Preparation method of surface-coated ultrahigh-nickel quaternary lithium nickel cobalt manganese aluminate material
Through high-speed mixing and high-temperature sintering, a lithium-rich material coating layer is formed, combined with oxide and non-oxide coatings, to solve the surface residual alkali and cycle stability problems of ultra-high nickel quaternary cathode materials, significantly improving the rate and The cycle performance meets the needs of the high-power discharge field.
Patent Information
- Application Number
- CN202411180629.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing ultra-high nickel quaternary cathode materials have problems such as high residual alkali on the surface, poor cycle stability and many electrolyte side reactions, which affect their energy density and rate performance.
A high-speed mixer is used to mix the quaternary cathode material precursor, lithium source micropowder and doping elements. After high-temperature sintering, sand grinding and spray drying are used to pelletize to form a coating layer with a lithium-rich material structure, combining oxides and non-oxides. Coating to form a fast ion conductor layer to improve the rate and cycle performance of the material.
It significantly improves the cycle performance and rate performance of the material, extends the service life of the material, enhances the lattice stability, and meets the performance requirements in the field of high-power discharge.
Smart Images

Figure CN118724084A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium ion battery positive electrode materials, and in particular to a method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material. Background Art
[0002] With the rapid development of the new energy industry, lithium-ion batteries have become the most widely used electrochemical power source. Chemical energy is converted into electrical energy by the deintercalation of lithium ions in positive and negative electrode materials. Nowadays, the negative electrode materials of lithium-ion batteries are mainly natural graphite, artificial graphite or silicon-based materials. The current theoretical capacity of negative electrode materials is around 350-2000mAh / g, which is much larger than the capacity of the current positive electrode material system (200mAh / g). Therefore, it is particularly urgent to increase the theoretical capacity of positive electrode materials and improve the energy density of lithium batteries. At present, the positive electrode material system mainly includes spinel lithium manganese oxide, layered lithium cobalt oxide, layered nickel cobalt manganese oxide, nickel cobalt aluminum oxide, and olivine lithium iron phosphate. Among them, layered nickel cobalt manganese oxide and nickel cobalt aluminum oxide are widely used in electric vehicles, power tools, consumer electronics, two-wheeled vehicles and other fields due to their high energy density, good cycle performance, excellent rate performance and simple synthesis process. In these two materials, the Co element is +3 and does not participate in the electrochemical reaction in the low voltage range (≤4.25V). In the high voltage field, it is oxidized from +3 to +4 to participate in the electrochemical reaction. The Mn element is +4 and plays a role in supporting the layered structure and does not participate in the electrochemical reaction. The Ni element +2 and +3 valences exist at the same time. In the low voltage range, it is mainly composed of Ni 2+ Converted to Ni 3+ , in the high voltage range mainly composed of Ni 3+ To Ni, which is more oxidizing 4+ , participate in electrochemical reactions, continuously release electrons, and release energy. Therefore, increasing the nickel content in the material can increase the amount of substances participating in the electrochemical reaction in the material, which can significantly increase the capacity of the material and the energy density of the lithium battery. With people's extreme requirements for energy density, materials with Nimol% ≥ 90% (ultra-high nickel) have been developed and used one after another. However, as the nickel content increases, the Ni generated in the electrochemical reaction 4+ The content of Ni 4+It has strong oxidizing properties and will oxidize oxygen atoms in the lattice into oxygen, causing the structure of the layered positive electrode material to collapse and release a large amount of heat. The generated oxygen gathers in the battery and further promotes the occurrence of thermal failure reactions, which is specifically manifested in the poor safety performance, poor thermal stability, and poor cycle performance of high-nickel NCM positive electrode materials; severe safety accidents can occur, endangering personal life. In recent years, researchers have found that with the addition of Al elements, Al-O bonds with stronger bond energy are generated inside the layered structure of layered nickel cobalt manganese oxide, which significantly enhances the thermal stability and cycle performance of high-nickel NCM positive electrode materials. Therefore, in the development process of ultra-high nickel materials, Al ions are introduced on the basis of conventional nickel cobalt manganese oxide to become nickel cobalt manganese aluminum oxide lithium quaternary materials, which significantly improves the thermal stability and cycle performance of ultra-high nickel materials.
[0003] Although the ultra-high nickel quaternary material has improved the thermal stability of the material by introducing Al ions and provided considerable discharge capacity, its ultra-high nickel still has relatively serious problems, such as high residual alkali on the surface of the ultra-high nickel quaternary material, poor cycle stability and more side reactions in the electrolyte. With my country's continued attention and investment in the field of "low-altitude economy", higher requirements are placed on the energy density and rate performance of lithium batteries. Therefore, it is particularly important to develop an ultra-high nickel quaternary nickel cobalt manganese aluminum oxide material with high capacity, easy preparation, excellent rate performance and long cycle performance.
