Chromophore compound, preparation method thereof and application of chromophore compound

By introducing chromophore compounds with multiple cross-linking groups into organic nonlinear electro-optical materials, the problems of high cross-linking temperature and poor stability of existing materials have been solved, and efficient cross-linking and stability improvement of electro-optical materials have been achieved, significantly Improved electro-optical coefficient and glass transition temperature.

CN118724849APending Publication Date: 2024-10-01HUAWEI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310364715.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The glass transition temperature of existing organic nonlinear electro-optical materials is low and the cross-linking temperature is high, which causes the polarized chromophore molecules to easily become negative, causing the electro-optical coefficient to attenuate or disappear, thereby causing device failure.

Method used

Design a chromophore compound containing an electron donor, an electron bridge group and an electron acceptor group to improve cross-linking by introducing at least two first cross-linkable groups and one second cross-linkable group efficiency and glass transition temperature, reduce the loss of electro-optical coefficient before and after cross-linking, and reduce the cross-linking temperature and time through the binary cross-linking system.

Benefits of technology

It achieves cross-linking at a lower temperature and a shorter time, improves the photothermal stability and polarization orientation stability of the electro-optical material, reduces the loss of the electro-optical coefficient, and increases the electro-optical coefficient and glass transition temperature of the electro-optical material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724849A_ABST
    Figure CN118724849A_ABST
Patent Text Reader

Abstract

The invention provides a chromophore compound, the structure of the chromophore compound is # imgabs0 #, and D is an atom or an organic group capable of providing electrons; a is an electron acceptor group; z, L1 and L2 are respectively and independently selected from organic groups with at least divalent atoms or at least two chemical bonds; x1 is a first crosslinkable group; x2 is a second crosslinkable group; pi 1 and Pi 2 are respectively and independently Pi bridges; p is an integer greater than or equal to 2, and q is an integer greater than or equal to 1. The invention also provides a preparation method of the chromophore compound, and an electro-optical material, a film, electro-optical glass, an electro-optical device and electronic equipment using the chromophore compound. According to the chromophore compound disclosed by the invention, at least three crosslinkable groups are introduced, so that the chromophore compounds can be crosslinked at a lower temperature within a shorter time, the glass transition temperature after crosslinking is relatively high, and the loss of electro-optical coefficients before and after crosslinking is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of organic optical materials, and specifically to a chromophore compound and a preparation method thereof, an electro-optical material containing the chromophore compound, a film and an electro-optical glass containing the electro-optical material, an electro-optical device using the film or the electro-optical glass, and an electronic device using the electro-optical device. Background Art

[0002] With the rapid development of technologies such as cloud computing, 5G communications, high-definition network video, and the Internet of Things, as well as the rapid growth of information demand, medium- and short-distance communication systems such as data center networks are increasingly demanding ultra-large-capacity optical fiber communications. For medium- and short-distance optical communication systems, how to achieve ultra-high-speed (single wavelength 400Gb / s or more) signal transmission under the limited bandwidth of optoelectronic devices will face huge challenges. Electro-optical modulators are the core components for realizing optoelectronic information conversion, and are also the key link in breaking through the two major technical challenges of bandwidth and signal transmission rate.

[0003] Electro-optical materials are the key components of electro-optic modulators. The glass transition temperature (Tg) of the chromophore of existing organic nonlinear electro-optical materials is low, and the cross-linking temperature is high. When the heating temperature reaches the cross-linking temperature of the chromophore, the temperature has exceeded the glass transition temperature, and the polarized chromophore molecules are prone to passivation (i.e. relaxation), and the electro-optic coefficient will decay or even disappear, resulting in device failure. Summary of the invention

[0004] In view of this, in order to solve at least one of the above defects, an embodiment of the present application provides a chromophore compound, which can complete the cross-linking reaction at a lower cross-linking temperature and a shorter cross-linking time, and the glass transition temperature (Tg) of the obtained cross-linked electro-optical material is higher, and the electro-optical coefficient loss of the electro-optical material before and after cross-linking is smaller.

[0005] In addition, the embodiments of the present application also provide a method for preparing the chromophore compound, an electro-optical material containing the chromophore compound, a film and an electro-optical glass containing the electro-optical material, an electro-optical device using the film or the electro-optical glass, and an electronic device using the electro-optical device. The electro-optical material using the chromophore compound has a large electro-optical coefficient, as well as high photothermal stability and polarization orientation stability.

[0006] The first aspect of the embodiment of the present application provides a chromophore compound, wherein the chromophore compound has the structure of the following formula (I):

[0007]

[0008] Wherein, D is an atom or organic group that can provide electrons;

[0009] A is an electron acceptor group;

[0010] Z is an atom having at least two valences or an organic group having at least two chemical bonds;

[0011] L 1 and L 2 are independently selected from an atom having at least two valences or an organic group having at least two chemical bonds;

[0012] π 1 and π 2 Each independently is a π bridge;

[0013] X 1 is a first cross-linkable group;

[0014] X 2 is a second cross-linkable group;

[0015] p is an integer greater than or equal to 2;

[0016] q is an integer greater than or equal to 1.

[0017] By introducing at least two structures having a first cross-linkable group on the electron donor of the chromophore compound, and at least one second cross-linkable group is connected to the electron bridge group, the macroscopic electro-optical activity of the chromophore compound can be improved. At the same time, the chromophore compound has at least three cross-linking sites. The three cross-linkable groups increase the possibility of a cross-linking reaction relative to two cross-linking groups, which helps to increase the glass transition temperature, thereby enabling the chromophore compounds to cross-link at a lower temperature, and effectively improving the cross-linking efficiency of the chromophore compounds, shortening the cross-linking time, thereby reducing the loss of the electro-optic coefficient of the chromophore compounds before and after cross-linking; the cross-linking process does not require the introduction of a cross-linking agent separately, thereby increasing the content of the chromophore compound in the electro-optical material, further increasing the electro-optical coefficient of the electro-optical material, and at the same time, cross-linking can further increase the glass transition temperature (Tg) of the electro-optical material, thereby improving the photothermal stability and polarization orientation stability of the electro-optical material.

[0018] In addition, the chromophore compound contains at least three cross-linkable groups, which can increase the distance between the molecules of the chromophore compound, weaken the electrostatic interaction between the molecules, and help improve the polarization efficiency of the chromophore compound.

[0019] In some embodiments, D in formula (I) is a nitrogen atom.

[0020] The nitrogen atom has a strong electron donating ability, which can enhance the electron donating ability of the electron donor group and facilitate the introduction of two structures containing the first cross-linkable group.

[0021] In some embodiments, Z in formula (I) is a sulfur atom, an oxygen atom or an alkyl group.

[0022] The stability of the molecular structure of the chromophore compound can be improved by introducing a sulfur atom, an oxygen atom or an alkyl group into the electron bridging group.

[0023] In some embodiments, L in formula (I) 1 and L 2 Each of the at least one groups is independently selected from an alkyl group, an ester group, an aryl group and a heteroaryl group.

[0024] By introducing L 1 and L 2 The length of the side chain of the chromophore compound can be adjusted to facilitate the subsequent cross-linking reaction between the chromophore compounds or between the chromophore compound and the polymer. At the same time, the flexibility of the chromophore compound can be changed by introducing different types of groups.

[0025] In some embodiments, p in the formula (I) can be 2 or 3, etc., and q can be 1 or 2, etc.

[0026] By limiting p and q in the formula (I), that is, the first cross-linkable group can be connected to two or three, and the second cross-linkable group can be connected to one or two, the number of cross-linking sites in the chromophore compound can be significantly increased, so as to further shorten the cross-linking time, thereby further reducing the electro-optical coefficient loss of the chromophore compound before and after cross-linking.

[0027] In some embodiments, both the first cross-linkable group and the second cross-linkable group are groups that can undergo click chemistry reaction, thermal cross-linking reaction, photo-cross-linking reaction, coupling reaction or polymerization reaction.

[0028] In some embodiments, the first crosslinkable group and the second crosslinkable group are independently selected from an anthracene group, a maleimide group, an acrylate group, an azide group, an alkynyl group, a hydroxyl group, an isocyanate group, a furan group, a thiol group, an olefin group, a coumarin group, a difluoroolefin group, a styrene group and any one of the derivatives of these groups.

[0029] Specifically, the first crosslinkable group and the second crosslinkable group are independently selected from any one of the following structures:

[0030]

[0031] as well as

[0032] In some embodiments, the first cross-linkable group and the second cross-linkable group are the same.

[0033] By introducing the same first cross-linkable group and the second cross-linkable group into the same chromophore compound, a binary cross-linking system can be realized. At the same time, the first cross-linkable group and the second cross-linkable group can be introduced simultaneously in a one-step reaction. The reaction process is easier to achieve, the reaction conditions are easy to control, and the synthesis steps can be simplified.

[0034] In some embodiments, the chromophore compound has a structure of Formula (II) or Formula (III):

[0035]

[0036] By introducing three anthracene groups or three maleimide groups into the chromophore compound, two different chromophore compounds can be obtained, thereby constructing a binary cross-linking system, wherein the reaction of three anthracene groups and three maleimide groups can effectively reduce the cross-linking temperature and shorten the cross-linking time (the cross-linking temperature of the above structure is reduced to below 120°C, and the cross-linking time can be shortened to below 15 minutes), which is beneficial to increase the glass transition temperature of the material (Tg reaches 178°C), thereby improving the stability of the material, and at the same time minimizing the loss of the electro-optic coefficient of the chromophore compound before and after cross-linking (the electro-optic coefficient of the binary chromophore cross-linking system of the above structure can reach 266pm / V).

