Ferronickel phosphide material as well as preparation method and application thereof
By gradually introducing phosphine gas into contact with the nickel-based metal after vacuuming in the reaction vessel, the problem of uneven phosphating in the preparation of nickel-phosphide-based materials is solved, and the uniformity of the nickel-iron phosphide material is improved. and catalytic activity, suitable for large-scale applications.
Patent Information
- Application Number
- CN202310325933.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing nickel phosphide-based material preparation methods have problems with phosphating inhomogeneity during large-scale or mass production, resulting in low energy conversion efficiency and difficulty in ensuring consistency of the electrode sheet, limiting its industrial application.
By gradually introducing phosphine gas into the reaction vessel after vacuuming, until the gas pressure reaches a preset value, it fully contacts the nickel-based metal, and then heats and phosphates to ensure uniformity and consistency, and prepare uniformly grown nanoparticles. Nickel iron phosphide material with chip array structure.
The uniformity and consistency of the nickel iron phosphide material is improved, the contact area between the electrolyte and the electrode is increased, the catalytic activity is improved, and it is suitable for large-scale application and reduces the cost.
Smart Images

Figure CN118723945A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a method for preparing a nickel-iron phosphide material, the nickel-iron phosphide material prepared by the preparation method, and applications of the nickel-iron phosphide material. Background Art
[0002] With the development of science and technology, facing the depletion of energy, the use of water splitting technology to produce hydrogen is an effective measure to alleviate energy pressure, reduce carbon emissions, and achieve green and sustainable development. Water splitting includes oxygen evolution reaction (OER) at the anode and hydrogen evolution reaction (HER) at the cathode. Currently, the commonly used OER catalysts are RuO2 or IrO2-based materials, and the commonly used HER catalysts are Pt / C materials. However, these precious metal catalysts have problems such as low reserves, high prices and poor stability, which also limits their widespread use. Therefore, seeking efficient non-precious metal water electrolysis catalysts has become a hot topic of research.
[0003] Among various non-precious metal catalysts, transition metal sulfides, selenides, phosphides and other non-precious metal-based electrocatalysts have been widely reported and have achieved good results in practical applications. Among them, metal phosphides have great potential in industrial applications due to their advantages such as low cost, good stability and low overpotential. The methods commonly used to prepare transition metal phosphide electrode sheets include gas phase phosphating method, hydrothermal method, electrophosphating method, etc. Among them, the gas phase phosphating method usually heats sodium hypophosphite and nickel-containing metal sheets in the same tubular furnace, and uses the phosphine gas generated by the thermal decomposition of sodium hypophosphite to phosphate the metal sheet to generate a phosphide catalyst on the surface. This method has the following problems: when sodium hypophosphite is thermally decomposed to produce phosphine, the metal precursor has reached a temperature at which the phosphating reaction can occur. When preparing large-sized materials, uneven phosphating is prone to occur, especially when preparing large quantities of samples, and consistency is difficult to ensure, which further hinders the industrial application of the gas phase phosphating method.
[0004] Therefore, it is of great practical significance to develop a method for preparing large-area phosphide electrode sheets with good uniformity and to improve the energy conversion efficiency of the electrode sheets. Summary of the invention
[0005] In view of this, the present application provides a nickel-iron phosphide material and a preparation method and application thereof, aiming to improve the problem of uneven preparation of existing nickel-phosphide-based nickel-iron phosphide materials.
[0006] The embodiment of the present application is implemented as follows: a method for preparing a nickel-iron phosphide material comprises the following steps:
[0007] Providing a nickel-based metal, wherein the nickel-based metal includes nickel and iron, and placing the nickel-based metal in a reaction container;
[0008] Evacuating the reaction vessel;
[0009] Phosphine gas is continuously introduced into the vacuumed reaction container. When the gas pressure in the reaction container reaches a preset pressure, the reaction container is heated to a temperature T. The nickel-based metal is kept warm for a period of time t at the preset pressure and temperature T to obtain a nickel-iron phosphide material.
[0010] Optionally, in some embodiments of the present application, the method for preparing the nickel-based metal includes:
[0011] Providing a nickel material, and soaking the nickel material in an acidic solution to obtain a first intermediate;
[0012] Soaking the first intermediate in pure water to obtain a second intermediate;
[0013] The second intermediate is immersed in an iron source solution to obtain a nickel-based metal.
