Pressed ceramic ultra-fine oilstone and preparation method thereof
By adjusting the formula and preparation process of ceramic super essential oil stones and using potassium silicate or sodium silicate to enhance connectivity, the problems of long production cycle and low qualification rate of ceramic super essential oil stones are solved, achieving more efficient production and lower costs. Scrap rate.
Patent Information
- Application Number
- CN202410723000.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-05
AI Technical Summary
The production cycle of ceramic super essential oil stone is long and the product qualification rate is low, resulting in low production efficiency and prone to cracks and cracking problems.
It is composed of 90%-95% abrasive and 5%-10% ceramic bond. The abrasive is corundum with a particle size of F800-F1500. The ceramic bond is composed of clay, boron glass, bentonite, dextrin powder and silicon. Composed of potassium acid, the oil stone is prepared through ultrasonic vibration mixing, three-dimensional mixing and stirring, hydraulic pressing and high-temperature firing, removing feldspar and talcum powder, and using potassium silicate or sodium silicate as a wetting agent to enhance connectivity and prevent cracks.
The drying period is significantly shortened to 2-3 days, production efficiency is improved, the scrap rate is reduced, and the qualification rate and surface smoothness of the whetstone are improved.
Smart Images

Figure BDA0004877756430000061 
Figure BDA0004877756430000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oilstone production, in particular to a pressed ceramic super-fine oilstone and a preparation method thereof. Background Art
[0002] Whetstone is a kind of grinding tool widely used in precision machining, metal surface treatment, arts and crafts, etc. It is famous for its delicate texture and excellent wear resistance. With the rapid development of high-end equipment, the requirements for the use of whetstones are getting higher and higher, especially ceramic super-fine whetstones. Most ceramic super-fine whetstones use ceramic binders, which have the characteristics of high strength, good heat resistance, not easy to heat up and clog during grinding, easy to control machining accuracy, and easy to trim. They are widely used in super-finishing of high-end precision equipment parts such as aerospace engines, instruments and meters, and high-precision machine tools. In the process of super-finishing of precision equipment parts, only when the surface roughness reaches the specified standard can high-precision parts with excellent performance be made. Whetstone plays a vital role in the final quality of high-end parts and can significantly affect the efficiency of the grinding process.
[0003] In the production process of ceramic superfine oilstone, due to the evaporation of water in the wetting agent, the contact area between the abrasive and the surface of the ceramic binder is reduced, and some of them will be separated. In the subsequent drying and firing process, cracks and cracks will appear on the surface of the superfine oilstone, resulting in the material being scrapped and unusable. In order to reduce the occurrence of cracks and cracks, the superfine oilstone is usually placed in a constant temperature and humidity environment for 10-15 days to allow the water to evaporate slowly to reduce the occurrence of cracks. However, this production method has a long cycle, slow production efficiency, and low product qualification rate, which seriously affects production efficiency. Although a mixture of coarse-grained ceramic binder and ultrafine abrasive can be used to make superfine oilstone, so as to reduce the production cycle and improve production efficiency, and the product qualification rate is high, due to the coarse particle size of the binder, the workpiece is easily damaged during the grinding process, and the surface roughness is poor, which cannot meet the requirements of ceramic superfine oilstone.
[0004] There is an urgent need to develop a pressed ceramic super-fine oilstone and a preparation method thereof to solve the above-mentioned problems of long production cycle and low product qualification rate of ceramic super-fine oilstone. Summary of the invention
[0005] In view of the above situation, in order to overcome the defects of the prior art;
[0006] The present invention provides a pressed ceramic superfine oilstone and a preparation method thereof, which is composed of 90%-95% of abrasive and 5%-10% of a ceramic binder by mass percentage, wherein:
[0007] The abrasive is composed of corundum with a particle size of F800-F1500;
[0008] The ceramic binder is composed of 5%-16% clay, 12%-60% boron glass, 10%-30% bentonite, 15%-40% dextrin powder, and 8%-54% potassium silicate;
[0009] Preferably, the potassium silicate in the ceramic binder can be replaced with sodium silicate of equal mass, and the corundum is one of white corundum or brown corundum.
[0010] A method for preparing oilstone comprises the following steps:
[0011] S1. Preparation of ceramic binder: Add the above ceramic binder raw materials into an ultrasonic vibrator and mix them evenly. The ultrasonic vibration time is 0.5-2h. After mixing, the finished ceramic binder is obtained;
[0012] S2. Mixing of oilstone: Add the abrasive and finished ceramic binder into a three-dimensional mixing pot at the same time and stir evenly for 2-4 hours at a speed of 60r / min. Pour the evenly mixed mixture into the mixing pot, and add dextrin liquid and water glass in turn. Stir continuously for 20-30 minutes to obtain the molding material of oilstone.