[0037] The second aspect of the embodiment of the present application further provides a method for preparing a chromophore compound, the preparation method comprising the following steps:

[0038] Connecting an electron bridge molecule containing at least one second reactive group to an electron donor molecule containing at least two first reactive groups to obtain an electron donor group-electron bridge group compound containing the at least two first reactive groups and the at least one second reactive group; and

[0039] At least one first crosslinkable group and at least one second crosslinkable group are respectively connected to each of the first reactive groups and each of the second reactive groups of the electron donor group-electron bridge group compound, and an electron acceptor group is connected to the electron bridge group of the electron donor group-electron bridge group compound, thereby obtaining the chromophore compound,

[0040] Wherein, the chromophore compound has the structure of the following formula (I):

[0041]

[0042] Wherein, D is an atom or organic group that can provide electrons;

[0043] A is an electron acceptor group;

[0044] Z is an atom having at least two valences or an organic group having at least two chemical bonds;

[0045] π 1 and π 2 Each independently is a π bridge;

[0046] L 1 and L 2 are independently selected from an atom having at least two valences or an organic group having at least two chemical bonds;

[0047] X 1 is the first cross-linkable group;

[0048] X 2 is the second cross-linkable group;

[0049] p is an integer greater than or equal to 2;

[0050] q is an integer greater than or equal to 1.

[0051] The electron donor molecule and the electron bridge molecule respectively contain at least two first reactive groups and at least one second reactive group, which can provide active connection sites, facilitate the introduction of at least two first cross-linkable groups and at least one second cross-linkable group, and do not need to add the step of introducing active connection sites on the electron donor molecule and the electron bridge molecule, making the synthesis of the chromophore compound easier. Therefore, the preparation method is easy to implement, simplifies the synthesis steps, has a high yield of intermediate products and final products, and the chromophore compound can be dissolved in most organic solvents, which is conducive to large-scale production and commercial application.

[0052] In some embodiments, the electron donor molecule has the structure of formula (IV):

[0053] Among them, R 3 is the first reactive group, and the first reactive group is selected from any one of a hydroxyl group, an azide group, an alkynyl group, a thiol group, an isocyanate group, an amino group and the like.

[0054] In some embodiments, D in formula (I) is a nitrogen atom.

[0055] In some embodiments, the second reactive group is selected from any one of a hydroxyl group, an azide group, an alkynyl group, a thiol group, an isocyanate group, and an amino group.

[0056] In some embodiments, before connecting the electron bridge molecule to the electron donor molecule, the preparation method further comprises the steps of:

[0057] attaching a first protecting group to each of the first reactive groups;

[0058] After the electron bridge molecule is connected to the electron donor molecule, the preparation method further comprises the steps of:

[0059] attaching a second protecting group to each of the second reactive groups;

[0060] Before respectively connecting at least one first crosslinkable group and at least one second crosslinkable group to each of the first reactive groups and each of the second reactive groups of the electron donor group-electron bridging group compound, the preparation method further comprises the steps of:

[0061] The first protecting group and the second protecting group are removed.

[0062] By generating the first protecting group and the second protecting group on the first reactive group and the second reactive group respectively and removing the first protecting group and the second protecting group after the corresponding reaction is completed, the first reactive group and the second reactive group can be protected from being affected during the reaction.

[0063] In some embodiments, the electron bridge molecule includes any one of isophorone, thiophene bridge, and pyrrole bridge.

[0064] In some embodiments, the first protecting group and the second protecting group are derived from any one of tert-butyldimethylsilyl chloride and its derivatives, tert-butyldiphenylsilyl chloride and its derivatives, and dihydropyran derivatives.

[0065] In some embodiments, the electron donor molecule has a structure of The first compound is prepared from a first crosslinkable group and a second crosslinkable group, wherein the electron bridge molecule is isophorone, the electron acceptor molecule is 2-(3-cyano-4-methyl-5-phenyl-5-(trifluoromethyl)furan-2(5H)-ethylidene)malononitrile, the first crosslinkable group and the second crosslinkable group are the same, and the preparation method comprises the following steps:

[0066] A tert-butyldimethylsilyl group is generated on the hydroxyl group of the first compound to obtain a structure of a second compound;

[0067] The second compound is reacted with isophorone in sodium ethoxide and 2-mercaptoethanol to obtain a compound having the structure A third compound;

[0068] A tert-butyldimethylsilyl group is generated on the hydroxyl group of the third compound to obtain a structure of The fourth compound of

[0069] The fourth compound is reacted with diethyl phosphate by Wittig-Hornor reaction to obtain a structure of The fifth compound;

[0070] The nitrile group in the fifth compound is reduced by diisobutylaluminum hydride to obtain a structure of The sixth compound of

[0071] The sixth compound is subjected to acid hydrolysis to remove the tert-butyldimethylsilyl group to obtain a structure of The seventh compound;

[0072] The seventh compound and R 4 OH undergoes nucleophilic substitution reaction or Steglich esterification reaction to obtain the structure An eighth compound of

[0073] The eighth compound is condensed with the electron acceptor molecule to obtain a product having a structure of The chromophore compound,

[0074] Among them, R connected to the N atom 4 is the first cross-linkable group, and R 4 The second cross-linkable group, R 4 Any one selected from anthracene group, maleimide group, acrylate group, azide group, alkynyl group, hydroxyl group, isocyanate group, furan group, thiol group, olefin group, coumarin group, difluoroolefin group, styrene group and derivatives of these groups, specifically any one of the following structures:

[0075]

[0076] By introducing an electron donor structure containing a hydroxyl group and an isophorone electron bridge containing a hydroxyl group, and by connecting a first protective group and a second protective group to the hydroxyl group and removing them respectively, it is avoided that the two hydroxyl groups are affected before the first crosslinkable group and the second crosslinkable group are introduced; the introduced first crosslinkable group and the second crosslinkable group are the same and can be introduced at the same time, the reaction conditions are easy to control, the reaction is more likely to occur, and the synthesis steps are simplified.

[0077] A third aspect of an embodiment of the present application provides an electro-optical material, which includes at least two chromophore compounds, and at least two of the chromophore compounds are used for cross-linking reaction. The chromophore compounds are the chromophore compounds described in the first aspect of the embodiment of the present application or the chromophore compounds prepared by the preparation method described in the second aspect of the embodiment of the present application.

[0078] The electro-optical material composed of the aforementioned chromophore compounds can effectively reduce the cross-linking temperature between the chromophore compounds and shorten the cross-linking time (for example, the cross-linking temperature can be reduced to below 120°C, and the cross-linking time can be shortened to less than 15 minutes), while increasing the glass transition temperature of the electro-optical material (Tg reaches above 178°C), which is beneficial to improving the photothermal stability and polarization orientation stability of the electro-optical material, reducing the loss of the electro-optic coefficient before and after the cross-linking of the chromophore compounds, and thereby increasing the electro-optic coefficient of the electro-optical material (for example, the electro-optic coefficient can reach above 266pm / V).

[0079] In some embodiments, the electro-optical material includes two chromophore compounds, and when the first cross-linkable group and the second cross-linkable group on any one of the chromophore compounds are the same, the first cross-linkable group on one chromophore compound and the first cross-linkable group in the other chromophore compound are selected from any one of the following group combinations: anthracene group and maleimide group, azide group and alkyne group, hydroxyl group and isocyanate group, anthracene group and acrylate group, furan group and maleimide group, thiol group and olefin, coumarin group and coumarin group, difluoroolefin group and difluoroolefin group, and styrene group and styrene group.

[0080] A fourth aspect of the embodiments of the present application provides a film, which is made of the electro-optical material described in the third aspect of the embodiments of the present application.

[0081] A fifth aspect of the embodiments of the present application provides an electro-optical glass, which includes a glass substrate and the thin film described in the fourth aspect of the embodiments of the present application located on the glass substrate.

[0082] A sixth aspect of the embodiments of the present application provides an electro-optical device, which includes the film described in the fourth aspect of the embodiments of the present application, or includes the electro-optical glass described in the fifth aspect of the embodiments of the present application.

[0083] The polarized electro-optical film provided in the embodiment of the present application has a relatively high electro-optical coefficient (at least 266 pv / m), which is beneficial to improving the performance of electro-optical devices (such as photoelectric modulators); in addition, since the polarized electro-optical film has a cross-linked network structure, the glass transition temperature of the electro-optical film is increased (at least 178°C), thereby increasing the operating temperature of the electro-optical device.

[0084] The seventh aspect of the present application provides an electronic device, which includes the electro-optical device described in the sixth aspect of the embodiment of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0085] Figure 1 This is a schematic diagram of the polarization process of a device made of traditional organic electro-optical materials.

[0086] Figure 2 It is a schematic diagram of the polarization process of a device prepared using the binary cross-linked chromophore system (FZL1+FZL2) provided in the examples of the present application.

[0087] Figure 3 A process flow chart of the preparation of a chromophore compound is provided for one embodiment of the present application.

[0088] Figure 4 Schematic diagram of a film provided in one embodiment of the present application.

[0089] Figure 5 It is a schematic diagram of the electro-optical glass provided in one embodiment of the present application.

[0090] Figure 6 Schematic diagram of an electro-optical device provided in one embodiment of the present application.

[0091] Figure 7 It is a schematic diagram of an electronic device provided by an embodiment of the present application.

[0092] Fig. 8A It is the DSC curve diagram of FZL1 and FZL2 provided in Example 1 of the present application.

[0093] Figure 8B It is the DSC curve diagram of 1:1FZL1:FZL2(NC) and 1:1FZL1:FZL2(X-link) provided in Example 1 of the present application.

[0094] Fig. 9 It is the UV-visible spectra of FZL1 in Example 1 of the present application and HLD1 in Comparative Example 1 in chloroform.

[0095] Fig.10 These are the UV-visible spectra of the HLD1 film, HLD2 film, 2:1 HLD1:HLD2 (RT) film and HLD1:HLD2 (150° C.) film provided in Comparative Example 1 of the present application.