[0014] Optionally, in some embodiments of the present application, the nickel material includes one or more of nickel foam and nickel alloy; and / or
[0015] The acidic solution includes one or more of hydrochloric acid, nitric acid, sulfuric acid, hydrobromic acid, hydroiodic acid, and hydrofluoric acid; and / or
[0016] The iron source includes one or more of ferric nitrate, ferric nitrate hydrate, ferric chloride, ferric chloride hydrate, ferric acetate, ferric acetate hydrate, ferric carbonate, ferric carbonate hydrate, ferrous chloride, ferrous chloride hydrate, ferrous acetate, ferrous acetate hydrate, ferrous carbonate, and ferrous carbonate hydrate.
[0017] Optionally, in some embodiments of the present application, the nickel alloy contains nickel element, and the mass fraction of nickel is 60% to 95%; and / or
[0018] The nickel alloy contains iron element, and the mass fraction of the iron is 0-40%.
[0019] Optionally, in some embodiments of the present application, the concentration of the acidic solution is 0.1 to 5 mol / L; and / or
[0020] The mass ratio of the nickel material to the acidic solution is 1:(5-100); and / or
[0021] The nickel material is immersed in the acidic solution for 0.5 to 3 hours; and / or
[0022] The mass ratio of the first intermediate to the pure water is 1:(10-100); and / or
[0023] The first intermediate is immersed in pure water for 5 to 48 hours; and / or
[0024] The molar concentration of the iron source is 0.1 to 1 mol / L; and / or
[0025] The mass ratio of the second intermediate to the iron source solution is 1:(5-100); and / or
[0026] The second intermediate is immersed in the iron source solution for 0.5 to 5 hours.
[0027] Optionally, in some embodiments of the present application, the vacuum flow rate is 30 to 50 mL / min; and / or
[0028] After the vacuuming, the gas pressure in the reaction container is less than 0.05 MPa.
[0029] Optionally, in some embodiments of the present application, the flow rate of the phosphine gas is 10 to 60 mL / min; and / or
[0030] In the phosphine gas, the partial pressure of phosphine molecules accounts for 20% to 95%; and / or
[0031] The temperature of the phosphine gas is 10°C to 80°C.
[0032] Optionally, in some embodiments of the present application, the preset pressure is 0.05-0.2 MPa; and / or
[0033] The heating rate is 0.5-10°C / min; and / or
[0034] The temperature T is 300-500° C.; and / or
[0035] The insulation time t is 0.5h to 5h; and / or
[0036] During the heating and the heat preservation process, the phosphine gas is continuously introduced.
[0037] Optionally, in some embodiments of the present application, the heat preservation further includes cooling after a period of time t.
[0038] Optionally, in some embodiments of the present application, the cooling rate is 0.5-10°C / min.
[0039] Correspondingly, the present application also provides a nickel-iron phosphide material prepared by the above preparation method.
[0040] Correspondingly, the present application also provides an electrode, comprising the nickel-iron phosphide material prepared by the above preparation method, or comprising the above nickel-iron phosphide material.
[0041] Correspondingly, the present application also provides a water electrolysis device, comprising the above-mentioned electrode.
[0042] The preparation method of the nickel-iron phosphide material described in the present application first extracts the gas in the reaction container to avoid spontaneous combustion when the phosphine gas is introduced, then introduces the phosphine gas into the reaction container, and after the gas pressure in the reaction container reaches a preset pressure, that is, after the phosphine gas is fully and evenly in contact with the nickel-based metal in the reaction container, heating is turned on to carry out the phosphating reaction, thereby ensuring uniform phosphating of the nickel-based metal; when preparing large quantities or large-sized nickel-iron phosphide materials, the consistency between batches and the uniformity of phosphating of each large-sized part can be improved; the microstructure of the prepared nickel-iron phosphide material is a uniformly grown nanosheet array, which helps to increase the contact area between the electrolyte and the electrode and improve the catalytic activity; the preparation method provided by the present application is simple to operate, low-cost, and suitable for large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0044] Figure 1 is a flow chart of a method for preparing a nickel-based metal phosphide nickel-iron material provided in an embodiment of the present application;
[0045] Figure 2 This is an optical photograph of the nickel-based metal nickel-iron phosphide material provided in Example 1 of the present application;
[0046] Figure 3 This is an optical photograph of the nickel-based metal nickel-iron phosphide material provided in the comparative example of the present application;
[0047] Figure 4 is a scanning electron microscope image of the nickel-based metal nickel-iron phosphide material provided in Example 1 of the present application;
[0048] Figure 5 This is a scanning electron microscope image of the nickel-based metal nickel-iron phosphide material provided in the comparative example of the present application;
[0049] Figure 6 This is the XRD diagram of the nickel-based metal nickel-iron phosphide material provided in Example 1 of the present application. DETAILED DESCRIPTION
[0050] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0051] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.