[0013] S3. Pressing of oilstone: Pass the mixed molding material through a 20#-46# screen, pour the molding material after passing through the screen into the molding mold, stir the molding material evenly with a scraper and a material fork, and flatten it. Put the mold with the molding material under a hydraulic press for pressing, and press continuously for 4 times at a pressure of 10-15Mpa. The holding time of each pressing is 15-30s. After unloading the mold, the oilstone blank can be obtained;
[0014] S4. Forming of oilstone: Dry the oilstone blank at room temperature for 2-4 days, then put it into a high-temperature furnace and fire it at 950℃-1070℃ for 10-26h, with a heating rate of 1-3℃ / min. Keep it warm for 3-5h after firing, and obtain the finished oilstone after natural cooling.
[0015] Preferably, the mass of the dextrin liquid in step S2 is 1%-1.5% of the total weight of the corundum and the ceramic binder, and the concentration is 30%-40%wt.
[0016] Preferably, the mass of the water glass in step S2 is 1.6%-1.9% of the total weight of the corundum and the ceramic binder, and the concentration is 35%-45%wt. The water glass can be replaced with an aqueous solution of glycerol or PEG2000 of equal mass.
[0017] Compared with the prior art, the present invention provides a pressed ceramic super-fine oil stone and a preparation method thereof, which has the following beneficial effects:
[0018] In the formula of the ceramic binder, the conventionally used feldspar and talcum powder are removed, and a wetting agent that can produce corresponding coordination with dextrin liquid and water glass is selected, and the wetting agent is potassium silicate or sodium silicate, which can increase the overall connectivity. The mixing of potassium silicate and dextrin liquid and the colloidal properties of dextrin can improve the rheology and stability of the potassium silicate solution, thereby increasing its adhesive performance and heat resistance, so as to increase its connection state and prevent cracking; and the combination of potassium silicate and water glass can provide a good alkaline environment and a strong complexing effect for the water glass, so as to increase the connectivity and prevent the occurrence of cracks and cracks during drying. At the same time, the drying period of 10-15 days can be shortened to the current 2-3 days, and the time is shortened by more than 80%, which greatly improves the production efficiency of the oilstone and reduces the scrap rate of the oilstone. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Embodiment 1:
[0021] The oilstone is composed of 92% abrasive and 8% vitrified binder by mass, of which:
[0022] The abrasive consisted of white corundum with a particle size of F1000;
[0023] The vitrified binder is composed of 7.5% clay, 21.25% boron glass, 15% bentonite, 25% dextrin powder, and 31.25% potassium silicate;
[0024] The mass of the dextrin liquid is 1.2% of the total weight of the corundum and the ceramic binder, and the concentration is 35%wt;
[0025] The mass of water glass is 1.7% of the total weight of corundum and ceramic binder, and the concentration is 40%wt;
[0026] A method for preparing oilstone comprises the following steps:
[0027] S1. Preparation of ceramic binder: Add the above ceramic binder raw materials into an ultrasonic vibrator and mix them evenly. The ultrasonic vibration time is 1 hour. After mixing, the finished ceramic binder is obtained;
[0028] S2. Mixing of oilstone: Add the abrasive and the finished ceramic binder into a three-dimensional mixing pot at the same time and stir evenly for 2.5 hours at a speed of 60r / min. Pour the evenly mixed mixture into the mixing pot, and add dextrin liquid and water glass in turn. Stir continuously for 25 minutes to obtain the molding material of oilstone.
[0029] S3. Pressing of oilstone: Pass the mixed molding material through a 30# screen, pour the molding material after passing through the screen into the molding mold, stir the molding material evenly with a scraper and a material fork, and flatten it. Put the mold with the molding material under a hydraulic press for pressing, press continuously for 4 times at a pressure of 11Mpa, and the holding time of each pressing is 20s. After unloading the mold, the oilstone blank can be obtained;
[0030] S4. Forming of oilstone: Dry the oilstone blank at room temperature for 2 days, then put it into a high-temperature furnace and fire it at 980℃ for 14 hours at a heating rate of 1.5℃ / min. Keep it warm for 4 hours after firing, and the finished oilstone will be obtained after natural cooling.
[0031] Embodiment 2:
[0032] The oilstone is composed of 95% abrasive and 5% vitrified binder by mass, wherein:
[0033] The abrasive consisted of white corundum with a particle size of F800;
[0034] The ceramic binder is composed of 10% clay, 15% boron glass, 5% bentonite, 20% dextrin powder, and 50% potassium silicate;
[0035] The mass of the dextrin liquid is 1% of the total weight of the corundum and the ceramic binder, and the concentration is 35%wt;
[0036] The mass of water glass is 3% of the total weight of corundum and ceramic binder, and the concentration is 40%wt;
[0037] The production steps remain the same as in Example 1;
[0038] The difference between Example 2 and Example 1 is that the percentage of abrasive and ceramic binder and the proportion of raw materials are changed, the particle size of the abrasive is adjusted, and the mass of dextrin liquid and water glass is changed. The remaining steps remain the same as Example 1.