[0096] Fig.11 These are the UV-visible spectra of the FZL1 film, FZL2 film, 1:1FZL1:FZL2(CN) film and 1:1FZL1:FZL2(X-link) film provided in Example 1 of the present application.

[0097] FIG. 12A to FIG. 12D It is a polarization efficiency curve diagram of the FZL1 film, FZL2 film, 1:1FZL1:FZL2(CN) film and 1:1FZL1:FZL2(X-link) film provided in the embodiments of the present application after being assembled into an electro-optical device.

[0098] Main component symbols

[0099] DETAILED DESCRIPTION

[0100] The embodiments of the present application are described below in conjunction with the accompanying drawings in the embodiments of the present application. The data ranges involved in the present application should include the end values ​​unless otherwise specified.

[0101] The glass transition temperature (Tg) of the chromophore molecules of commonly used organic electro-optical materials is low, while the cross-linking temperature is high. During the polarization process, the chromophore compound molecules are polarized and oriented. However, when the temperature reaches the cross-linking temperature, the temperature exceeds the glass transition temperature of the chromophore molecules, and the thermal motion of the chromophore compound molecules becomes violent. The chromophore compound molecules that were originally polarized and oriented in the electric field are destroyed in antiparallel stacking due to thermal motion and intermolecular electrostatic interaction, and deorientation (i.e., relaxation) occurs. Figure 1 As shown, the photothermal stability and polarization orientation stability of organic electro-optical materials are poor, and the electro-optic coefficient is prone to decay or even disappear, thus causing the device to fail. In addition, since the commonly used chromophore molecules have a long cross-linking time, the degree of de-orientation mentioned above is further aggravated, making the degree of electro-optic coefficient decay more serious.

[0102] In view of this, an embodiment of the present application provides a chromophore compound, which can be used in electro-optical devices, such as electro-optical modulators, but is not limited thereto. The synthesis of the chromophore compound is optimized and selected so that the chromophore compound has a higher glass transition temperature, a lower cross-linking temperature and a shorter cross-linking time, which is beneficial to improving the photothermal stability and polarization orientation stability of the electro-optical material using the chromophore compound, while reducing the attenuation of the electro-optic coefficient before and after cross-linking, so that the electro-optical material has a higher electro-optical coefficient.

[0103] The chromophore compound comprises an electron donor group, an electron bridge group and an electron acceptor group, wherein the electron donor group is electronically conjugated with the electron acceptor group via the electron bridge group. The chromophore compound has the following structure (I):

[0104] Wherein, D is an atom or organic group that can provide electrons (i.e., an electron donor), A is an electron acceptor group, Z is an atom with at least two valences or an organic group with at least two chemical bonds, and L 1 and L 2 are independently selected from an atom having at least two valences or an organic group having at least two chemical bonds, 1 and π 2 are independently π bridges (or conjugated bridges), X 1 is the first cross-linkable group, X 2is a second crosslinkable group, p is an integer greater than or equal to 2, and q is an integer greater than or equal to 1. It can be understood that the maximum values ​​of p and q in the formula (I) can be determined based on the structure of D and L. 2 The maximum number of connectable groups in the structure is determined.

[0105] The D in the electron donor group can be a nitrogen atom, which has a strong electron donating ability and can enhance the electron donating ability of the electron donor group. In addition, the nitrogen atom can be connected to two -L 1 -X 1 It is understood that D in the electron donor group can also be other atoms or organic groups that can provide electrons (such as π electrons).

[0106] Z in the electron bridge group is a sulfur atom, an oxygen atom or an alkyl group. By introducing a sulfur atom, an oxygen atom or an alkyl group on the electron bridge group, the stability of the molecular structure of the chromophore compound can be improved, especially when Z is a sulfur atom or an oxygen atom, the stability of the chromophore compound is significantly improved. In some embodiments, the electron bridge group can be derived from an electron bridge molecule, and the electron bridge molecule can be one of high-performance electron bridges such as isophorone, thiophene bridge and pyrrole bridge. Specifically, the electron bridge group is derived from isophorone, and isophorone contains an alcoholic hydroxyl group, which is convenient for the introduction of the second cross-linkable group.

[0107] L 1 and L 2 They can be independently selected from olefins or isoolefins having 1 to 20 carbon atoms, aryl groups having 6 to 10 carbon atoms, heteroaryl groups having 5 to 10 carbon atoms, and combinations thereof.

[0108] The first crosslinkable group and the second crosslinkable group are both functional groups capable of undergoing click chemistry (e.g., cycloaddition reaction), thermal crosslinking reaction, photocrosslinking reaction, coupling reaction, or polymerization reaction, i.e., two chromophore compounds containing different first crosslinkable groups and second crosslinkable groups can react with each other to connect the two chromophore compound molecules together. Wherein, the first crosslinkable group and the second crosslinkable group are independently selected from anthracene, maleimide, acrylate, azide, alkynyl, hydroxyl, isocyanate, furan, thiol, olefin, coumarin, difluoroolefin, styrene, and derivatives of the foregoing groups. Specifically, the first crosslinkable group and the second crosslinkable group are independently selected from any one of the following structures:

[0109]

[0110] as well as

[0111] The following lists some typical cross-linking reaction examples using the above first cross-linkable group and the second cross-linkable group. For example, the group combination that can undergo click chemistry reaction includes the Husigen cycloaddition reaction of azide-alkyne group; the group combination that can undergo thermal cross-linking reaction includes: hydroxyl and isocyanate group, anthracene group and acrylate group, anthracene group and maleimide group, furan group and maleimide group; the group combination that can undergo photocross-linking reaction includes: thiol and olefin, coumarin and coumarin; coupling reaction between difluoroolefin group and difluoroolefin group and polymerization reaction between styrene group and styrene group, etc.

[0112] The first crosslinkable group and the second crosslinkable group in the same chromophore compound molecule may be the same or different. In some embodiments, the first crosslinkable group and the second crosslinkable group are the same, for example, the first crosslinkable group and the second crosslinkable group in the same chromophore compound molecule may be an anthracene group or a maleimide group at the same time. The first crosslinkable group and the second crosslinkable group in the same chromophore compound may be designed to be the same, so that the first crosslinkable group and the second crosslinkable group can be introduced simultaneously in a one-step reaction, the reaction process is easier to achieve, the reaction conditions are easy to control, and the synthesis steps can be simplified.

[0113] In some embodiments, p in formula (I) can be 2 or 3, etc., and q can be 1 or 2, etc. By limiting the values ​​of p and q in formula (I), that is, the first cross-linkable groups can be two or three, and the second cross-linkable groups can be one or two, the number of cross-linking sites in the chromophore compound can be significantly increased to further shorten the cross-linking time, thereby further reducing the electro-optic coefficient loss of the chromophore compound before and after cross-linking.

[0114] In some embodiments, the electron acceptor group can be derived from 2-(3-cyano-4-methyl-5-phenyl-5-(trifluoromethyl)furan-2(5H)-ethylidene)malononitrile, or 2-(3-cyano-4,5,5-trimethylfuran-2(5H)-ethylidene)malononitrile and other electron withdrawing groups. Specifically, the electron acceptor molecule used in this embodiment is 2-(3-cyano-4-methyl-5-phenyl-5-(trifluoromethyl)furan-2(5H)-ethylidene)malononitrile. It can be understood that the electron acceptor group can also be derived from other existing conventional electron acceptor molecules.

[0115] According to the different types of the first crosslinkable group and the second crosslinkable group connected in the chromophore compound, two types of chromophore compounds are synthesized in the embodiment of the present application, wherein the first crosslinkable group and the second crosslinkable group are the same. An anthracene group is connected to the electron donor group and the electron bridge group of one chromophore compound, and the chromophore compound has the structure of the following formula (II); a maleimide group is connected to the electron donor group and the electron bridge group of the other chromophore compound, and the chromophore compound has the structure of formula (III):

[0116]

[0117] In the above two chromophore compounds, the chromophore compound of formula (II) uses an anthracene group as the first crosslinkable group and the second crosslinkable group, and is named an anthracene-containing chromophore (abbreviated as FZL1); the chromophore compound of formula (III) uses a maleimide group as the first crosslinkable group and the second crosslinkable group, and is named a maleimide-containing chromophore (abbreviated as FZL2).

[0118] By introducing three anthracene groups and three maleimide groups into the chromophore compounds FZL1 and FZL2, respectively, a binary crosslinking system can be obtained, wherein the reaction of the three anthracene groups and the three maleimide groups can effectively reduce the crosslinking temperature and shorten the crosslinking time, which is beneficial to increase the glass transition temperature of the material, thereby improving the stability of the material, and at the same time, the electro-optic coefficient loss of the chromophore compound before and after crosslinking is minimized. Specifically, the crosslinking temperature of the above structure is reduced to below 120°C, the crosslinking time can be shortened to below 15 minutes, the Tg can reach above 178°C, and the electro-optic coefficient of the electro-optic material containing the above two chromophore compounds FZL1 and FZL2 can reach above 266pm / V.

[0119] In the above formula (I), at least two -L containing a first crosslinkable group are introduced into the electron donor. 1 -X 1The structure is characterized in that at least one second cross-linkable group is introduced on the electronic bridge, so that the chromophore compound has at least three cross-linking sites, and the distance between at least three cross-linking sites is relatively far, which reduces the degree of mutual interference during the cross-linking process, is conducive to the contact of cross-linking sites on different chromophore compounds, and increases the number of effective cross-linking sites, thereby enabling the chromophore compounds to cross-link at a lower temperature and in a shorter time, effectively improving the cross-linking efficiency of the chromophore compounds, reducing the influence of cross-linking curing on the electro-optic coefficient, and thus reducing the loss of the electro-optic coefficient of the chromophore compound before and after cross-linking. At the same time, cross-linking can further increase the glass transition temperature of the electro-optical material, reduce the risk of deorientation of polarized molecules during the cross-linking process, further improve the photothermal stability and polarization orientation stability of the electro-optical material, and is conducive to further reducing the loss of the electro-optic coefficient of the chromophore compound before and after cross-linking.