[0052] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0053] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0054] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0055] The technical solution of this application is as follows:
[0056] In a first aspect, an embodiment of the present application provides a method for preparing a nickel-iron phosphide material, comprising the following steps:
[0057] Step S11: providing a nickel-based metal, wherein the nickel-based metal includes nickel and iron, and placing the nickel-based metal in a reaction container;
[0058] Step S12: evacuating the reaction container;
[0059] Step S13: continuously introduce phosphine gas into the vacuumized reaction container, and when the gas pressure in the reaction container reaches a preset pressure, heat the reaction container to a temperature T, and keep the nickel-based metal warm for a period of time t at the preset pressure and temperature T to obtain a nickel-iron phosphide material.
[0060] The preparation method of the nickel-iron phosphide material described in the present application first extracts the gas in the reaction container to avoid spontaneous combustion when the phosphine gas is introduced, then introduces the phosphine gas into the reaction container, and after the gas pressure in the reaction container reaches a preset pressure, that is, after the phosphine gas is fully and evenly in contact with the nickel-based metal in the reaction container, heating is turned on to carry out the phosphating reaction, thereby ensuring uniform phosphating of the nickel-based metal; when preparing large batches or large-sized nickel-iron phosphide materials, the consistency between batches and the uniformity of phosphating of each large-sized part can be improved; the microstructure of the prepared nickel-iron phosphide material is a uniformly grown nanosheet array, which helps to increase the contact area between the electrolyte and the electrode and improve the catalytic activity; the preparation method provided by the present application is simple to operate, low-cost, and suitable for large-scale application.
[0061] In the step S11:
[0062] In some embodiments, the method for preparing the nickel-based metal comprises:
[0063] Step S111: providing a nickel material, and soaking the nickel material in an acidic solution to obtain a first intermediate;
[0064] Step S112: Soaking the first intermediate in pure water to obtain a second intermediate;
[0065] Step S113: soaking the second intermediate in an iron source solution to obtain a nickel-based metal.
[0066] In step S111:
[0067] In some embodiments, the nickel material includes one or more of nickel foam and nickel alloy.
[0068] In some embodiments, the nickel material is an ultrasonically cleaned nickel material. It is understandable that during the transportation and storage of the nickel material, it is difficult to avoid the generation of oil and dust on the surface of the nickel material. Ultrasonic cleaning can effectively remove the oil and dust, facilitating the subsequent preparation of nickel-based metals.
[0069] In some embodiments, the ultrasonic cleaning includes acetone cleaning, anhydrous ethanol cleaning and deionized water cleaning. The acetone cleaning and anhydrous ethanol cleaning can remove oil stains on the surface of the nickel material, and the deionized water cleaning can remove dust on the surface of the nickel material.
[0070] In some embodiments, the time of acetone cleaning, anhydrous ethanol cleaning and deionized water cleaning is independently 5 to 60 minutes, for example, 5 to 60 minutes, 8 to 50 minutes, 10 to 40 minutes, 15 to 30 minutes, 20 to 25 minutes, etc. Within the time range of the ultrasonic cleaning, it is beneficial to effectively remove oil impurities on the surface of the nickel material.
[0071] In at least one embodiment, the ultrasonic cleaning is to place the nickel material in acetone, anhydrous ethanol and deionized water in sequence and clean it for 30 minutes each.
[0072] It is understood that the size and shape of the nickel material are not limited. For example, the size of the nickel material is 1 cm×1 cm, 10 cm×10 cm, 60 cm×60 cm, 50 cm×100 cm or 100 cm×100 cm, etc.; the shape of the nickel material is square, rectangular, circular or any irregular shape, etc.
[0073] In some embodiments, the nickel alloy contains nickel element, and the mass fraction of the nickel element is 60% to 95%, for example, 62% to 92%, 65% to 90%, 68% to 88%, 70% to 85%, 75% to 80%, etc. Within the mass fraction range, the content of the nickel element is high, and the phosphating reaction can be fully carried out to generate nickel-iron phosphide material.
[0074] In some embodiments, the nickel alloy contains iron, and the mass fraction of the iron is 0-40%, for example, 5-38%, 8-35%, 10-32%, 15-30%, 20-25%, etc. Within the mass range, the iron can increase the color, toughness, flatness and hardness of the nickel alloy.
[0075] It can be understood that the nickel alloy contains some other impurity elements, and the impurity elements include one or more of Cr, Si, S, and C.
