, the bonding temperature is 400°C and the bonding pressure is 4×10 5 Pa, the temperature difference between the first wafer 11 and the second wafer 16 is less than 5° C., and the bonding time is 30 minutes.

[0101] In one embodiment, Figure 13-Figure 15 As shown, a first pad 14 is provided on the surface of the connecting column 13 on the MEMS chip 12 away from the first wafer 11 , and a second pad is provided on the surface of the second wafer 16 close to the connecting column 13 . The MEMS chip 12 is connected to the second pad on the second wafer 16 via the first pad 14 .

[0102] In one embodiment, the metal electrode 28 disposed on the first wafer 11 is a stacked electrode composed of chromium, platinum and gold (not shown in the figure), which serves as the first pad 14 on the first wafer 11 for gold-silicon eutectic bonding.

[0103] In one embodiment, Fig.13 As shown, a first stacked electrode consisting of a chromium layer 151, a platinum layer 152, and a first gold layer 153 is arranged on the second wafer 16, an amorphous silicon layer 154 is arranged on the first stacked electrode, and a second stacked electrode consisting of a titanium layer 155 and a second gold layer 156 is arranged on the amorphous silicon layer 154, and a second pad corresponding to the first pad 14 on the first wafer 11 is obtained on the second wafer 16 after photolithography and etching.

[0104] In one embodiment, the bonding method between the first wafer 11 and the second wafer 16 includes one or any combination of gold-gold hot pressing welding, gold-silicon eutectic welding, gold-tin solder bonding, copper-tin solder bonding, and copper-copper hot pressing welding.

[0105] In this embodiment, the first wafer 11, the second wafer 16, and the connecting pillars 13 are all made of silicon. Specifically, practitioners can select other suitable materials according to the application.

[0106] In one embodiment, the second wafer 16 includes a plurality of units, each unit having a length of 660 microns and a width of 280 microns.

[0107] In one embodiment, the second wafer 16 is a silicon-based, glass-based or ceramic-based transfer plate wafer, and an integrated circuit can be disposed on the wafer.

[0108] In one embodiment, the bonding temperature is less than or equal to 400° C., and the time at 400° C. is less than or equal to 30 minutes.

[0109] Then, if Figure 16-18 As shown, step 4 is performed to deform the suspended portion 132 of the connecting column 13 until it breaks, so that the MEMS chip 12 is transferred from the first wafer 11 to the second wafer 16 .

[0110] In the prior art, the MEMS chip 12 is packaged on a PCB (printed circuit board), or the two-dimensional integrated wiring of the MEMS is performed on a silicon substrate, or the MEMS is wire-bonded on the integrated chip through stacked packaging. However, since the PCB process occupies a large volume, the area occupied by the two-dimensional integration is also large, and the wire bonding method is prone to parasitic effects at the wire connection.

[0111] The present invention improves the integration level of the MEMS chip 12 on the wafer by preparing the MEMS chip 12 and then transferring it to the wafer for integration. At the same time, since the MEMS chip 12 is transferred by face-to-face bonding, the parasitic effects caused by wire bonding in the prior art are avoided. In addition, the MEMS chip 12 is directly prepared on the wafer and then cut into pieces, thereby improving the preparation efficiency of the MEMS integrated circuit.

[0112] In one embodiment, the method for deforming the suspended portion 132 of the connecting column 13 to break is: applying lateral shear forces to the surfaces of the first wafer 11 and the second wafer 16 connected to the connecting column 13, respectively, and the two lateral shear forces are opposite in direction and equal in magnitude.

[0113] In one embodiment, a shear force of more than 320 N is applied to the upper and lower surfaces of the bonded structure to break all the connecting pillars 13 to obtain a transferred structure.

[0114] In one embodiment, the absolute value of the maximum surface stress of the connecting column 13 caused by the transverse shear force is greater than the absolute value of the fracture stress of the connecting column 13 .

[0115] Specifically, when the cross section is a simple geometric shape and the length L is much greater than When , the maximum surface stress caused by lateral deformation can be obtained by analytical formula. For example, for a homogeneous silicon column with a cylindrical cross section, the minimum lateral shear force F on the designed chip is j , the number of connecting columns 13 N, the hanging length of the connecting column 13 L, the radius of the connecting column 13 r i , T s is the fracture stress, and the maximum surface stress T caused by the transverse shear force on the connecting column 13 M ,satisfy For the connection column 13 with complex cross-section and material, the finite element method is used to calculate the maximum surface stress and perform the design.

[0116] In one embodiment, the method for deforming the suspended portion 132 of the connecting column 13 to break is: setting the surface temperature of the first wafer 11 connected to the connecting column 13 to T3, and the surface temperature of the second wafer 16 to T4, and then setting The connecting pillars 13 that are greater than R1 from the center of the first wafer 11 are all broken; and then, forces of equal magnitude and opposite directions are applied to the first wafer 11 and the second wafer 16 at the same time, so that the other connecting pillars 13 are all broken.