[0004] The Chinese invention patent with publication number CN112670506B discloses a fast ion conductor coated nickel-cobalt-manganese-tantalum composite quaternary positive electrode material and its preparation method, which comprises the following steps: tantalum salt and lithium salt are mixed and powdered, and then mixed with a ternary nickel-cobalt-manganese precursor, and then calcined at a temperature of 680-780°C after the mixing is completed. After the calcination is completed, the furnace is cooled, and the tantalum element is used to obtain a quaternary positive electrode material with bulk phase doping and surface coating. The tantalum salt reacts with the residual alkali on the surface to generate a tantalum element with a certain thickness. The LiTaO3 fast ion coating layer has a high degree of Li-ion conductivity. This fast ion conductor layer can increase the speed of lithium ion insertion and extraction, improve the rate performance of the material during the charge and discharge process, and maintain structural stability, so that the high-nickel material exhibits good cycle stability performance. However, during the high-temperature sintering process, the lithium source will become a molten state, which will cause the tantalum element coated on the surface to be unevenly distributed. After the battery is made, the surface is directly in contact with the electrolyte, resulting in a large number of side reactions, causing the electrochemically inactive salt rock phase to accumulate on the surface, causing the material's cyclability and rate performance to drop sharply.
[0005] The Chinese invention patent with publication number CN114551835B discloses an ultra-high nickel quaternary positive electrode material and its preparation method, wherein the NCMA (Ni, Co, Mn, Al) precursor obtained by the co-precipitation process is mixed and sintered with a lithium source to obtain a sintered product, which is then crushed and then co-coated with phosphoric acid and calcium nitrate by a dry process. The sum of the peak intensities of the characteristic diffraction splitting peaks (006) + (012) of the finished product and the peak intensity ratio of the characteristic diffraction peak (110) are selected from the XRD test results to be 0.430~0.450; the ratio of the lithium-nickel mixed arrangement to the 100% The ratio is ≤1.05%; the grain size of the characteristic diffraction peak (003) is between 49.0 and 54.5 nm to obtain an ultra-high nickel polycrystalline positive electrode material with high discharge specific capacity and high energy density; the method adopts a dry process for coating, and phosphoric acid is directly in contact with the surface of the positive electrode material, which not only damages the surface of the material, but also fails to effectively remove the residual alkali in the ultra-high nickel lattice gap, and the coating method does not take into account that the ultra-high nickel surface will form a NiO salt rock phase after deintercalation of Li+, resulting in the formation of lithium ion inactive areas on the surface, resulting in a cycle dive during the material cycle and a rapid cycle attenuation.
[0006] A Chinese invention patent with publication number CN112952074B discloses a boron oxide-coated quaternary positive electrode material and a preparation method thereof, wherein a NCMA (Ni, Co, Mn, Al) precursor obtained by a coprecipitation process is mixed with a lithium source and sintered to obtain a sintered product, the sintered product is crushed, washed with water, and dried, and then the material is mixed with a certain amount of metaboric acid or pyroboric acid and then sintered at a low temperature to finally obtain a quaternary positive electrode material uniformly coated with boron oxide. This method can effectively remove residual alkali on the surface of the material. The uniformity of the distribution of the B element on the surface is difficult to ensure using a dry mixing process, which may cause a large side reaction between the positive electrode material and the electrolyte locally, resulting in the formation of a rock salt phase on the surface.
[0007] Therefore, how to obtain ultra-high nickel quaternary positive electrode materials with good electrochemical performance is a technical problem that needs to be solved urgently. Summary of the invention
[0008] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and provide a method for preparing a surface-coated ultra-high nickel quaternary nickel cobalt manganese aluminum lithium oxide material.
[0009] To achieve the above object, the present invention adopts the following technical solutions: The present invention provides a method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material, comprising the following steps: S1, the quaternary cathode material precursor Ni x Co y Mn z Al 1-x-y-z(OH)2 is mixed with lithium source powder and doping element K, and mixed at high speed using a high-speed mixer, wherein the speed is 250r / min≤≤500r / min, and the mixing time is 12min≤≤20min; After the mixing is completed, the material A to be sintered is obtained, and the material A to be sintered is placed in a sagger, and the material in the sagger is marked in a tic-tac-toe pattern with a 3-5 mm wide iron sheet to facilitate full contact between the material and oxygen; In terms of molar ratio, in the quaternary cathode material precursor, 0.90≤x≤0.98, 0.01≤y≤0.06, and D50≤4 μm; The element valence state of the doping element K is ≥4+; The doping element K is one or more of Zr, Nb, Ti, W, and Ta; In terms of weight percentage, the total content k of the doping element K is: 2000ppm≤k≤4000ppm; S2, placing the material A to be sintered into a box furnace for high-temperature sintering, and maintaining the oxygen concentration in the furnace ≥ 96% throughout the process, the temperature is raised from 25°C at 3°C / min, raised to 500°C and kept for 4 hours, after the insulation is completed, the temperature is raised to 700-850°C at 3°C / min for constant temperature sintering for 12 hours, then cooled to 300°C at 5°C / min, the power is turned off, and the material temperature is taken out after it drops to room temperature to obtain material B; S3, the binary precursor Ni a Mn 1-a (OH)2 is added to a sand mill. The grinding balls used for sand milling are zirconium balls with a diameter of 0.8 mm. The sand milling medium is deionized water. The dispersant is polyacrylate. The sand milling time is ≥8 h. The particle size of the precursor after sand milling is controlled to be 100-1000 nm. The sand milled slurry is mixed with the material B to obtain material C. The material C is rotated at high speed with a stirring paddle. The stirring paddle speed is ≥350 rpm. The high-speed mixing time is 15 M C / 2.5min to obtain material D, where M C is the weight of material C in kg; material D is spray dried to form balls, the inlet temperature of the spray drying chamber is 350°C, the outlet temperature is 100°C, the solid content of the material is ≥60% by mass, the spray disk speed is 30,000 rpm, and the ultra-high nickel quaternary material E uniformly coated with the binary precursor is obtained after spray drying process.