[0076] In some embodiments, the acidic solution includes one or more of hydrochloric acid, nitric acid, sulfuric acid, hydrobromic acid, hydroiodic acid, and hydrofluoric acid. The acidic solution can remove the oxide on the surface of the nickel material and dissolve the nickel material to produce Ni 2+ .
[0077] In some embodiments, the concentration of the acidic solution is 0.1-5 mol / L, for example, 0.2-4.5 mol / L, 0.5-4 mol / L, 1-3.5 mol / L, 1.5-3 mol / L, 2-2.5 mol / L, etc. Within the molar concentration range, it is beneficial for the acidic solution to fully contact and react with the nickel material.
[0078] In some embodiments, the mass ratio of the nickel material to the acidic solution is 1:(5-100), for example, 1:(10-90), 1:(15-80), 1:(20-70), 1:(30-60), 1:(40-50), etc. Within the mass ratio range, the acidic solution can fully dissolve the nickel element in the nickel material.
[0079] In some embodiments, the nickel material is immersed in the acidic solution for 0.5 to 3 hours, for example, 0.6 to 2.8 hours, 0.8 to 2.6 hours, 1 to 2.5 hours, 1.2 to 2.2 hours, 1.5 to 2 hours, etc. Within the immersion time range, the acidic solution can effectively remove the oxide on the surface of the nickel material and dissolve the nickel material.
[0080] It can be understood that when the nickel material is nickel foam, the first intermediate contains nickel and nickel salt, and the nickel salt contains Ni 2+ When the nickel material is a nickel alloy, the first intermediate contains nickel, a nickel salt and an iron salt, wherein the nickel salt contains Ni 2 + The iron salt contains Fe 3+ .
[0081] In step S112:
[0082] In some embodiments, the mass ratio of the first intermediate to the pure water is 1:(10-100), for example, 1:(15-95), 1:(20-90), 1:(30-80), 1:(40-70), 1:(50-60), etc. Within the mass ratio range, the pure water can fully convert the nickel salt into nickel hydroxide or nickel-iron hydroxide, thereby promoting the synthesis of nickel-based metals.
[0083] In some embodiments, the first intermediate is immersed in pure water for 5 to 48 hours, for example, 10 to 45 hours, 12 to 42 hours, 15 to 40 hours, 20 to 35 hours, 24 to 30 hours, etc. Within the immersion time range, the pure water can fully convert the nickel salt into nickel hydroxide, thereby promoting the synthesis of the nickel-based metal.
[0084] It can be understood that the second intermediate contains nickel hydroxide.
[0085] In step S113:
[0086] In some embodiments, the iron source includes one or more of ferric nitrate, ferric nitrate hydrate, ferric chloride, ferric chloride hydrate, ferric acetate, ferric acetate hydrate, ferric carbonate, ferric carbonate hydrate, ferrous chloride, ferrous chloride hydrate, ferrous acetate, ferrous acetate hydrate, ferrous carbonate, and ferrous carbonate hydrate.
[0087] In some embodiments, the molar concentration of the iron source is 0.1-1 mol / L, for example, 0.15-0.9 mol / L, 0.2-0.8 mol / L, 0.3-0.7 mol / L, 0.4-0.6 mol / L, 0.5-0.55 mol / L, etc. It is understood that Fe 3+ The binding capacity with OH- is stronger than Ni 2+ , part of Ni 2+ Fe 3+ In nickel-iron phosphide materials, nickel can produce a bimetallic synergistic effect with iron, and a small amount of iron doping can significantly improve the performance of nickel-iron phosphide materials.
[0088] In some embodiments, the mass ratio of the second intermediate to the iron source solution is 1:(5-100), for example, 1:(10-90), 1:(20-80), 1:(30-70), 1:(40-60), 1:(50-55). Within the mass ratio range, the iron ions in the iron source can partially replace the nickel ions in the second intermediate.
[0089] In some embodiments, the second intermediate is immersed in the iron source solution for 0.5 to 5 hours, for example, 0.5 to 4.5 hours, 0.8 to 4.2 hours, 1 to 4 hours, 1.5 to 3 hours, 2 to 2.5 hours, etc. Within the immersion time range, the iron ions in the iron source can partially replace the nickel ions in the second intermediate.
[0090] In some embodiments, after soaking the second intermediate in an iron source solution, the process further comprises drying to obtain a nickel-based metal.