[0120] Moreover, the cross-linking process does not require the introduction of a separate cross-linking agent, which increases the content of chromophore compounds in the electro-optical material. The use of chromophore compounds FZL1 and FZL2 can form a pure chromophore electro-optical film of more than 95wt%, further improving the electro-optical coefficient of the electro-optical material.

[0121] In addition, the chromophore compound contains at least three cross-linkable groups at a relatively long distance, which can increase the distance between the molecules of the chromophore compound, weaken the electrostatic interaction between the molecules, and help improve the polarization efficiency of the chromophore compound.

[0122] Based on the same inventive concept, please refer to Figure 3 The present application also provides a method for preparing the chromophore compound (Formula I), which specifically includes the following steps.

[0123] Step S10, connecting an electron bridge molecule containing at least one second reactive group to an electron donor molecule containing at least two first reactive groups to obtain an electron donor group-electron bridge group compound containing the at least two first reactive groups and the at least one second reactive group.

[0124] Specifically, the structure of the electron donor molecule is Wherein, the specific structural types of D and L1 refer to the description of the above formula (I), R 3 is the first reactive group, and p is an integer greater than or equal to 2.

[0125] In some embodiments, D in the electron donor molecular structure is a nitrogen atom, which has a strong electron donating capacity, and the benzene ring further increases the electron donating capacity. In addition, the introduction of the benzene ring can increase the glass transition temperature of the chromophore compound.

[0126] In some embodiments, the first reactive group and the second reactive group are independently selected from any one of hydroxyl, azide, alkynyl, thiol, isocyanate and amino groups. In this embodiment, the first reactive group and the second reactive group are both hydroxyl groups.

[0127] Specifically, in the process of obtaining the electron donor group-electron bridge group compound by implementing step S10, before connecting the electron bridge molecule to the electron donor molecule, it is also necessary to connect the first protective group to each first reactive group. After connecting the electron bridge molecule to the electron donor molecule, it is also necessary to connect the second protective group to each second reactive group. Since the reactivity of the first reactive group and the second reactive group is large, by generating the first protective group and the second protective group on the first reactive group of the electron donor molecule and the second reactive group of the electron bridge molecule, respectively, and removing the first protective group and the second protective group after the corresponding reaction is completed, the first reactive group and the second reactive group can be protected from being affected during the reaction.

[0128] In some embodiments, the first protecting group and the second protecting group are respectively derived from any one of tert-butyldimethylsilyl chloride and its derivatives, tert-butyldiphenylsilyl chloride and its derivatives, and dihydropyran derivatives, etc. It is understandable that other groups capable of protecting the first reactive group and the second reactive group may also be used.

[0129] Step S20, connecting at least one first crosslinkable group and at least one second crosslinkable group to the first reactive group and the second reactive group of the electron donor group-electron bridging group compound, respectively, and connecting an electron acceptor group to the electron bridging group of the electron donor group-electron bridging group compound, thereby obtaining a chromophore compound as shown in the aforementioned formula (I).

[0130] In some embodiments, before introducing the first crosslinkable group and the second crosslinkable group into the electron donor group-electron bridge group compound, the first protecting group and the second protecting group need to be removed. In this embodiment, since the first reactive group and the second reactive group are both hydroxyl groups, and the introduced first crosslinkable group and the second crosslinkable group are the same, the first protecting group and the second group can have the same structure and can be removed at the same time, which simplifies the reaction steps.

[0131] The electron donor molecule of the embodiment of the present application contains at least two first reactive groups, which can provide active connection sites, and is convenient for introducing two first cross-linkable groups. In addition, the electron bridge molecule contains a second reactive group, which is convenient for introducing the second cross-linkable group. There is no need to add the step of introducing active connection sites on the electron donor molecule and the electron bridge molecule, making the synthesis of the chromophore compound easier. Therefore, the preparation method is easy to implement, the reaction conditions are mild, the yield of the intermediate product and the final product is high, and the chromophore compound can be dissolved in most organic solvents, which is conducive to large-scale production and commercial application.

[0132] The specific synthesis methods of the chromophore compound (FZL1) of the aforementioned formula (II) and the chromophore compound (FZL2) of the formula (III) are given below, wherein the electron donor molecule is a molecule having a structure of The first compound, the electron bridge molecule is isophorone, and the electron acceptor molecule is 2-(3-cyano-4-methyl-5-phenyl-5-(trifluoromethyl)furan-2(5H)-ethylidene)malononitrile or other conventional acceptor molecules.

[0133] The specific preparation method of the chromophore compounds (FZL1 and FZL2) comprises the following steps:

[0134] Step S1, generating a tert-butyldimethylsilyl group on the alcoholic hydroxyl group of the first compound to obtain a structure of First, the alcoholic hydroxyl group of the first compound is protected by connecting a protective group to prevent the subsequent reaction from destroying the alcoholic hydroxyl group.

[0135] Step S2, subjecting the second compound to a knoevenagel condensation reaction with isophorone in sodium ethoxide and 2-mercaptoethanol to obtain a compound having a structure of The third compound.

[0136] A tert-butyldimethylsilyl group is generated on the alcoholic hydroxyl group of the third compound to obtain a structure of Since the introduced electron bridge molecule also contains alcoholic hydroxyl groups, it also needs to be protected.

[0137] Step S3, the fourth compound reacts with diethyl phosphate through Wittig-Hornor reaction to obtain a structure of The fifth compound.

[0138] Step S4, reducing the nitrile group in the fifth compound by diisobutylaluminum hydride to obtain a structure of The sixth compound.

[0139] Step S5, the sixth compound is subjected to acid hydrolysis to remove the tert-butyldimethylsilyl group to obtain a structure of Seventh compound. Since the keto group of the electron bridge molecule is chain extended after the reaction of step S4 and step S5, the first crosslinkable group and the second crosslinkable group need to be connected subsequently, therefore, the protective group connecting the alcoholic hydroxyl group on the electron donor group and the electron bridge group needs to be removed to reduce the alcoholic hydroxyl group.

[0140] Step S6, reacting the seventh compound with R 4 OH undergoes nucleophilic substitution reaction or Steglich esterification reaction to obtain the structure The eighth compound, wherein R 4 Specifically

[0141] Step S7, the eighth compound is condensed with the electron acceptor molecule to obtain the chromophore compound (FZL1) of the aforementioned formula (II) or the chromophore compound (FZL2) of the aforementioned formula (III).

[0142] The above-mentioned synthesis method avoids the alcoholic hydroxyl groups from being affected before the first crosslinkable group and the second crosslinkable group are introduced by introducing an electron donor structure containing two alcoholic hydroxyl groups and an electron bridge structure containing one alcoholic hydroxyl group, and by connecting and removing protective groups on the three alcoholic hydroxyl groups; the first crosslinkable group and the second crosslinkable group introduced are the same, the reaction conditions are easy to control, the reaction is easier to occur, and the synthesis steps are simplified. Therefore, the preparation method is easy to implement, the reaction conditions are mild, the yield of the intermediate product and the final product is high, and the chromophore compound can be dissolved in most organic solvents, which is conducive to large-scale production and commercial application.

[0143] An embodiment of the present application further provides an electro-optical material, which includes at least two chromophore compounds as described above, and the at least two chromophore compounds are used for cross-linking reaction.

[0144] In some embodiments, the electro-optical material comprises two chromophore compounds, and the first crosslinkable group and the second crosslinkable group in each chromophore compound are the same, and the two chromophore compounds can undergo a crosslinking reaction to form a crosslinked macromolecule. It is understandable that when the first crosslinkable group (or the second crosslinkable group) introduced in one chromophore compound is different from the first crosslinkable group (or the second crosslinkable group) introduced in another chromophore compound, the composed electro-optical material is a binary chromophore system.

[0145] In some embodiments, the electro-optical material includes two chromophore compounds, thereby forming a binary cross-linked chromophore system. When the first cross-linkable group and the second cross-linkable group on any chromophore compound are the same, the first cross-linkable group on one chromophore compound and the first cross-linkable group on the other chromophore compound are selected from any one of the following group combinations: anthracene group and maleimide group, azide group and alkyne group, hydroxyl group and isocyanate group, anthracene group and acrylate group, furan group and maleimide group, thiol group and olefin, coumarin group and coumarin group, difluoroolefin group and difluoroolefin group, and styrene group and styrene group.

[0146] In some embodiments, the first cross-linkable group and the second cross-linkable group connected to one chromophore compound are both anthracene groups, and the first cross-linkable group and the second cross-linkable group connected to another chromophore compound are both maleimide groups, that is, in this embodiment, the electro-optical material is a binary cross-linked chromophore system. Specifically, the two chromophore compounds are chromophore compound FZL1 and chromophore compound FZL2, and their structures are as described above. Chromophore compound FZL1 and chromophore compound FZL2 can undergo a cross-linking reaction to generate a cross-linked structure, and the combination Figure 2 As shown, in the polarization process of the binary cross-linked chromophore system composed of chromophore compounds FZL1 and FZL2, FZL1 and FZL2 can undergo a cross-linking reaction to form a cross-linked structure. After the cross-linked structure is formed, the glass transition temperature of the electro-optical material further increases and is higher than the cross-linking temperature. During the continuous cross-linking process, even if the cross-linking time is extended or the temperature is appropriately increased, the polarized molecules will not relax, thereby improving the photothermal stability and polarization orientation stability of the electro-optical material, reducing the attenuation of the electro-optic coefficient of the chromophore molecules before and after cross-linking, and making the cross-linked electro-optical material have a higher electro-optic coefficient.