[0010] Furthermore, it also includes: S4. Place ultra-high nickel quaternary material E into the box body, and use 3~5mm wide iron sheets to mark the material in the box in a tic-tac-toe pattern to facilitate full contact between the material and oxygen. The oxygen concentration is ≥96%. The temperature is raised from 25℃ at 33℃ / min to 500℃ and kept for 4h. After the insulation, the temperature is raised to 550-700℃ at 3℃ / min for constant temperature sintering for 10h, then cooled to 300℃ at 5℃ / min. Turn off the power, and take out the material after the temperature drops to room temperature to obtain material F, and mix material F with additive W.
[0011] Furthermore, it also includes: S5. Then put the mixed materials into a sagger, and use a 3-5 mm wide iron sheet to mark the materials in the sagger in a tic-tac-toe pattern to facilitate full contact between the materials and oxygen. The oxygen concentration is ≥96%. The temperature is raised from 25°C at 3°C / min to 300-400°C for 8h, and then lowered to 300°C at 5°C / min. Turn off the power, and take out the finished material G after the material temperature drops to room temperature; wherein the finished material G is an ultra-high nickel quaternary material doped with high-valent ions; S6. Make material G into a soft-pack battery for electrical performance evaluation.
[0012] Furthermore, the lithium source powder is battery-grade lithium hydroxide, lithium carbonate or a mixture of the two in different proportions.
[0013] Furthermore, the binary precursor Ni a Mn 1-a In (OH)2, a≤40mol%.
[0014] Furthermore, the binary precursor Ni a Mn 1-a In (OH)2, the particle size D50 of the binary precursor is 2~10μm, and the solid content of the slurry is ≥50% by mass.
[0015] Furthermore, the additive W is one or two of TiO2, Al2O3, BO3, LaO2, WO3, Co(OH), AlPO4, and NH4PO3.
[0016] Furthermore, in terms of mass percentage, the total amount of the additive W is controlled to be ≤4000 ppm.
[0017] Among them, the additive W plays a coating role.
[0018] The beneficial effects of the present invention are as follows: high-valent cations are used for doping, because the average valence of M in LiMO2 is +3, Co and Mn are constant-valence elements, and more high-valent oxygen ions will promote Ni 2+The generation of Ni can promote the generation of more Ni in the ultra-high nickel positive electrode material. 2+ , in the electrochemical reaction Ni 2+ First it is converted into 3+, and then into 4+ nickel ions with high oxidation properties. More electrons are released, which increases the capacity of the material. The Ni / Mn precursor is sand-milled by a sand mill to make the precursor D50 about 300-1000nm, and then the positive electrode material is calcined and crushed and the sand-milled material is added with a spray coating agent, and after spray treatment, it is placed in a box furnace for high-temperature sintering to form a coating layer of a lithium-rich manganese-based material structure on the surface of the material, and then oxides and non-oxides are coated on the surface of the material and placed in a box furnace for low-temperature sintering to form a fast ion conductor layer on the surface, which can protect the lithium-rich layer generated on the surface of the material on the basis of improving the material rate and cycle performance; There is a large amount of Li2MnO3 in the lithium-rich layer. After the battery is made, SEI film and CEI film will be formed at the positive and negative electrodes during the early cycle. In this process, some lithium ions will be consumed. These lithium ions will be replenished from the lithium-rich layer in the later cycle, which will increase the capacity of the lithium-ion battery and the capacity retention rate. In addition, in the later stage of the cycle, lithium ions are continuously consumed. The cut-off voltage can be increased to about 4.45V by using a small rate, and then the lithium ions in the lithium-rich layer are continuously replenished to restore the battery's capacity retention rate. During the cycle, the capacity retention will first decrease and then increase, and then the capacity retention rate will gradually decrease as the cycle progresses, and the cycle performance is good; During the charging process of lithium batteries, as the voltage increases, lithium ions continue to be deintercalated from the positive electrode layered structure to the negative electrode. As lithium ions in the positive electrode material continue to be removed, the structure of the positive electrode material undergoes a structural phase change from H1 (hexagonal phase) - M1 (monoclinic phase) - H2 (hexagonal) - H3 (hexagonal). The H2-H3 structural phase change is easy to occur when the voltage is ≥ 4.2V, and the process is prone to produce irreversible phase change, resulting in the collapse of the material structure and poor cycle performance. The surface lithium-rich layer is easy to release lithium ions under high voltage, which slows down the deintercalation rate and amount of lithium ions in the positive electrode material, and can effectively protect the layered structure of the ternary positive electrode, reduce the irreversible phase change of the material, improve the stability of the lattice, and improve the cycle performance of the material. By using small particle precursors with Nimol% ≥ 90 and D50 of about 3 microns, the lithium ion diffusion path becomes shorter, the specific surface area increases, and the lithium-rich layer content is higher, which greatly improves the rate performance of the material and can meet the performance requirements in the field of high-power discharge. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a process flow chart of a method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material; Figure 2It is the diagram of the capacity of the deduction; Figure 3 It is the power-off curve diagram; Figure 4 This is the full electric cycle curve. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0021] A method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material comprises the following steps: S1, the quaternary cathode material precursor Ni x Co y Mn z Al 1-x-y-z (OH)2 is mixed with lithium source powder and doping element K, and mixed at high speed using a high-speed mixer, wherein the speed is 250r / min≤≤500r / min, and the mixing time is 12min≤≤20min; After the mixing is completed, the material A to be sintered is obtained, and the material A to be sintered is placed in a sagger, and the material in the sagger is marked in a tic-tac-toe pattern with a 3-5 mm wide iron sheet to facilitate full contact between the material and oxygen; In terms of molar ratio, in the quaternary cathode material precursor, 0.90≤x≤0.98, 0.01≤y≤0.06, and D50≤4 μm; In a specific embodiment, in the quaternary positive electrode material precursor, D50≤4μm, that is, the particles are small and have better rate performance, which is suitable for the needs of unmanned aerial vehicles in the current low-altitude economic field.