[0091] In some embodiments, the drying temperature is 50-90°C, for example, 52-85°C, 55-80°C, 58-78°C, 60-75°C, 65-70°C, etc.; the drying time is 5-48h, for example, 10-45h, 12-42h, 15-40h, 20-35h, 24-30h, etc. Within the drying temperature and time range, it is beneficial to remove the solvent and improve the purity of the reaction product nickel iron phosphide material.
[0092] In some embodiments, the nickel-based metal contains nickel-iron hydroxide, including hydroxide and oxyhydroxide, the main component of which is FeNi(OH) x and Ni 1-x Fe x OOH.
[0093] The reaction vessel includes a tubular furnace. The volume of the reaction vessel is not limited. In some embodiments, the volume of the reaction vessel is 3 to 15 dm 3 , for example, 4 to 13 dm 3 , 5~12dm 3 , 6~11dm 3 , 7~10dm 3 , 8~9dm 3 wait.
[0094] In step S12:
[0095] It can be understood that there is air in the reaction container. Since phosphine gas is easily self-igniting in the air, the reaction container is first vacuumed.
[0096] In some embodiments, the vacuum flow rate is 30-50 mL / min, for example, 32-48 mL / min, 33-46 mL / min, 35-45 mL / min, 36-42 mL / min, 38-40 mL / min, etc. Within the flow rate range, the air in the reaction container can be effectively removed.
[0097] In some embodiments, after the vacuuming, the process further includes introducing and extracting an inert gas. It is understood that introducing and extracting an inert gas can further reduce the oxygen content in the reaction container, prevent spontaneous combustion of phosphine gas, and ensure reaction safety.
[0098] It should be noted that the number of times of introducing and extracting the inert gas is not limited, and can be 1 time, 3 times, 5 times, 10 times, etc. The more times of extraction, the lower the oxygen content in the reaction container can be ensured. In some embodiments, the inert gas includes one or more of argon, nitrogen, helium, neon, krypton and xenon.
[0099] In some embodiments, the reaction container comprises a gas outlet, and when the gas is extracted, the gas outlet is in an open state, and when the inert gas is introduced, the gas outlet is in a closed state.
[0100] In some embodiments, after the vacuum is drawn, the gas pressure in the reaction container is less than 0.05 MPa, for example, it may be 0.005-0.045 MPa, 0.01-0.04 MPa, 0.02-0.03 MPa, etc. Within the gas pressure range, the oxygen content in the reaction container can be ensured to be in a relatively low range, thereby avoiding the spontaneous combustion of phosphine.
[0101] In step S13:
[0102] In some embodiments, the phosphine gas is prepared from a phosphine gas generator connected to the reaction vessel.
[0103] In some embodiments, in the phosphine gas generator, the phosphine gas is prepared from sodium hypophosphite or calcium hypophosphite.
[0104] In some embodiments, when the phosphine gas is introduced, the gas outlet is in an open state. It is understood that the gas outlet of the reaction vessel can be connected to an exhaust gas treatment device, and during the entire process of introducing the phosphine gas and the phosphating reaction, the gas outlet is in an open state, and the exhaust gas treatment device can perform exhaust gas treatment on the phosphine gas flowing out of the reaction vessel to prevent it from flowing into the air and causing atmospheric pollution.
[0105] In some embodiments, the flow rate of the phosphine gas is 10-60 mL / min, for example, 12-55 mL / min, 15-50 mL / min, 18-45 mL / min, 20-40 mL / min, 25-35 mL / min, etc. Within the flow rate range, the flow rate of the phosphine gas is stable and can effectively react with the nickel-based metal.
[0106] In some embodiments, the partial pressure ratio of phosphine molecules in the phosphine gas is 20% to 95%, for example, 25% to 90%, 30% to 85%, 35% to 80%, 40% to 70%, 50% to 60%, etc. It can be understood that the phosphine gas is a mixture containing phosphine molecules, water and other impurity gases, and within the partial pressure ratio range, the phosphine molecules can effectively phosphate the nickel-based metal.
[0107] In some embodiments, the temperature of the phosphine gas is 10-80° C., for example, 15-75° C., 20-70° C., 30-60° C., 35-55° C., 40-50° C., etc. In this way, when the phosphine gas is introduced, it is beneficial for the phosphine gas to be evenly distributed in the reaction container, thereby promoting the uniform reaction of the phosphine gas and the nickel-based metal.
[0108] It can be understood that first filling the reaction container with the phosphine gas and then performing heat treatment is conducive to the uniform reaction of the phosphine gas and the nickel-based metal, thereby improving the uniformity of the nickel-iron phosphide material.