[0147] In some embodiments, in the aforementioned binary cross-linked chromophore system, the chromophore compound FZL1 and the chromophore compound FZL2 have the same number of cross-linked groups and can be mixed in a ratio of 1:1.

[0148] The electro-optic material composed of the above-mentioned chromophore compounds can effectively reduce the cross-linking temperature between the chromophore compounds and shorten the cross-linking time, while increasing the glass transition temperature of the electro-optic material, thereby improving the photothermal stability and polarization orientation stability of the electro-optic material, reducing the loss of the electro-optic coefficient before and after the cross-linking of the chromophore compounds, and thereby increasing the electro-optic coefficient of the electro-optic material. For example, the electro-optic material using the chromophore compound FZL1 and the chromophore compound FZL2 can reduce the cross-linking temperature to below 120°C, shorten the cross-linking time to below 15 minutes, and achieve a Tg of above 178°C after cross-linking, and an electro-optic coefficient of above 266 pm / V, with minimal loss of the electro-optic coefficient.

[0149] See also Figure 4 The embodiment of the present application further provides an electro-optic film 100, wherein the electro-optic film 100 is made of any of the above electro-optic materials. Since the chromophore compound is soluble in an organic solvent, the electro-optic material has good film-forming properties.

[0150] See also Figure 5 The embodiment of the present application further provides an electro-optic glass 200, which includes a glass substrate 210 and the electro-optic film 100 located on the surface of the glass substrate 210. The glass substrate 210 may be indium oxide (ITO) glass.

[0151] The specific preparation method of the electro-optic glass is as follows: the aforementioned electro-optic material is dissolved in an organic solvent (e.g., dibromomethane), after filtering through a 0.2 mm PTFE filter, the filtered solution is spin-coated on the surface of an indium oxide (ITO) glass substrate, and heated overnight under a vacuum condition at 50° C. to remove the solvent, thereby obtaining an electro-optic film 100 attached to the glass substrate 210. It is understandable that the electro-optic material solution can also be coated on the glass substrate 210 by spraying or other coating methods.

[0152] See also Figure 6 The embodiment of the present application further provides an electro-optical device 300 , which includes a housing 310 and the above-mentioned film 100 or the above-mentioned electro-optical glass 200 located on the housing 310 .

[0153] The electro-optical device 300 can be an optoelectronic modulator, such as a Mach-Zehnder Modulator (MZM), an optoelectronic modulator microring, a spatial light modulator, etc., to realize the modulated wireless transmission function of the electro-optical signal, as well as other electro-optical modulator scenarios using organic electro-optical materials, including wireless high-speed interconnection between data centers, unmanned driving, Industry 4.0, etc.

[0154] The electro-optic film 100 provided in the present application has a relatively high electro-optic coefficient (at least 266 pm / V), which is beneficial to improving the performance of the electro-optic device 300; in addition, since the polarized electro-optic film 100 has a cross-linked network structure, the glass transition temperature of the electro-optic film 100 is increased (at least 178°C), thereby increasing the operating temperature of the electro-optic device 300.

[0155] See also Figure 7 The embodiment of the present application further provides an electronic device 400 , which includes a housing 410 and the electro-optical device 300 as described above located on the housing 410 .

[0156] The embodiments of the present application are further described below through specific examples.

[0157] Synthesis example 1

[0158] An organic optical nonlinear chromophore compound FZL1 based on a single donor structure, wherein the chromophore compound FZL1 has the structure of the above formula (II).

[0159] The chromophore compound FZL1 exhibits good solubility in common organic solvents (such as trichloroethane, etc.), and its synthesis method comprises the following steps:

[0160] S11: Synthesis of compound 2

[0161] In a double-necked round-bottom flask, imidazole (4.09 g, 60 mmol) and tert-butyldimethylsilyl chloride (9.04 g, 60 mmol) were placed, then vacuumed and backfilled with argon, repeated three times. After that, N, N-dimethylformamide was slowly injected into the flask to dissolve 4-[N, N-bis(2-hydroxyethyl)amino]benzaldehyde (5 g, 24 mmol). After reacting at room temperature for 3 hours, 100 ml of water was poured into the reaction mixture, and then the product was extracted three times with ethyl acetate, and finally MgSO4 was added to remove excess water. The solvent was removed in vacuo, and the crude product (acetone: hexane = 1: 15 to 1: 10) was flash chromatographed on SiO2 to obtain oily compound 2 (10.1 g, 23.1 mmol) with a yield of 96%.

[0162] Product characterization:

[0163] MS (MALDI) (M+, C 23 H 43 NO3Si2):calcd:437.27; found:437.30.

[0164] 1H NMR (600MHz, CDCl3) δ9.70 (s, 1H), 7.69 (d, J = 8.8Hz, 2H), 6.74 (d, J = 8.9Hz, 2 H), 3.80 (t, J = 6.1Hz, 4H), 3.62 (t, J = 6.1Hz, 4H), 0.87 (s, 18H), 0.02 (s, 12H).

[0165] S12: Synthesis of compound 3

[0166] Under ice bath conditions, sodium metal (0.64 g, 27.72 mmol) was slowly dissolved in 30 mL of ethanol. The above reaction took place in a 500 mL two-necked flask filled with argon. Then 2-mercaptoethanol (2.17 g, 27.72 mmol) was added to the above solution. After reacting at room temperature for 20 minutes, compound 2 (10.1 g, 23.1 mmol) was added. A magnetic stirrer was used to stir for 1 h at room temperature. The reaction was heated to reflux overnight at 65 ° C, MgSO4 was added to the mixture to remove water, and the solvent was stripped by a rotary evaporator. The crude product was ethyl acetate and n-hexane (1: 10 to 1: 4) as eluents, and compound 3 (11.8 g, 18.6 mmol) was obtained by column chromatography with a yield of 81%.

[0167] Product characterization:

[0168] MS (MALDI) (M+, C 34 H 59 NO4SSi2):calcd:633.37; found:633.40.

[0169] 1 H NMR(600MHz, CDCl3) δ7.89(d,J=16.0Hz,1H),7.44(d,J=7.6Hz,2H),7.02(d,J=16.0Hz, 1H),6.69(d,J=7.6Hz,2H),4.15–4.11(m,2H),4.09(td,J=6.8,1.5Hz,2H),3.79(t,J=5 .8Hz,4H),3.57(t,J=5.8Hz,4H),3.47(s,1H),3.00(td,J=6.5,1.6Hz,2H),2.95(ddd,J =15.0,6.9,1.8Hz,2H),1.10(d,J=1.2Hz,6H),0.93–0.92(m,18H),0.14–0.07(m,12H).

[0170] S13: Synthesis of compound 4

[0171] In a 500mL round-bottomed flask, imidazole (1.52g, 22.3mmol) and tert-butyldimethylsilyl chloride (3.36g, 22.2mmol) were combined and then added to 30MLN, compound 3 (11.8g, 18.6mmol) dissolved in N-dimethylformamide. The solution was stirred at room temperature for 3 hours under an argon atmosphere, then 100mL of water was poured in, the solution was filtered to remove water and MgSO4, and the solvent was removed by a rotary evaporator. After vacuum removal of the solvent, the crude product was purified by silica gel chromatography, and eluted with ethyl acetate / n-hexane (1:15~1:10) to obtain compound 4 (12.36g, 16.5mmol), and the yield was 89%.

[0172] Product characterization:

[0173] MS (MALDI) (M+, C 40 H 73 NO4Si3):calcd:747.45; found:748.30.

[0174] 1 H NMR (600MHz, CDCl3) δ7.91(d,J=16.2Hz,1H),7.45(d,J=8.9Hz,2H),7.00(d,J=16.2Hz,1H),6.69(d,J=8.9Hz,2H),4.13(q,J=7.1Hz,2H),3.83–3. 76(m,4H),3.71(t,J=7.1Hz,2H),3.58(t,J=6.3Hz,4H),2.89(t,J=7.1Hz ,2H),2.62(s,2H),1.09(s,6H),0.95–0.90(m,27H),0.12–0.10(m,18H).

[0175] 13 C NMR (151MHz, CDCl3) δ195.89,157.88,149.07,137.21,129.43,128.08,124.10,123.48,111.62,62.90,60.26,5 3.49,51.97,51.83,41.30,36.47,32.29,28.39,28.11,25.92,25.90,25.66,18.27,17.99,-3.58,-5.23,-5.35.

[0176] S14: Synthesis of compound 5

[0177] Compound 4 (12.36 g, 16.5 mmol), diethyl cyanomethylphosphonate (11.69 g, 66 mmol) and sodium hydride (1.58 g, 66 mmol) were added to 40 mL of tetrahydrofuran in a flask, and the above reaction was carried out under argon protection and ice bath conditions. After the solution was clarified, the reactants were heated to reflux overnight at 65 ° C. After the tetrahydrofuran was removed in vacuo, it was directly purified by silica gel elution column chromatography with ethyl acetate / n-hexane (1:15-1:10) to obtain red compound 5 (8.91 g, 11.55 mmol) with a yield of 70%.

[0178] Product characterization:

[0179] MS (MALDI) (M+, C 42 H 75 NO4SSi3):calcd:773.47; found:773.50.

[0180] 1 H NMR (600MHz, CDCl3) δ10.16(d,J=8.1Hz,1H),7.97(d,J=16.2Hz,1H),7.42(d,J=8.8Hz,2H ),7.02(d,J=8.1Hz,1H),6.87(d,J=16.2Hz,1H),6.69(d,J=8.9Hz,2H),3.79(t,J=6.3Hz,4 H),3.71(t,J=7.2Hz,2H),3.57(t,J=6.3Hz,4H),2.76(s,2H),2.72(t,J=7.2Hz,2H),2.52( s,2H),1.06(s,6H),0.91(d,J=4.6Hz,18H),0.88(s,9H),0.05(s,12H),0.04–0.02(m,6H).