[0022] The element valence state of the doping element K is ≥4+; The doping element K is one or more of Zr, Nb, Ti, W, and Ta; In terms of weight percentage, the total content k of the doping element K is: 2000ppm≤k≤4000ppm; In a specific embodiment, the doping elements generally diffuse from the surface of the material to the interior of the material lattice through high temperature, causing a small part of the lattice distortion inside the lattice, making the lattice stronger and increasing the strength of the material. In addition, they form bonds with oxygen atoms to increase the lattice strength of the material. However, if the amount of doping elements is too much, they will occupy the transition metal sites or lithium sites in the ternary positive electrode material, increase the structural distortion of the lattice, and affect the performance of the material.
[0023] S2. Put the material A to be sintered into a box furnace for high-temperature sintering, and keep the oxygen concentration in the furnace ≥96% throughout the process. The temperature is raised from 25°C at 3°C / min to 500°C and kept for 4 hours. After the insulation is completed, the temperature is raised to 700-850°C at 3°C / min for constant temperature sintering for 12 hours, and then cooled to 300°C at 5°C / min. Turn off the power, and take out the material after the temperature drops to room temperature to obtain material B; keep the oxygen concentration level in the furnace consistent throughout the process.
[0024] In a specific embodiment, the higher the oxygen concentration of material A in the box furnace, the easier it is to separate Ni 2+ Oxidation to Ni 3+ , thereby reducing the Li / Ni mixing of ternary cathode materials; S3, the binary precursor Ni a Mn 1-a (OH)2 is added to a sand mill. The grinding balls used for sand milling are zirconium balls with a diameter of 0.8 mm. The sand milling medium is deionized water. The dispersant is polyacrylate. The sand milling time is ≥8 h. The particle size of the precursor after sand milling is controlled to be 100-1000 nm. The sand milled slurry is mixed with the material B to obtain material C. The material C is rotated at high speed with a stirring paddle. The stirring paddle speed is ≥350 rpm. The high-speed mixing time is 15 M C / 2.5min to obtain material D, where M C is the weight of material C in kg; material D is spray dried to form balls, the inlet temperature of the spray drying chamber is 350°C, the outlet temperature is 100°C, the solid content of the material is ≥60% by mass, the spray disk speed is 30,000 rpm, and the ultra-high nickel quaternary material E uniformly coated with the binary precursor is obtained after spray drying process.
[0025] Also includes: S4. Place ultra-high nickel quaternary material E into the box body, and use 3~5mm wide iron sheets to mark the material in the box in a tic-tac-toe pattern to facilitate full contact between the material and oxygen. The oxygen concentration is ≥96%. The temperature is raised from 25℃ at 33℃ / min to 500℃ and kept for 4h. After the insulation, the temperature is raised to 550-700℃ at 3℃ / min for constant temperature sintering for 10h, then cooled to 300℃ at 5℃ / min. Turn off the power, and take out the material after the temperature drops to room temperature to obtain material F, and mix material F with additive W.
[0026] Also includes: S5. Then put the mixed materials into a sagger, and use a 3-5 mm wide iron sheet to mark the materials in the sagger in a tic-tac-toe pattern to facilitate full contact between the materials and oxygen. The oxygen concentration is ≥96%. The temperature is raised from 25°C at 3°C / min to 300-400°C for 8h, and then lowered to 300°C at 5°C / min. Turn off the power, and take out the finished material G after the material temperature drops to room temperature; wherein the finished material G is an ultra-high nickel quaternary material doped with high-valent ions; S6. Make material G into a soft-pack battery for electrical performance evaluation.
[0027] The lithium source powder is battery-grade lithium hydroxide, lithium carbonate or a mixture of the two in different proportions.
[0028] The binary precursor Ni a Mn 1-a In (OH)2, a≤40mol%.
[0029] In a specific embodiment, a is the molar amount of Ni element, the nickel element will react with manganese element to form NiMn binary oxide, and the remaining Mn element will form Li2MnO3, which is lithium-rich. The less nickel, the more lithium-rich phase, but the corresponding crystal structure is more difficult to synthesize.