[0109] In some embodiments, the preset pressure is 0.05-0.2 MPa, for example, 0.06-0.18 MPa, 0.08-0.16 MPa, 0.1-0.15 MPa, 0.11-0.14 MPa, 0.12-0.13 MPa, etc. Within the preset pressure range, the phosphine gas is in uniform and sufficient contact with the nickel-based metal, and the safety of the reaction between the phosphine gas and the nickel-based metal is ensured.
[0110] In some embodiments, the heating rate is 0.5-10°C / min, for example, 1-9.5°C / min, 2-9°C / min, 2.5-8°C / min, 3-7°C / min, 4-6°C / min, etc. Within the heating rate range, the heating rate is gentle, thereby promoting uniform phosphating treatment.
[0111] In some embodiments, the temperature T is 300-500°C, for example, 320-480°C, 340-460°C, 350-450°C, 360-440°C, 380-420°C, 390-400°C, etc.
[0112] In some embodiments, the insulation time t is 0.5 to 5 hours, for example, 0.8 to 4.5 hours, 1 to 4.2 hours, 1.5 to 4 hours, 2 to 3.5 hours, 2.5 to 3.2 hours, 2.6 to 2.8 hours, etc. Thus, within the insulation temperature and time range, it is beneficial for the phosphine gas to effectively phosphate the nickel-based metal.
[0113] In some embodiments, the phosphine gas is continuously introduced during the heating and heat preservation process. Before obtaining the nickel-iron phosphide material, the gas pressure in the reaction container is controlled at 0.05-0.2 MPa.
[0114] In some embodiments, the heat preservation further includes cooling down after a period of time t.
[0115] In some embodiments, the cooling rate is 0.5-10°C / min, for example, 1-9.5°C / min, 2-9°C / min, 2.5-8°C / min, 3-7°C / min, 4-6°C / min, etc. Within the cooling rate range, the cooling rate is gentle, so that the performance of the nickel-iron phosphide material is stable.
[0116] It should be noted that the main component of the nickel-based metal includes Ni2P containing part of Ni and Fe.
[0117] In a second aspect, an embodiment of the present application further provides a nickel-iron phosphide material, wherein the nickel-iron phosphide material is prepared by the above-mentioned method for preparing the nickel-iron phosphide material.
[0118] The nickel-iron phosphide material described in the present application is prepared by reacting phosphine gas and nickel-based metal after sufficient and uniform contact. The nickel-iron phosphide material has good uniformity and good consistency between different batches, and exhibits excellent water decomposition performance.
[0119] In a third aspect, an embodiment of the present application also provides an application of the nickel-iron phosphide material obtained by the above-mentioned preparation method.
[0120] In some embodiments, the applications include but are not limited to electrodes and water electrolysis devices.
[0121] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.
[0122] Example 1
[0123] This embodiment provides a nickel-iron phosphide material, and the preparation method thereof is as follows:
[0124] Provide nickel foam, cut into 4 pieces of nickel material with a size of 20 cm×40 cm, put into acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 30 minutes, take out and put in an oven at 60° C. for 12 hours, and then take out for use;
[0125] The dried sample was placed in a 3 mol / L hydrochloric acid solution and soaked for 1.5 h. After being taken out and cleaned, it was placed in pure water and soaked for 24 h. Then, it was placed in a 0.1 mol / L ferric nitrate solution and soaked for 1 h. After being washed with deionized water, it was dried at 60°C for 12 h for later use.
[0126] The above samples were placed in a tubular furnace with a diameter of 8 cm and a length of 1 m. The air inlet of the tubular furnace was connected to a phosphine gas generator. The tubular furnace was first evacuated at a rate of 50 mL / min, and then filled with nitrogen. After evacuation and filling for 3 times, the gas pressure in the tubular furnace was controlled to be 0.01 MPa, and phosphine gas with a partial pressure of 60%, a temperature of 25°C, and a flow rate of 30 mL / min was introduced to make the gas pressure of the tubular furnace reach 0.05 MPa;
[0127] The phosphating reaction was carried out by heat treatment in a tubular furnace, the temperature was raised from room temperature to 350°C at a heating rate of 2°C / min, kept at that temperature for 2h, cooled to room temperature at a cooling rate of 5°C / min, and then taken out to obtain phosphated nickel-iron material.
[0128] Example 2
[0129] This embodiment is substantially the same as the embodiment 1, except that in this embodiment, the nickel foam is replaced by a nickel-iron alloy, wherein the nickel content is 95% and the iron content is 5%.
[0130] Example 3
[0131] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the partial pressure of phosphine gas accounts for 20%.
[0132] Example 4
[0133] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the partial pressure of phosphine gas accounts for 95%.