[0181] 13 C NMR (151MHz, CDCl3) δ191.60,156.66,150.11,148.64,134.74,128.96,128.29,126.92,124.74,111.6 5,62.61,60.28,53.52,41.68,39.93,37.52,30.07,28.34,25.91,18.33,18.28,14.21,-5.25,-5.34.

[0182] S15: Synthesis of compound 6

[0183] Under argon protection, diisobutylaluminum hydride solution (2.74mL, 23.1mmol) was slowly added to 80.0mL of fresh dry toluene solution of compound 5 (8.91g, 11.55mmol), which had been precooled in a low-temperature reactor at -78°C for 2 hours, then 10g of wet silica gel and 15.0mL of water were added, and the reaction was continued at 0°C for 2 hours. Water was poured into the reaction product and the crude product was extracted with ethyl acetate. The crude product was purified by vacuum concentration and silica gel chromatography, and eluted with ethyl acetate / n-hexane (1:15-1:10) solution. Finally, red solid compound 6 (6.27g, 8.1mmol) was obtained with a yield of 70.1%.

[0184] Product characterization:

[0185] MS (MALDI) (M+, C 24 H 33 NO4S):calcd:431.21; found:431.40.

[0186] 1 H NMR (600MHz, CDCl3) δ10.15 (d, J=8.0Hz, 1H), 7.46 (dd, J=8.9, 2.2Hz, 2H), 7.0 1(d,J=8.0Hz,1H),6.91(d,J=16.1Hz,1H),6.72(t,J=8.9Hz,2H),6.55(dd,J=1 5.7,7.9Hz,1H),3.92(dt,J=9.6,4.9Hz,4H),3.68(dt,J=17.9,4.7Hz,6H),3.5 5(s,1H),3.37(s,2H),2.78(dd,J=10.5,4.4Hz,2H),2.54(s,4H),1.06(s,6H).

[0187] 13 C NMR (151MHz, CDCl3) δ193.88,153.61,135.04,128.92,127.83,126.86,124. 22,122.49,112.36,61.18,60.72,60.56,41.74,39.91,38.18,30.12,28.31.

[0188] S16: Synthesis of compound 7

[0189] In the flask containing compound 6 (6.27g, 8.1mmol) and 50mL acetone, 30mL HCl with a concentration of 1M was added. After stirring at room temperature for 3 hours, it was neutralized with sodium bicarbonate and concentrated in vacuo using a vacuum drying oven. 50mL water was poured into the concentrated solution and extracted three times with 100mL dichloromethane. The resulting product was concentrated in vacuo and dehydrated with MgSO4. The crude product was purified by silica gel column chromatography and gradient eluted with dichloromethane / ethyl acetate (10: 1~1: 1) to obtain red solid compound 7.

[0190] Product characterization:

[0191] MS (MALDI) (M+C 75 H 69 NO7S):calcd:1127.47; found:1127.50.

[0192] 1 H NMR (600MHz, CDCl3) δ10.20(dd,J=19.0,8.0Hz,1H),8.36(dt,J=25.2,8.8Hz,2H),8.22(dd,J=16.2,8.6Hz,4H),7.97(ddt,J=20.4,13.6,11. 6Hz,5H),7.73(d,J=8.2Hz,1H),7.64–7.50(m,5H),7.50–7.35(m,7H),7.30–7.18(m,6H),7.03(dd,J=22.0,8.0Hz,1H),6.87(ddd,J=16.8,12 .5,7.6Hz,1H),6.73(ddd,J=19.8,8.8,4.9Hz,1H),6.63(ddd,J=16.8,14.4,7.7Hz,1H),6.59–6.53(m,1H),4.26–4.06(m,4H),3.98–3.86(m, 4H), 3.41(dddd,J=22.4,17.6,13.8,7.5Hz,4H),2.88–2.71(m,7H),2.64–2.46(m,2H),2.33–2.22(m,2H),2.08(s,4H),1.08(d,J=7.2Hz,6H).

[0193] 13C NMR (151MHz, CDCl3) δ191.58,172.90,171.18,156.19,139.51,139.39,136.14,134.86,133.76,133.0 4,132.35,132.14,131.58,129.49,129.38,129.28,129.03,127.98,127.12,126.51,126.31,126.03, 125.37,125.20,124.98,123.85,111.97,63.02,61.38,60.44,49.08,46.28,41.73,39.90,35.17,34.06,33.33,32.25,31.99,30.82,30.13,29.75,28.37,26.96,23.69,23.31,23.18,22.79,21.10,14.26.

[0194] S17: Synthesis of compound 8a

[0195] 3-(Anthracene-9-yl)propionic acid (1.30 g, 5.22 mmol), 4-dimethylaminopyridine (0.063 g, 0.52 mmol), 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (1.00 g, 5.22 mmol) were added to 20 mL of dichloromethane in a 100 mL two-necked flask filled with argon. After reacting at 0°C for 1 hour, the solution gradually became clear, and then compound 7 (0.50 g, 1.16 mmol) dissolved in 10 mL of dichloromethane was added, and then the above reaction was continued at 0°C for 2 hours. The flask was then removed from the ice bath, and the mixture was refluxed at 65°C overnight. 100 ml of water was poured into the reaction mixture, and the product was extracted three times with ethyl acetate, and finally MgSO4 was added to remove excess water. The solvent was removed in vacuo and the crude product was flash chromatographed on SiO2 (acetone:hexane=1:8 to 1:1) to give compound 8a (0.79 g, 0.70 mmol) as a red oil in 60% yield.

[0196] Product characterization:

[0197] MS (MALDI) (M+, C 75 H 69 NO7S):calcd:1128.44; found:1128.55.

[0198] 1H NMR(600MHz, CDCl3)δ10.02(d,J=8.0Hz,1H),7.79(d,J=16.1Hz,1H),7.27–7.18(m,21H),7.18–7.15 (m,6H),7.15–7.11(m,5H),7.09(d,J=2.1Hz,5H),6.89(d,J=7.9Hz,1H),6.66(d,J=2.0Hz,1H),6.62( d,J=6.1Hz,3H),6.58(d,J=8.0Hz,2H),4.82(d,J=21.8Hz,12H),4.29(dd,J=36.3,30.7Hz,5H),4.20( t,J=6.2Hz,2H),3.59(d,J=5.3Hz,4H),2.77(t,J=6.1Hz,2H),2.57(s,2H),2.23(s,2H),0.88(s,6H).

[0199] 13 C NMR (151MHz, CDCl3) δ191.59,171.18,166.19,165.92,159.88,159.83,156.14,150.9 7,148.18,136.54,136.52,134.83,131.97,131.68,129.16,128.70,128.68,128.18, 128.16,127.71,127.64,127.62,127.60,127.11,125.83,125.20,112.26,108.58,108.43,107.62,107.37,70.26,63.63,62.19,60.46,49.49,30.09,28.42,21.13,14.32.

[0200] S18: Synthesis of the chromophore FZL1

[0201] Compound 8a (0.79 g, 0.70 mmol) and 2-(dicyanomethylene)-4-methyl-5-phenyl-5-(trifluoromethyl)-2,5-dihydrofuran-3-carbonitrile (0.27 g, 0.84 mmol) were added to a two-necked flask filled with anhydrous ethanol (10 mL) filled with argon. After reacting at 65° C. for 6 hours, the solution was concentrated using a rotary evaporator. The crude product was flash chromatographed on SiO2 (acetone: hexane = 1: 8 to 1: 1) to obtain a green solid chromophore FZL1 with a yield of 80% (0.80 g, 0.56 mmol).

[0202] Product characterization:

[0203] HRMS(ESI)([M+H]+,C 103 H 58 F 33 N4O 13 S):calcd:2217.3194;found:2317.3190。

[0204] 1 H NMR(600MHz,CDCl3)δ8.02(s,1H,ArH),7.93(d,J=15.9Hz,1H,ArH),7.54(ddd,J=17.4,15.5,7.6Hz,5H,ArH),7.44(d,J=12.3Hz,1H,ArH),7.37(d,J=8.8Hz,2H,ArH),7.28(s,1H,ArH),7.27(d,J=2.3Hz,2H,ArH),7.25(d,J=2.3Hz,3H,CH),6.86(t,J=17.2Hz,1H,CH),6.82–6.69(m,5H,ArH),6.51(d,J=14.6Hz,1H,CH),5.06(d,J=18.6Hz,12H,OCH2),4.54(t,J=5.9Hz,4H,OCH2),4.36(t,J=6.2Hz,2H,OCH2),3.88(t,J=5.8Hz,4H,NCH2),2.94(t,J=6.4Hz,2H,SCH2),1.64(d,J=11.5Hz,4H,CH2),0.99(s,3H,CH3),0.90(s,3H,CH3)。

[0205] 13 C NMR(151MHz,CDCl3)δ175.49,171.19,165.78,165.44,163.00,159.19,159.17,153.86,146.70,145.08,145.06,141.56,141.46,139.91,139.81,139.25,132.04,131.77,131.40,129.89,129.71,129.67,129.52,128.38,126.78,125.65,125.02,123.00,121.10,117.43,112.18,110.57,108.84,108.60,107.69,107.50,107.40,70.98,62.09,60.41,57.80,49.30,41.60,41.01,33.99,30.29,29.71,28.53,27.74,21.05。

[0206] Synthesis example 2

[0207] Another organic optical nonlinear chromophore compound FZL2 based on a single donor structure has the structure of the above formula (III).

[0208] The chromophore compound FZL1 exhibits good solubility in common organic solvents (such as trichloroethane, etc.), and its synthesis method comprises the following steps:

[0209] For steps S21 to S26, please refer to steps S11 to S16 in embodiment 1.