[0030] The binary precursor Ni a Mn 1-a In (OH)2, the particle size D50 of the binary precursor is 2~10μm, and the solid content of the slurry is ≥50% by mass.
[0031] The additive W is one or two of TiO2, Al2O3, BO3, LaO2, WO3, Co(OH), AlPO4, and NH4PO3.
[0032] In terms of mass percentage, the total amount of the additive W is controlled to be ≤4000ppm.
[0033] Embodiment 1
[0034] 10kg of quaternary cathode material precursor Ni 0.92 Co 0.04 Mn 0.03 Al 0.01(OH)2, D50 is 3.5μm, and lithium hydroxide is mixed according to Li / M (lithium ratio) of 1.045. The additive ZrO is added to the mixture at 2000ppm. A high-speed mixer is used for high-speed mixing at a speed of 500r / min. The high-speed mixing is stopped for 12min. The mixed materials are placed in a sagger with a size of 330x330x110nm, and the materials in the sagger are marked in a tic-tac-toe pattern with an iron sheet of 3~5nm width to facilitate full contact between the materials and oxygen. The oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is carried out according to the sintering temperature system, that is, the heating rate is 33℃ / min, and the temperature is increased from room temperature to 500℃ and kept for 4h. After the insulation, the temperature is increased to 750℃, and constant temperature sintering is carried out for 12h, and then the temperature is reduced at a cooling rate of 5℃ / min. When the temperature is reduced to 300℃, the box furnace power is turned off, and the furnace is taken out after cooling to room temperature.
[0035] The binary precursor Ni 0.35 Mn 0.65 (OH)2 is added to the sand mill, the precursor D50 is 4μm, the solid content of the slurry is controlled at 60%, the diameter of the grinding ball used for sand milling is 0.8m zirconium ball, the sand milling medium is deionized water, the dispersant is sodium polyacrylate, the sand milling time is ≥8h, the particle size of the binary precursor after sand milling is 300nm, 5kg of quaternary calcined crushed material is added to the sand milling slurry, deionized water is added to control the solid content of the slurry at 60%, the binary precursor accounts for 10000ppm, and the stirring is carried out at a high speed with a stirring paddle, the speed is 500r / min, the stirring time is 5x15 / 2.5=30min, and after stirring, the mixed slurry is spray dried to form balls. The inlet temperature of the spray drying chamber is 350℃, the outlet temperature is 100℃, the solid content of the material is 60%, and the spray disk speed is 30000 rpm. After the spray drying process, an ultra-high nickel quaternary positive electrode material uniformly coated with the binary precursor is obtained.
[0036] The ultra-high nickel quaternary positive electrode material uniformly coated with the binary precursor is placed in the sagger, and the material in the sagger is marked in a tic-tac-toe pattern with an iron sheet 3 to 5 nm wide to facilitate full contact between the material and oxygen. The oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is carried out according to the sintering temperature system, and the heating rate is 3℃ / min, from room temperature to 500℃ and kept for 4h. After the insulation, the temperature is raised to 680℃ and constant temperature sintering is carried out for 8h, and then the temperature is cooled at a cooling rate of 5℃ / min. When the temperature drops to 300℃, the box furnace power is turned off, and the material is taken out after the furnace cools down to room temperature.
[0037] 5 kg of secondary sintered material, nano-alumina and nano-titanium oxide were added to a high-speed mixer for high-speed mixing at a speed of 500 r / min. The high-speed mixing was stopped after 12 minutes. The mixed material was put into a sagger, and the material in the sagger was marked with a 3-5 mm wide iron sheet in a well shape to facilitate full contact between the material and oxygen. The oxygen atmosphere in the box furnace was controlled at 99%, and then constant temperature sintering was carried out according to the sintering temperature system (heating rate 3°C / min, heating from room temperature to 400°C and keeping warm for 8 hours, and then cooling at a cooling rate of 5°C / min after the insulation was completed. The box furnace power was turned off when the temperature was cooled to 200°C, and the material was taken out after cooling to room temperature with the furnace) to obtain a finished product of ultra-high nickel quaternary material with 92% mol of Ni element as sample 1; Among them, nano-alumina is 1000ppm and nano-titanium oxide is 1500ppm.
[0038] Embodiment 2
[0039] 10kg of quaternary cathode material precursor Ni 0.92 Co 0.04 Mn 0.03 Al 0.01 (OH)2, D50 is 3.5μm, mixed with lithium hydroxide according to Li / M (lithium ratio) of 1.045, the additive ZrO is added to the mixture at 2000ppm, and a high-speed mixer is used for high-speed mixing at a speed of 500r / min. The high-speed mixing is stopped after 12min, and the mixed materials are placed in the box body, and the materials in the box body are marked with a 3-5mm wide iron sheet in a well shape to facilitate full contact between the materials and oxygen, and the oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is carried out according to the sintering temperature system (heating rate 3℃ / min, heating from room temperature to 500℃ and keeping for 4h, heating to 750℃ after the end of the insulation, and constant temperature sintering for 12h, and then cooling at a cooling rate of 5℃ / min, cooling to 300℃, turning off the box furnace power, and taking it out after cooling to room temperature with the furnace); The binary precursor Ni 0.25 Mn 0.75(OH)2 is added to the sand mill, the precursor particle size D50 is 3μm, the solid content of the slurry is controlled at 60%, the diameter of the grinding ball used for sand milling is 0.8m zirconium ball, the sand milling medium is deionized water, the dispersant is sodium polyacrylate, the sand milling time is ≥8h, and the particle size of the binary precursor after sand milling is 300nm. 5kg of quaternary calcined crushed material is added to the ball mill slurry, and deionized water is added to control the solid content of the slurry to about 60%. The proportion of binary precursor is 10000ppm, and the stirring is carried out at a high speed with a stirring paddle, the speed is 500r / min, and the stirring time is 5x15 / 2.5=30min. After stirring, the mixed slurry is spray dried to form balls. The inlet temperature of the spray drying chamber is 350℃, the outlet temperature is 100℃, the solid content of the material is 60%, and the spray disk speed is 30,000 rpm. After the spray drying process, an ultra-high nickel quaternary positive electrode material uniformly coated with the binary precursor is obtained.