[0134] Example 5
[0135] This embodiment is substantially the same as Embodiment 1, except that the flow rate of the phosphine gas in this embodiment is 10 mL / min.
[0136] Example 6
[0137] This embodiment is substantially the same as Embodiment 1, except that the flow rate of the phosphine gas in this embodiment is 60 mL / min.
[0138] Example 7
[0139] This embodiment is substantially the same as embodiment 1, except that the temperature of the phosphating reaction in this embodiment is 300°C.
[0140] Example 8
[0141] This embodiment is substantially the same as embodiment 1, except that the temperature of the phosphating reaction in this embodiment is 500°C.
[0142] Example 9
[0143] This embodiment is basically the same as Embodiment 1, except that the holding time of the phosphating reaction in this embodiment is 0.5 h.
[0144] Example 10
[0145] This embodiment is basically the same as Embodiment 1, except that the holding time of the phosphating reaction in this embodiment is 5 hours.
[0146] Embodiment 11
[0147] This embodiment is substantially the same as Embodiment 1, except that in this embodiment, hydrochloric acid is replaced by sulfuric acid.
[0148] Example 12
[0149] This embodiment is basically the same as Embodiment 1, except that in this embodiment, ferric nitrate is replaced by ferric acetate.
[0150] Comparative Example
[0151] This comparative example is basically the same as Example 1, except that a burning boat is placed upstream of the tube furnace and loaded with 3.3 g of sodium hypophosphite monohydrate sample, the burning boat is kept open, and the sample soaked and treated with ferric nitrate solution is placed downstream of the tube furnace;
[0152] The air inlet of the tubular furnace is connected to nitrogen. The tubular furnace is first evacuated, and then nitrogen is introduced to fill the tubular furnace. After continuous evacuation and filling for 3 times, the vacuum pump is turned off, and then the air outlet of the tubular furnace is opened, and the flow rate of nitrogen is maintained at 70 mL / min. Heat treatment reaction is carried out, and sodium hypophosphite monohydrate is decomposed to obtain phosphine gas. The phosphine gas reacts with the treated nickel foam to obtain nickel-iron phosphide material.
[0153] The nickel-iron phosphide materials in Example 1 and the comparative example were photographed with an optical camera, and the photos of the nickel-iron phosphide materials were as follows: Figure 2 and Figure 3 shown.
[0154] Depend on Figure 2 It can be seen that the nickel iron phosphide material prepared in Example 1 has good uniformity and high consistency. Figure 3It can be seen that the nickel-iron phosphide material in the comparative example is not uniform and has a clear dividing line. This is because the generation of phosphine and the phosphating reaction in the comparative example are carried out in one device. When heating to produce phosphine, the sodium hypophosphite upstream of the tubular furnace gas flow is thermally decomposed to produce phosphine, and the nickel foam has also reached a temperature at which the phosphating reaction can occur. The local phosphating reaction begins before the tubular furnace is filled with phosphine, and most of the generated phosphine gas is consumed by the nickel foam at the front end, so the phosphating is uneven during preparation. In Example 1, the generation of phosphine gas and the phosphating reaction are assigned to different positions, the phosphine gas is first filled into the pre-evacuated tubular furnace, and then the tubular furnace is heated for the phosphating reaction, which can ensure that the gas is fully in contact with the metal sheet during the phosphating process, thereby improving the uniformity of the nickel-iron phosphide material.
[0155] The nickel-iron phosphide materials in Example 1 and the comparative example were subjected to scanning electron microscopy test, and the scanning electron microscopy images of the nickel-iron phosphide materials were obtained as shown in FIG. Figure 4 and Figure 5 shown.
[0156] Depend on Figure 4 and Figure 5 It can be seen that the surface of the nickel-iron phosphide material in the comparative example is uneven, with bumps and cracks, indicating that the nickel-iron phosphide material in the comparative example is not uniformly phosphated, while relative to the comparative example, the uniformity and consistency of the nickel-iron phosphide material in Example 1 are significantly improved, the surface phosphine gas is in full and uniform contact with the nickel foam, the phosphating reaction is carried out, and a uniform and consistent nickel-iron phosphide material is obtained.
[0157] The nickel-iron phosphide material of Example 1 was subjected to an X-ray diffraction test to obtain an XRD pattern of the nickel-iron phosphide material as shown in Figure 6 shown.
[0158] Depend on Figure 6 It can be seen that after the phosphating reaction, the main component of the nickel-iron phosphide material obtained is Ni2P. Ni2P has the advantages of low cost, high performance, and low overpotential, and has great potential for application in electrodes and water electrolysis devices.