[0210] S27: Synthesis of compound 8b

[0211] According to the reaction process of the aforementioned compound 8a, compound 7 and 3-pyrrolidine-1-propionic acid were used as reactants to obtain a red oily compound 8b (0.72 g, 0.81 mmol) with a yield of 70%.

[0212] Product characterization:

[0213] MS (MALDI) (M+, C 45 H 48 N4O 13 S):calcd:884.95;found:884.86.

[0214] 1 H NMR (600MHz, CDCl3) δ10.13(d,J=8.0Hz,1H,CHO),7.92(d,J=16.2Hz,1H,CH),7.41(d,J=8.7Hz,2H,ArH),6.94(d,J=8.0Hz ,1H),6.86(d,J=16.2Hz,1H,CH),6.74(d,J=8.8Hz,2H,ArH),6.68(d,J=11.8Hz,6H,CH),4.25(t,J=6.2Hz,4H,NCH2),4.10( t,J=7.1Hz,2H,NCH2),3.80(t,J=6.7Hz,4H,NCH2),3.75(t,J=7.0Hz,2H,OCH2),3.65(t,J=6.1Hz,4H,OCH2),2.78(t,J=6.5 Hz,2H,SCH2),2.63(t,J=7.0Hz,4H,CH2),2.59(t,J=7.0Hz,2H,CH2),2.51(s,2H,CH2),2.03(s,2H,CH2),1.04(s,6H,CH3).

[0215] 13C NMR (151MHz, CDCl3) δ191.57,170.65,170.44,170.38,156.20,150.79,147.90,134.78,134.22,129.05,127.60,127.0 2,125.77,125.21,112.11,63.09,61.63,60.38,49.41,41.65,39.82,33.55,33.20,32.90,30.08,28.30,21.04,14.19.

[0216] S28: Synthesis of the chromophore FZL2

[0217] Compound 8b (0.72 g, 0.81 mmol) and 2-(dicyanomethylene)-4-methyl-5-phenyl-5-(trifluoromethyl)-2,5-dihydrofuran-3-carbonitrile were placed in a flask as raw materials, and the chromophore FZL2 (0.70 g, 0.59 mmol) was prepared by referring to the reaction process of the chromophore FZL1 in the aforementioned step S18 to obtain a green solid product with a yield of 73%.

[0218] Product characterization:

[0219] HRMS (ESI) ([M+H]+, C 61 H 55 F3N7O 13 S):calcd:1182.3531; found:1182.3539.

[0220] 1 H NMR (600MHz,CDCl3) 1H NMR(600MHz, CDCl3)δ7.98(d,J=16.0Hz,2H,CH),7.59–7.52(m,5H,ArH,CH),7.48–7.41(m,3H,CH),6.99(d,J=16.0Hz,1H,CH ),6.78(d,J=9.0Hz,2H,ArH),6.71(d,J=7.9Hz,6H,CH),6.56(d,J=14.6Hz,1H,CH),4.28(t,J=6.2Hz,4H),4.16–4.10(m,2H,N CH2),3.83(t,J=7.0Hz,4H,NCH2),3.77(t,J=7.1Hz,2H,NCH2),3.70(t,J=6.2Hz,4H,OCH2),2.80(t,J=6.5Hz,2H,OCH2),2.65 (t,J=7.0Hz,4H,OCH2),2.60(t,J=6.6Hz,2H,SCH2),2.06(s,2H,CH2),1.66(s,2H,SCH2),1.01(s,3H,CH3),0.91(s,3H,CH3).

[0221] 13 C NMR(151MHz, CDCl3)δ175.49(s),170.64(s),170.34(d,J=7.5Hz),163.01(s),156.88(s),153.76(s),148.60(s),147.21(s) ,137.31(s),134.24(s),131.42(s),130.06–129.66(m),129.56(s),128.40(d,J=17.4Hz),126.82(s),125.73(s),125.22(s) ,117.55(s),112.23(s),111.25(s),111.06(s),110.60(s),77.26(s),77.05(s),76.84(s),63.02(s),61.54(s),58.54(s),4 9.44(s), 41.76(s), 41.09(s), 34.00(s), 33.53(d,J=9.4Hz), 32.87(d,J=15.6Hz), 30.39(s), 29.71(s), 28.59(s), 27.84(s).

[0222] Combined with the specific compound structural formula, the synthesis process of the chromophore compound FZL1 and the chromophore compound FZL2 is given below:

[0223]

[0224] Example 1

[0225] 100 wt % of FZL1 obtained in Synthesis Example 1 is dissolved in an organic solvent (such as trichloroethane, etc.) to obtain a FZL1 solution, and then the FZL1 solution is formed into a film to obtain a FZL1 electro-optical film (named FZL1).

[0226] 100 wt % of FZL2 obtained in Synthesis Example 2 is dissolved in an organic solvent (such as trichloroethane) to obtain a FZL2 solution, and then the FZL2 solution is formed into a film to obtain a FZL2 electro-optical film (named FZL2).

[0227] The chromophore compound FZL1 obtained in Synthesis Example 1 and the chromophore compound FZL2 obtained in Synthesis Example 2 are mixed in a molar ratio of 1:1 and dissolved in an organic solvent (such as trichloroethane, etc.) to obtain a FZL1+FZL2 mixed solution, and then the FZL1 and FZL2 mixed solution is formed into a film to obtain an electro-optical film of uncrosslinked FZL1+FZL2 (named 1:1FZL1:FZL2(NC)).

[0228] The uncrosslinked FZL1+FZL2 electro-optical film was crosslinked at about 120° C. for about 15 min to obtain a crosslinked FZL1+FZL2 electro-optical film (named 1:1FZL1:FZL2 (X-link)).

[0229] Comparative Example 1

[0230] The structure is:

[0231]

[0232] Among them, one cross-linkable group (anthracene group) is connected to the electron donor and the electron bridge in HLD1, and two cross-linkable groups (acrylate groups) are connected to the electron donor and the electron bridge in HLD2.

[0233] According to the method of Example 1, HLD1 was prepared into an HLD1 electro-optical film (named as HLD1).

[0234] HLD2 was prepared into an HLD2 electro-optical film (named as HLD2).

[0235] HLD1 and HLD2 were mixed in a molar ratio of 2:1 to prepare an electro-optical film of uncrosslinked HLD1+HLD2 (named HLD1:HLD2(RT)).

[0236] The uncrosslinked electro-optical film of HLD1+HLD2 was crosslinked at about 150°C for about 30 minutes to obtain a crosslinked electro-optical film of HLD1+HLD2 (named HLD1:HLD2(150°C)).

[0237] The thickness of the electro-optical film obtained in the above Example 1 and Comparative Example 1 remains consistent.

[0238] Device Embodiment

[0239] After the electro-optical thin films obtained in Example 1 and Comparative Example 1 were assembled into electro-optical devices, the electro-optical coefficient (r 33 ).

[0240] The electro-optical films of Example 1 and Comparative Example 1 were assembled into electro-optical devices, and the contact polarization process was carried out above the glass transition temperature (Tg) of the electro-optical material, specifically at a temperature of 5 to 10°C. The electro-optic coefficient (r 33 ), this method uses thin ITO glass with low reflectivity and good transparency as electrodes to minimize multiple reflections.

[0241] The above Example 1 and Comparative Example 1 are characterized and described below.

[0242] like Fig. 8A and Figure 8B Shown are differential scanning calorimeter (DSC) curves of the chromophore compounds FZL1 and FZL2 of Example 1, and FZL1+FZL2 before and after cross-linking.

[0243] like Fig. 9 Shown are the UV-visible absorption spectra of the chromophore compound FZL1 of Example 1 and the chromophore compound HLD1 of Comparative Example 1.

[0244] Table 1

[0245]

[0246] from Fig. 8A It can be seen from Table 1 that the glass transition temperatures (Tg) of FZL1 and FZL2 are 68°C and 70°C, respectively. Figure 8BIt can be seen from Table 1 that the glass transition temperature (Tg) of the uncrosslinked FZL1+FZL2 film (expressed as: 1:1FZL1:FZL2(NC)) mixed at a molar ratio of 1:1 is 110°C. During the heating process, the anthracene group of FZL1 and the maleimide group of FZL2 undergo a crosslinking reaction, and the small molecules become large crosslinked polymers. The glass transition temperature (Tg) of the crosslinked FZL1+FZL2 film (expressed as: 1:1FZL1:FZL2(X-link)) mixed at a molar ratio of 1:1 is increased to 178°C. Therefore, the glass transition temperature (Tg) of the crosslinked electro-optical material is significantly improved. During the continuous crosslinking process, due to the high glass transition temperature, the polarization-oriented molecules will not have de-orientation problems, thereby improving the photothermal stability and polarization orientation stability of the electro-optical material and reducing the loss of the electro-optic coefficient. Therefore, the glass transition temperature of the chromophore compound FZL1 in the embodiment of the present application after cross-linking is increased by 110°C compared with the glass transition temperature before cross-linking. After cross-linking, the glass transition temperature of 1:1FZL1:FZL2 (X-link) reaches 178°C, which is higher than the glass transition temperature (174°C) of HLD1 in comparative example 1 after cross-linking.

[0247] Combination Fig. 9 As can be seen from Table 1, the maximum absorption wavelength of the chromophore compound FZL1 in chloroform is 717 nm, which is not significantly changed compared with HLD1 in Comparative Example 1 (the maximum absorption wavelength in chloroform is 749 nm), indicating that when two -L 1 -X 1 The structure has little effect on the electron donating ability of aniline electron donor.

[0248] In addition, by detecting the disappearance of the absorption peak of the cross-linking group (anthracene group) in the spectrum, the time required for the end of cross-linking can be determined, so as to facilitate the regulation of the cross-linking temperature and cross-linking time of the chromophore compound.

[0249] like Fig.10 Shown are the UV-visible absorption spectra of the chromophore compounds HLD1 and HLD2 of Comparative Example 1 before and after cross-linking.