[0040] The ultra-high nickel quaternary positive electrode material uniformly coated with the binary precursor is placed in the sagger, and the material in the sagger is crossed in a tic-tac-toe pattern with a 3-5 nm wide iron sheet to facilitate full contact between the material and oxygen, and the oxygen atmosphere in the box-type furnace is controlled at 99%, and then constant temperature sintering is performed according to the sintering temperature system (heating rate 3℃ / min, heating from room temperature to 500℃ and keeping for 3h, heating to 650℃ after the end of the insulation, and constant temperature sintering for 8h, and then cooling at a cooling rate of 5℃ / min, cooling to 300℃, turning off the box-type furnace power, and taking it out after cooling to room temperature with the furnace); 5 kg of the secondary sintered material, nano-alumina and nano-titanium oxide were added to a high-speed mixer for high-speed mixing at a speed of 500 rpm. The high-speed mixing was stopped after 12 minutes. The mixed material was put into a sagger, and the material in the sagger was marked with a 3-5 mm wide iron sheet in a tic-tac-toe pattern to facilitate full contact between the material and oxygen. The oxygen atmosphere in the box furnace was controlled at 99%, and then constant-temperature sintering was performed according to the sintering temperature system (heating rate 3°C / min, heating from room temperature to 400°C and keeping warm for 8 hours, and then cooling at a cooling rate of 5°C / min after the insulation was completed. The box furnace power was turned off when the temperature was cooled to 200°C, and the material was taken out after cooling to room temperature with the furnace) to obtain a finished product of ultra-high nickel quaternary material with 92% mol of Ni element as sample 2; Among them, nano-alumina is 1000ppm and nano-titanium oxide is 1500ppm.
[0041] Embodiment 3
[0042] 10kg of quaternary material precursor Ni 0.95 Co 0.03 Mn 0.015 Al 0.005(OH)2, D50 is 3.5μm, mixed with lithium hydroxide according to Li / M (lithium ratio) of 1.045, the additive ZrO is added to the mixture at 2000ppm, and a high-speed mixer is used for high-speed mixing at a speed of 500r / min. The high-speed mixing is stopped after 12min, and the mixed materials are placed in a sagger, and the materials in the sagger are marked in a well-shaped pattern with a 3-5nm wide iron sheet to facilitate full contact between the materials and oxygen, and the oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is carried out according to the sintering temperature system (heating rate 3℃ / min, heating from room temperature to 500℃ and holding for 4h, heating to 730℃ after the end of the holding, and constant temperature sintering for 12h, and then cooling at a cooling rate of 5℃ / min, cooling to 300℃, turning off the box furnace power, and taking out after cooling to room temperature with the furnace); The binary precursor Ni 0.35 Mn 0.65 (OH)2 is added to the sand mill, the precursor D50 is 4μm, the solid content of the slurry is controlled at 60%, the diameter of the grinding ball used for sand milling is 0.8m zirconium ball, the sand milling medium is deionized water, the dispersant is sodium polyacrylate, the sand milling time is ≥8h, the particle size of the binary precursor after sand milling is 300nm, 5kg of quaternary calcined crushed material is added to the sand milling slurry, deionized water is added to control the solid content of the slurry at 60%, the binary precursor accounts for 10000ppm, and the stirring is carried out at a high speed with a stirring paddle, the speed is 500r / min, the stirring time is 5x15 / 2.5=30min, and after stirring, the mixed slurry is spray dried to form balls. The inlet temperature of the spray drying chamber is 350℃, the outlet temperature is 100℃, the solid content of the material is 60%, and the spray disk speed is 30,000 rpm. After the spray drying process, an ultra-high nickel quaternary positive electrode material uniformly coated with the binary precursor is obtained.