[0039] Embodiment 3:
[0040] The oilstone is composed of 94% abrasive and 6% vitrified binder by mass, of which:
[0041] The abrasive consisted of white corundum with a particle size of F1200;
[0042] The ceramic binder is composed of 7.5% clay, 21.25% boron glass, 15% bentonite, 25% dextrin powder, and 31.25% sodium silicate;
[0043] The mass of the dextrin liquid is 1.1% of the total weight of the corundum and the ceramic binder, and the concentration is 35%wt;
[0044] The mass of water glass is 3.0% of the total weight of corundum and ceramic binder, and the concentration is 40%wt;
[0045] The production steps remain the same as in Example 1;
[0046] The difference between Example 3 and Example 1 is that the percentage of abrasive and ceramic binder is changed, the particle size of the abrasive is changed, and the mass of dextrin liquid and water glass added is adjusted. The other steps remain the same as Example 1.
[0047] Comparative Example 1:
[0048] The oilstone is composed of 92% abrasive and 8% binder by mass, of which:
[0049] The abrasive consisted of white corundum with a particle size of F1000;
[0050] The binder is composed of 7.5% clay, 21.25% boron glass, 15% bentonite, 25% dextrin powder, 26.25% feldspar, and 5% talc;
[0051] The mass of the dextrin liquid is 1.2% of the total weight of the corundum and the binder, and the concentration is 35%wt;
[0052] The mass of water glass is 1.7% of the total weight of corundum and binder, and the concentration is 40%wt;
[0053] A method for preparing oilstone comprises the following steps:
[0054] S1. Preparation of binder: Add the above binder raw materials into an ultrasonic vibrator and mix them evenly. The ultrasonic vibration time is 1 hour. After mixing, the finished binder is obtained;
[0055] S2. Mixing of oilstone: Add the abrasive and finished binder into a three-dimensional mixing pot at the same time and stir evenly for 2.5 hours at a speed of 60r / min. Pour the evenly mixed mixture into the mixing pot, and add dextrin liquid and water glass in turn. Stir continuously for 25 minutes to obtain the molding material of oilstone.
[0056] S3. Pressing of oilstone: Pass the mixed molding material through a 30# screen, pour the molding material after passing through the screen into the molding mold, stir the molding material evenly with a scraper and a material fork, and flatten it. Put the mold with the molding material under a hydraulic press for pressing, press continuously for 4 times at a pressure of 11Mpa, and the holding time of each pressing is 20s. After unloading the mold, the oilstone blank can be obtained;
[0057] S4. Forming of oilstone: Dry the oilstone blank at room temperature for 10 days, then put it into a high-temperature furnace and fire it at 980℃ for 20h at a heating rate of 1.1℃ / min. Keep it warm for 4h after firing, and obtain the finished oilstone after natural cooling.
[0058] The difference between Comparative Example 1 and Example 1 is that the potassium silicate in the binder is replaced with feldspar and talcum powder of the same mass, and the parameters in the molding step are adjusted accordingly according to the drying of the oilstone, and the remaining steps remain the same as Example 1.
[0059] Comparative Example 2:
[0060] The oilstone is composed of 92% abrasive and 8% binder by mass, of which:
[0061] The abrasive consisted of white corundum with a particle size of F800;
[0062] The binder is composed of 7.5% clay, 21.25% boron glass, 15% bentonite, 25% dextrin powder, 26.25% feldspar, and 5% talc;
[0063] The mass of the dextrin liquid is 1.2% of the total weight of the corundum and the binder, and the concentration is 35%wt;
[0064] The mass of water glass is 1.7% of the total weight of corundum and binder, and the concentration is 40%wt;
[0065] The production steps remain the same as those of Comparative Example 1;
[0066] The difference between Comparative Example 2 and Example 1 is that the particle size of the abrasive is changed, and the potassium silicate in the binder is replaced with feldspar and talc of the same mass, and the production steps remain the same as those of Comparative Example 1.
[0067] Comparative Example 3:
[0068] The oilstone is composed of 94% abrasive and 6% binder by mass, of which:
[0069] The abrasive consisted of white corundum with a particle size of F1200;
[0070] The binder is composed of 7.5% clay, 21.25% boron glass, 15% bentonite, 25% dextrin powder, 26.25% feldspar, and 5% talc;
[0071] The mass of the dextrin liquid is 1.2% of the total weight of the corundum and the binder, and the concentration is 35%wt;
[0072] The mass of water glass is 1.7% of the total weight of corundum and binder, and the concentration is 40%wt;
[0073] The production steps remain the same as those of Comparative Example 1;
[0074] The difference between Comparative Example 3 and Example 3 is that the potassium silicate in the binder is replaced with feldspar and talc of the same mass, and the masses of dextrin liquid and water glass added are adjusted, and the production steps remain the same as those of Comparative Example 1.