[0159] The nickel iron phosphide material, preparation method and application thereof provided in the embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing nickel-iron phosphide material, characterized in that: The steps include: Providing a nickel-based metal, wherein the nickel-based metal includes nickel and iron, and placing the nickel-based metal in a reaction container; Evacuating the reaction container; Phosphine gas is continuously introduced into the vacuumed reaction container. When the gas pressure in the reaction container reaches a preset pressure, the reaction container is heated to a temperature T. The nickel-based metal is kept warm for a period of time t at the preset pressure and temperature T to obtain a nickel-iron phosphide material.
2. The preparation method according to claim 1, characterized in that: The preparation method of the nickel-based metal comprises: Providing a nickel material, and soaking the nickel material in an acidic solution to obtain a first intermediate; Soaking the first intermediate in pure water to obtain a second intermediate; The second intermediate is immersed in an iron source solution to obtain a nickel-based metal.
3. The preparation method according to claim 2, characterized in that: The nickel material includes one or more of nickel foam and nickel alloy; and / or The acidic solution includes one or more of hydrochloric acid, nitric acid, sulfuric acid, hydrobromic acid, hydroiodic acid, and hydrofluoric acid; and / or The iron source includes one or more of ferric nitrate, ferric nitrate hydrate, ferric chloride, ferric chloride hydrate, ferric acetate, ferric acetate hydrate, ferric carbonate, ferric carbonate hydrate, ferrous chloride, ferrous chloride hydrate, ferrous acetate, ferrous acetate hydrate, ferrous carbonate, and ferrous carbonate hydrate.
4. The preparation method according to claim 3, characterized in that: The nickel alloy contains nickel element, and the mass fraction of nickel is 60% to 95%; and / or The nickel alloy contains iron element, and the mass fraction of the iron is 0-40%.
5. The preparation method according to claim 2, characterized in that: The concentration of the acidic solution is 0.1 to 5 mol / L; and / or The mass ratio of the nickel material to the acidic solution is 1:(5-100); and / or The nickel material is immersed in the acidic solution for 0.5 to 3 hours; and / or The mass ratio of the first intermediate to the pure water is 1:(10-100); and / or The first intermediate is immersed in pure water for 5 to 48 hours; and / or The molar concentration of the iron source is 0.1 to 1 mol / L; and / or The mass ratio of the second intermediate to the iron source solution is 1:(5-100); and / or The second intermediate is immersed in the iron source solution for 0.5 to 5 hours.
6. The preparation method according to claim 1, characterized in that: The vacuum flow rate is 30 to 50 mL / min; and / or After the vacuuming, the gas pressure in the reaction container is less than 0.05 MPa.
7. The preparation method according to claim 1, characterized in that: The flow rate of the phosphine gas is 10-60 mL / min; and / or In the phosphine gas, the partial pressure of phosphine molecules accounts for 20% to 95%; and / or The temperature of the phosphine gas is 10°C to 80°C.
8. The preparation method according to claim 1, characterized in that: The preset pressure is 0.05-0.2 MPa; and / or The heating rate is 0.5-10°C / min; and / or The temperature T is 300-500° C.; and / or The insulation time t is 0.5h to 5h; and / or During the heating and the heat preservation process, the phosphine gas is continuously introduced.
9. The preparation method according to claim 1, characterized in that: After the heat preservation for a period of time t, the temperature is also lowered.
10. The preparation method according to claim 9, characterized in that: The cooling rate is 0.5-10°C / min.
11. A nickel-iron phosphide material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 10.
12. An electrode, characterized in that: The invention comprises the nickel-iron phosphide material prepared by the preparation method according to any one of claims 1 to 10, or comprises the nickel-iron phosphide material according to claim 11.
13. A water electrolysis device, characterized in that: Comprising the electrode as claimed in claim 12.
Citation Information
Patent Citations
Ferro-nickel phosphate / carbon nanotube composite material and preparation method and application thereof
CN109433234A
Preparation method and application of nickel phosphide-iron phosphide-ruthenium phosphide / foamed nickel three-dimensional self-supporting electrode material
CN113201764A
Method for producing hydrogen by coupling dicarboxylic acid prepared by electrocatalytic oxidation of cyclic alcohol / cyclic ketone
CN113832485A
Cobalt-doped nano Ni2P / foamed nickel electrode material and preparation method thereof
CN115595633A
Cited By
Sodium-ion battery negative electrode material, preparation method thereof and sodium-ion battery
CN120136085A