[0043] The ultra-high nickel quaternary positive electrode material uniformly coated with the binary precursor is placed in the box body, and the material in the box body is marked with a 3-5nm wide iron sheet in a tic-tac-toe pattern to facilitate full contact between the material and oxygen, and the oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is performed according to the sintering temperature system (heating rate 3℃ / min, heating from room temperature to 500℃ and keeping for 4h, heating to 680℃ after the end of the insulation, and constant temperature sintering for 8h, and then cooling at a cooling rate of 5℃ / min, cooling to 300℃, turning off the box furnace power, and taking it out after cooling to room temperature with the furnace); 5 kg of secondary sintered material, nano-alumina and nano-titania were added to a high-speed mixer for high-speed mixing at a speed of 500 r / min. The high-speed mixing was stopped after 12 minutes. The mixed material was placed in a box body, and the material in the box body was marked in a tic-tac-toe pattern with an iron sheet with a width of 3-5 nm to facilitate full contact between the material and oxygen. The oxygen atmosphere in the box furnace was controlled at 99%, and then constant-temperature sintering was carried out according to the sintering temperature system (heating rate of 3°C / min, heating from room temperature to 400°C and keeping warm for 8 hours, and then cooling at a cooling rate of 5°C / min after the insulation was completed. The box furnace was turned off when the temperature dropped to 200°C, and the material was taken out after the furnace cooled to room temperature) to obtain the ultra-high nickel quaternary material with 95% mol of Ni element, which was sample 3.
[0044] Comparative Example 1 10kg of quaternary material precursor Ni 0.92 Co 0.04 Mn 0.03 Al 0.01 (OH)2, D50 is 3.5μm, mixed with lithium hydroxide according to Li / M (lithium ratio) of 1.045, the additive ZrO is added to the mixture according to 2000ppm, and a high-speed mixer is used for high-speed mixing at a speed of 500r / min. The high-speed mixing is stopped for 12min, and the mixed materials are placed in a sagger, the sagger is 330x330x110nm, and the materials in the sagger are marked in a well-shaped pattern with a 3~5nm wide iron sheet to facilitate full contact between the materials and oxygen. The oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is carried out according to the sintering temperature system (heating rate 3℃ / min, heating from room temperature to 500℃ and keeping for 4h, heating to 750℃ after the end of the insulation, and constant temperature sintering for 12h, and then cooling at a cooling rate of 5℃ / min, cooling to 300℃, turning off the box furnace power, and taking out after cooling to room temperature with the furnace; 5 kg of the primary sintered material was washed with deionized water, and the speed of the stirring paddle was controlled at 400 r / min. After washing for 15 minutes, the material was dehydrated and dried, and the dried material was placed in a drying box for drying. After drying, the material was placed in a high-speed mixer, and nano-alumina and nano-titanium oxide were added to the high-speed mixer for high-speed mixing at a speed of 500 r / min. The high-speed mixing was stopped for 12 minutes, and the mixed material was placed in a box body, and the material in the box body was marked in a well shape with a 3-5 nm wide iron sheet to facilitate full contact between the material and oxygen. The oxygen atmosphere in the box furnace was controlled at 99%, and then constant temperature sintering was carried out according to the sintering temperature system (heating rate of 3°C / min, heating from room temperature to 400°C and keeping for 8 hours, and then cooling at a cooling rate of 5°C / min after the insulation was completed, and the box furnace power was turned off when the temperature was cooled to 200°C, and the box furnace was taken out after cooling to room temperature with the furnace), and the finished product of ultra-high nickel quaternary material with 92% mol of Ni element was obtained as comparison sample 1.
[0045] Among them, nano-alumina is 1000ppm and nano-titanium oxide is 1500ppm.
[0046] Comparative Example 2 10kg of quaternary material precursor Ni 0.95 Co 0.03 Mn 0.015 Al 0.005 (OH)2, D50 is 3.5μm, mixed with lithium hydroxide according to Li / M (lithium ratio) of 1.045, the additive ZrO is added to the mixture according to 2000ppm, and a high-speed mixer is used for high-speed mixing at a speed of 500r / min. The high-speed mixing is stopped after 12min, and the mixed materials are put into a sagger, and the materials in the sagger are marked in a well-shaped pattern with a 3-5nm wide iron sheet to facilitate full contact between the materials and oxygen. The oxygen atmosphere in the box furnace is controlled at 99%, and then constant temperature sintering is carried out according to the sintering temperature system (heating rate 3℃ / min, heating from room temperature to 500℃ and holding for 4h, heating to 750℃ after the end of the holding, and constant temperature sintering for 12h, and then cooling at a cooling rate of 5℃ / min, cooling to 300℃, turning off the box furnace power, and taking out after cooling to room temperature with the furnace); 5 kg of the primary sintered material was washed in deionized water, and the speed of the stirring paddle was controlled at 400 r / min. After washing for 15 minutes, the material was dehydrated and dried, and the dried material was placed in a drying box for drying. After drying, the material was placed in a high-speed mixer, and nano-alumina and nano-titanium oxide were added to the high-speed mixer for high-speed mixing at a speed of 500 r / min. The high-speed mixing was stopped for 12 minutes, and the mixed material was placed in a box body, and the material in the box body was marked in a well shape with a 3-5 mm wide iron sheet to facilitate full contact between the material and oxygen. The oxygen atmosphere in the box furnace was controlled at 99%, and then constant temperature sintering was performed according to the sintering temperature system (heating rate 3°C / min, heating from room temperature to 400°C and keeping for 8 hours, and then cooling at a cooling rate of 5°C / min after the insulation was completed, and the box furnace power was turned off when the temperature was cooled to 200°C, and the box furnace was cooled to room temperature and then taken out) to obtain a 95% mol ultra-high nickel quaternary material of Ni element as comparison sample 2; Among them, nano-alumina is 1000ppm and nano-titanium oxide is 1500ppm.