[0075] The following is a comparative analysis of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3:
[0076] Under the same parameters, the firing quantity, drying time, amount of waste after drying, firing quantity, firing time, amount of waste after firing and qualified rate of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were compared respectively.
[0077] Table 1 Performance comparison
[0078]
[0079]
[0080] It can be seen from the above table that the data of Example 1, Example 2 and Example 3 using the preparation method in combination with a ceramic binder are better than those of Comparative Example 1, Comparative Example 2 and Comparative Example 3 using a common binder, among which Example 1 has the best overall qualified rate, and the amount of waste after drying and firing in Example 1 is less than that in Example 2 and Example 3. At the same time, it can also be seen from the above table that the time for Example 1, Example 2 and Example 3 to be placed in the outside for drying is shorter than that of Comparative Example 1, Comparative Example 2 and Comparative Example 3, indicating that the preparation method can effectively shorten the time required for the oilstone to be dried, and at the same time, the firing time is also shortened accordingly.
[0081] It can be seen from this that through the mutual cooperation of potassium silicate or sodium silicate and dextrin liquid, the oil stone using the preparation method can effectively shorten the firing time, and at the same time can shorten the corresponding firing time, and the qualified rate of the oil stone made by this production method is better than other oil stones, and the drying cycle is effectively shortened, and the number of waste products after drying is small. In addition, the oil stone will not produce cracks during drying, which greatly improves production efficiency.
Claims
1. A pressed ceramic superfine oil stone, characterized in that: By mass percentage, it is composed of 90%-95% abrasive and 5%-10% vitrified binder, of which: The abrasive is composed of corundum with a particle size of F800-F1500; The ceramic binder is composed of 5%-16% clay, 12%-60% boron glass, 10%-30% bentonite, 15%-40% dextrin powder, and 8%-54% potassium silicate.
2. A pressed ceramic superfine oil stone and a preparation method thereof according to claim 1, characterized in that: The potassium silicate in the ceramic binder can be replaced with sodium silicate of equal mass, and the corundum is one of white corundum and brown corundum.
3. A method for preparing an oilstone, for producing a pressed ceramic superfine oilstone as claimed in claims 1 to 2, characterized in that: The method for preparing the oilstone comprises the following steps: S1. Preparation of ceramic binder: Add the above ceramic binder raw materials into an ultrasonic vibrator and mix them evenly. The ultrasonic vibration time is 0.5-2h. After mixing, the finished ceramic binder is obtained; S2. Mixing of oilstone: Add the abrasive and finished ceramic binder into a three-dimensional mixing pot at the same time and stir evenly for 2-4 hours at a speed of 60r / min. Pour the evenly mixed mixture into the mixing pot, and add dextrin liquid and water glass in turn. Stir continuously for 20-30 minutes to obtain the molding material of oilstone. S3. Pressing of oilstone: Pass the mixed molding material through a 20#-46# screen, pour the molding material after passing through the screen into the molding mold, stir the molding material evenly with a scraper and a material fork, and flatten it. Put the mold with the molding material under a hydraulic press for pressing, and press continuously for 4 times at a pressure of 10-15Mpa. The holding time of each pressing is 15-30s. After unloading the mold, the oilstone blank can be obtained; S4. Forming of oilstone: Dry the oilstone blank at room temperature for 2-4 days, then put it into a high-temperature furnace and fire it at 950℃-1070℃ for 10-26h, with a heating rate of 1-3℃ / min. Keep it warm for 3-5h after firing, and obtain the finished oilstone after natural cooling.
4. A pressed ceramic superfine oil stone and a preparation method thereof according to claim 3, characterized in that: The mass of the dextrin liquid in step S2 is 1%-1.5% of the total weight of the corundum and the ceramic binder, and the concentration is 30%-40%wt.
5. A pressed ceramic superfine oil stone and a preparation method thereof according to claim 3, characterized in that: The mass of the water glass in step S2 is 1.6%-1.9% of the total weight of the corundum and the ceramic binder, and the concentration is 35%-45%wt. The water glass can be replaced with an aqueous solution of glycerol or PEG2000 of equal mass.
Citation Information
Patent Citations
Shaft grinding abrasive wheel
CN101186028A
Novel ceramic corundum grinding tool of low-temperature and high-strength ceramic bonding agent and preparation method thereof
CN102699825A
Stainless steel and titanium alloy screen cloth matrix ceramic grinding wheel for grinding
CN103042475A
Vitrified bonded grinding wheel manufacturing method