[0117] Specifically, since the stress required to fracture all the connecting columns 13 using stress is very large, a relatively complex stress applying device is required. The present invention reduces the complexity of the process by first applying a temperature difference to fracture some of the connecting columns 13 and then applying stress to fracture the remaining connecting columns 13.

[0118] The present invention also provides a wafer-level transfer structure, and the wafer-level transfer structure is obtained using any one of the wafer-level transfer methods described above.

[0119] In summary, the wafer-level transfer structure and transfer method of the present invention can improve the integration of MEMS chips on wafers by preparing MEMS chips and then transferring them to wafers for integration; at the same time, MEMS chips are transferred by face-to-face bonding, thereby avoiding the parasitic effects of wire bonding; in addition, MEMS chips are directly prepared on wafers, thereby improving the preparation efficiency of MEMS integrated circuits; finally, the method of combining temperature difference and stress application reduces the process complexity.

[0120] Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.

[0121] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A wafer-level transfer method, characterized in that: The method comprises: providing a first wafer; Forming a MEMS chip on the first wafer, and providing connecting pillars so that the first wafer and the MEMS chip are connected only through the connecting pillars, and a suspended portion of the connecting pillars is exposed between the first wafer and the MEMS chip; Bonding the first wafer to the second wafer via the MEMS chip, so that an effective electrical connection is formed between the MEMS chip and the second wafer; The suspended portion of the connecting column is deformed until it breaks, so that the MEMS chip is transferred from the first wafer to the second wafer.

2. The wafer-level transfer method according to claim 1, characterized in that: The absolute value of the normal stress on the connecting column along the axial direction of the connecting column generated by the first wafer and the second wafer when bonding is smaller than the absolute value of the fracture stress of the connecting column, and the fracture stress is the maximum compressive stress that the cross section of the connecting column can withstand without breaking; The absolute value of the normal stress generated on the connecting column along the axial direction of the connecting column when the first wafer is bonded to the second wafer is smaller than the absolute value of the buckling stress of the connecting column, and the buckling stress is the normal stress that causes the resonant frequency of the connecting column to drop to 0 and buckle; The absolute value of the positive stress generated on the connecting column along the axial direction of the connecting column when the first wafer is bonded to the second wafer is less than the absolute value of the yield stress of the connecting column at the bonding temperature, and the yield stress is the minimum positive stress that causes the connecting column to yield.

3. The wafer-level transfer method according to claim 1, characterized in that: When the first wafer is bonded to the second wafer, the process temperature of the first wafer is T1, the process temperature of the second wafer is T2, ɑ is the thermal expansion coefficient of the connecting column, R is the radius of the first wafer, and w s is the minimum displacement of the MEMS chip relative to the first wafer when the connecting column is broken, and the first wafer and the second wafer are bonded to each other when:

4. The wafer-level transfer method according to claim 1, characterized in that: The method for deforming the suspended part of the connecting column to fracture is: applying lateral shear forces to the surfaces of the first wafer and the second wafer connected to the connecting column respectively, wherein the two lateral shear forces are in opposite directions and have the same magnitude.

5. The wafer-level transfer method according to claim 4, characterized in that: The absolute value of the maximum surface stress caused by the transverse shear force on the connecting column is greater than the absolute value of the fracture stress of the connecting column.

6. The wafer-level transfer method according to claim 1, characterized in that: The method for deforming the suspended part of the connecting column to the point of fracture is as follows: setting the surface temperature of the first wafer connected to the connecting column to T3 and the surface temperature of the second wafer to T4, then setting The connecting pillars that are more than R1 away from the center of the first wafer are all broken; and then forces of equal magnitude and opposite directions are applied to the first wafer and the second wafer at the same time, so that the other connecting pillars are all broken.

7. The wafer-level transfer method according to claim 1, characterized in that: The connecting column includes a chip portion H located in the MEMS chip, a suspended portion L between the first wafer and the MEMS chip, and a wafer portion L located in the first wafer. a , L a is 1-50 microns, and L is 5-80 microns.

8. The wafer-level transfer method according to claim 1, characterized in that: A first pad is disposed on a surface of the connection column on the MEMS chip away from the first wafer, a second pad is disposed on a surface of the second wafer close to the connection column, and the MEMS chip is connected to the second pad on the second wafer via the first pad.

9. The wafer-level transfer method according to claim 1, characterized in that: The bonding method between the first wafer and the second wafer includes one or any combination of gold-gold hot pressing welding, gold-silicon eutectic welding, gold-tin solder bonding, copper-tin solder bonding, and copper-copper hot pressing welding.

10. A wafer-level transfer structure, characterized in that: The wafer-level transfer structure is obtained using the wafer-level transfer method described in any one of claims 1-9.