[0047] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention should be based on the attached claims.
Claims
1. A method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material, It is characterized in that The following steps are involved: S1, the quaternary cathode material precursor Ni x Co y Mn z Al 1-x-y-z (OH) 2 Mix with lithium source powder and doping element K, and use a high-speed mixer for high-speed mixing, wherein the speed is 250r / min≤≤500r / min, and the mixing time is 12min≤≤20min; After the mixing is completed, the material A to be sintered is obtained, and the material A to be sintered is placed in a sagger, and the material in the sagger is marked in a tic-tac-toe pattern with a 3-5 mm wide iron sheet to facilitate full contact between the material and oxygen; In terms of molar ratio, in the quaternary cathode material precursor, 0.90≤x≤0.98, 0.01≤y≤0.06, and D50≤4 μm; The element valence state of the doping element K is ≥4+; The doping element K is one or more of Zr, Nb, Ti, W, and Ta; In terms of weight percentage, the total content k of the doping element K is: 2000ppm≤k≤4000ppm; S2, placing the material A to be sintered into a box furnace for high-temperature sintering, and maintaining the oxygen concentration in the furnace ≥ 96% throughout the process, the temperature is raised from 25°C at 3°C / min, raised to 500°C and kept for 4 hours, after the insulation is completed, the temperature is raised to 700-850°C at 3°C / min for constant temperature sintering for 12 hours, then cooled to 300°C at 5°C / min, the power is turned off, and the material temperature is taken out after it drops to room temperature to obtain material B; S3, the binary precursor Ni a Mn 1-a (OH) 2 Add to the sand mill, the grinding ball used for sand milling is a zirconium ball with a diameter of 0.8 mm, the sand milling medium is deionized water, the dispersant is polyacrylate, the sand milling time is ≥8h, the particle size of the precursor after sand milling is controlled to be 100~1000nm, the sand milled slurry is mixed with the material B to obtain material C, and the material C is rotated at high speed with a stirring paddle, the stirring paddle speed is ≥350 rpm, and the high-speed mixing time is 15M C / 2.5min to obtain material D, where M C is the weight of material C in kg; material D is spray dried to form balls, the inlet temperature of the spray drying chamber is 350°C, the outlet temperature is 100°C, the solid content of the material is ≥60% by mass, the spray disk speed is 30,000 rpm, and the ultra-high nickel quaternary material E uniformly coated with the binary precursor is obtained after spray drying process.
2. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 1, It is characterized in that Also includes: S4. Place ultra-high nickel quaternary material E into the box body, and use 3~5mm wide iron sheets to mark the material in the box in a tic-tac-toe pattern to facilitate full contact between the material and oxygen. The oxygen concentration is ≥96%. The temperature is raised from 25℃ at 3℃ / min to 500℃ and kept warm for 4h. After the insulation, the temperature is raised to 550-700℃ at 3℃ / min for constant temperature sintering for 10h, then cooled to 300℃ at 5℃ / min. Turn off the power, and take out the material after the temperature drops to room temperature to obtain material F, and mix material F with additive W.
3. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 2, It is characterized in that Also includes: S5. Then put the mixed materials into a sagger, and use a 3-5 mm wide iron sheet to mark the materials in the sagger in a tic-tac-toe pattern to facilitate full contact between the materials and oxygen. The oxygen concentration is ≥96%. The temperature is raised from 25°C at 3°C / min to 300-400°C for 8h, and then lowered to 300°C at 5°C / min. Turn off the power, and take out the finished material G after the material temperature drops to room temperature; wherein the finished material G is an ultra-high nickel quaternary material doped with high-valent ions; S6. Make material G into a soft-pack battery for electrical performance evaluation.
4. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 1, Features: The lithium source powder is battery-grade lithium hydroxide, lithium carbonate or a mixture of the two in different proportions.
5. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 1, Features: The binary precursor Ni a Mn 1-a (OH) 2 , a≤40mol%.
6. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 1, Features: The binary precursor Ni a Mn 1-a (OH) 2 In the process, the particle size D50 of the binary precursor is 2-10 μm, and the solid content of the slurry is ≥50% by mass.
7. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 2, Features: The additive W is TiO 2 、Al 2 O 3 , BO 3 、LaO 2 , WO 3 、Co(OH)、AlPO 4 NH 4 PO 3 One or both of the following.
8. The method for preparing a surface-coated ultra-high nickel quaternary nickel-cobalt-manganese-aluminum lithium oxide material according to claim 7, Features: In terms of mass percentage, the total amount of the additive W is controlled to be ≤4000ppm.
Citation Information
Patent Citations
Preparation method of manganese-based compound positive pole material for secondary lithium ion battery
CN102820464A
Ternary cathode material for lithium ion battery and preparation method thereof
CN106532035A
Lithium battery nickel-cobalt lithium manganate ternary anode material and preparation method thereof
CN107302087A
Preparation method of modified single-crystal ultrahigh-nickel quaternary NCMA positive electrode material
CN114524468A
Preparation method of over-lithium layered manganese-based oxide coated ternary positive electrode material
CN115231629A
Cited By
Preparation method of ternary high-nickel positive electrode material applied to mobile power bank
CN120698517A
A method for preparing ternary high-nickel cathode material for use in portable power banks
CN120698517B