[0250] like Fig.11 Shown are the UV-visible absorption spectra of the chromophore compounds FZL1 and FZL2 of Example 1 before and after cross-linking.

[0251] The spectral absorption parameters and corresponding glass transition temperature data of the chromophore compound FZL1 of Example 1 and the chromophore compound HLD1 of Comparative Example 1 are shown in Table 1.

[0252] The relevant test data of the chromophore compounds of Example 1 and Comparative Example 1 are shown in Table 2.

[0253] Table 2

[0254]

[0255] from Fig.10 It can be seen from Table 2 that the electro-optic coefficient of the chromophore compounds HLD1 and HLD2 of Comparative Example 1 before cross-linking is 460pm / V under the cross-linking conditions (150°C, 30min), and the electro-optic coefficient after cross-linking is 290pm / V, which is a serious decrease of 170pm / V. However, under this cross-linking condition, the absorption peak (~390nm, triplet) of the cross-linking functional group anthracene group has not completely disappeared, which means that a higher cross-linking temperature and / or a longer cross-linking time are required to achieve a complete reaction of the anthracene group until the absorption peak disappears. However, when the cross-linking temperature is further increased and / or the cross-linking reaction time is extended, the electro-optic coefficient will further deteriorate, indicating that after further increasing the cross-linking temperature and / or extending the cross-linking time, the polarization-oriented molecules have undergone serious deorientation.

[0256] from Fig.11 It can be seen from Table 2 that the chromophore compounds FZL1 and FZL2 of Example 1 of the present application, the anthracene group and the maleimide group can complete crosslinking and curing at a lower crosslinking temperature and a shorter crosslinking time (crosslinking conditions are 120° C., 15 min), such as Fig.11 As shown, the absorption peak (~390nm, triplet) of the cross-linking functional group (anthracene) almost completely disappears, indicating that the cross-linking reaction has been completed, the cross-linking temperature is low, and the cross-linking speed is fast. Moreover, as shown in Table 2, the electro-optic coefficient loss before and after cross-linking is minimal, with only a loss of 50pm / V. The electro-optic coefficient after cross-linking also reaches 266pm / V, which is close to the electro-optic coefficient (290pm / V) of Comparative Example 1 when it is not completely cross-linked.

[0257] The performance indicators of polarization efficiency and electro-optic coefficient of different electro-optical films are shown in Table 3.

[0258] Table 3

[0259]

[0260] As mentioned above, the introduction of two first cross-linkable groups and one second cross-linkable group into the chromophore compound can also control the geometric structure and delocalization of electrons, and can minimize the interaction between the chromophore compounds. Therefore, the first-order hyperpolarizability (β) value can be better converted into the electro-optic coefficient (r33) value, thereby improving the macroscopic electro-optic activity of the chromophore compound. If the intermolecular electrostatic interaction is ignored, the electro-optic coefficient (r33) increases with the increase of the number density (N) of the chromophore compound, the first-order hyperpolarizability (β) and the polarization electric field strength (Ep). However, with the increase of the number density of the chromophore compound, the strong dipole-dipole interaction between the molecules of the chromophore compound will hinder the polarization process of the chromophore compound and reduce the polarization efficiency. The introduction of the first cross-linkable group and the second cross-linkable group can increase the distance between the molecules of the chromophore compound, weaken the intermolecular electrostatic interaction, and help improve the polarization efficiency of the chromophore compound.

[0261] like Fig. 12A and Fig. 12B , is a polarization efficiency curve of FZL1 and FZL2 in Example 1 after being formed into an electro-optical device separately. Combined with Table 3, it can be seen that because FZL1 and FZL2 have large first-order hyperpolarizability, the polarization efficiency of 100wt% FZL1 film and 100wt% FZL2 film reaches 1.78±0.07nm 2 / V 2 and 2.33±0.09nm 2 / V 2 Under a polarization field of 100V / μm, the electro-optic coefficients of the two reached 180pm / V and 223pm / V.

[0262] In addition, if Fig. 12C As shown in FIG. 1 , the polarization efficiency curve of the binary chromophore system formed by mixing FZL1 and FZL2 in Example 1 after film formation and assembly into an electro-optical device is shown. Combined with Table 3, it can be seen that when FZL1 and FZL2 are mixed together in a molar ratio of 1:1 to form a binary electro-optical film, the polarization efficiency of the uncrosslinked 1:1 FZL1:FZL2 (NC) is increased to 3.11±0.10nm 2 / V 2 , the electro-optic coefficient has also increased to 316m / V.

[0263] like Fig.12DAs shown in Figure 1, it is a polarization efficiency curve of the binary chromophore system formed by mixing FZL1 and FZL2 in Example 1 after film formation and cross-linking and assembly into an electro-optical device. Combined with Table 3, it can be seen that when the temperature is raised to 120°C and cross-linked for 15 minutes, FZL1 and FZL2 can fully undergo cross-linking reaction. Cross-linking can improve the polarization orientation stability of the electro-optical film, but it will indeed inhibit the improvement of polarization efficiency to a certain extent due to the formation of a polymer network structure. The polarization efficiency of the cross-linked 1:1FZL1:FZL2 (X-link) is lower than that of the uncross-linked 1:1FZL1:FZL2 (NC), and the polarization efficiency is 2.02±0.08nm 2 / V 2 , the electro-optic coefficient loss is small, still as high as 266pm / V.

[0264] It is worth noting that the embodiment of the present application proposes an anthracene and maleimide cross-linked chromophore system FZL1+FZL2, by introducing three anthracene groups and three maleimide groups into the chromophore compounds FLZ1 and FLZ2 respectively, which can achieve cross-linking and curing at a lower temperature and in a shorter time (cross-linking temperature is 120°C, cross-linking time is 15min), and the glass transition temperature after cross-linking is relatively high (reaching 178°C), which improves the stability of the electro-optical material, so that the electro-optical coefficient loss before and after the cross-linking of the anthracene and maleimide groups is small (only 50pm / V is lost), which is beneficial to improve the electro-optical coefficient of the electro-optical material.

[0265] It should be noted that the above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application; the implementation methods of the present application and the features in the implementation methods can be combined with each other without conflict. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A chromophore compound, characterized in that The chromophore compound has the structure of the following formula (I): Wherein, D is an atom or organic group that can provide electrons; A is an electron acceptor group; Z is an atom having at least two valences or an organic group having at least two chemical bonds; π 1 and π 2 Each independently is a π bridge; L 1 and L 2 are independently selected from an atom having at least two valences or an organic group having at least two chemical bonds; X 1 is a first cross-linkable group; X 2 is a second cross-linkable group; p is an integer greater than or equal to 2; q is an integer greater than or equal to 1.

2. The chromophore compound according to claim 1, characterized in that D in the formula (I) is a nitrogen atom.

3. The chromophore compound according to claim 1, characterized in that In the formula (I), Z is a sulfur atom, an oxygen atom or an alkyl group.

4. The chromophore compound according to claim 1, characterized in that In the formula (I), L 1 and L 2 Each of the at least one groups is independently selected from an alkyl group, an ester group, an aryl group and a heteroaryl group.

5. The chromophore compound according to claim 4, characterized in that In the formula (I), p is 2 or 3, and q is 1 or 2.

6. The chromophore compound according to claim 4, characterized in that The first crosslinkable group and the second crosslinkable group are both groups that can undergo click chemistry reaction, thermal crosslinking reaction, photocrosslinking reaction, coupling reaction or polymerization reaction.

7. The chromophore compound according to claim 6, characterized in that The first crosslinkable group and the second crosslinkable group are independently selected from an anthracene group, a maleimide group, an acrylate group, an azide group, an alkynyl group, a hydroxyl group, an isocyanate group, a furan group, a thiol group, an olefin group, a coumarin group, a difluoroolefin group, a styrene group, and the like, and any one of the derivatives of these groups.

8. The chromophore compound according to claim 7, characterized in that The first cross-linkable group and the second cross-linkable group are the same.

9. The chromophore compound according to claim 8, characterized in that The chromophore compound has the structure of the following formula (II) or formula (III):

10. A method for preparing a chromophore compound, characterized in that: The following steps are involved: Connecting an electron bridge molecule containing at least one second reactive group to an electron donor molecule containing at least two first reactive groups to obtain an electron donor group-electron bridge group compound containing the at least two first reactive groups and the at least one second reactive group; and At least one first crosslinkable group and at least one second crosslinkable group are respectively connected to each of the first reactive groups and each of the second reactive groups of the electron donor group-electron bridge group compound, and an electron acceptor group is connected to the electron bridge group of the electron donor group-electron bridge group compound, thereby obtaining the chromophore compound, Wherein, the chromophore compound has the structure of the following formula (I): Wherein, D is an atom or organic group that can provide electrons; A is an electron acceptor group; Z is an atom having at least two valences or an organic group having at least two chemical bonds; π 1 and π 2 Each independently is a π bridge; L 1 and L 2 are independently selected from an atom having at least two valences or an organic group having at least two chemical bonds; X 1 is the first cross-linkable group; X 2 is the second cross-linkable group; p is an integer greater than or equal to 2; q is an integer greater than or equal to 1.

11. The preparation method according to claim 10, characterized in that: The electron donor molecule has the structure of the following formula (IV): Among them, R 3 is the first reactive group, and the first reactive group is selected from any one of a hydroxyl group, an azide group, an alkynyl group, a thiol group, an isocyanate group and an amino group.

12. The preparation method according to claim 11, characterized in that: D in the formula (I) is a nitrogen atom.

13. The preparation method according to any one of claims 10 to 12, characterized in that: The second reactive group is selected from any one of a hydroxyl group, an azide group, an alkynyl group, a thiol group, an isocyanate group and an amino group.

14. The preparation method according to any one of claims 10 to 13, characterized in that: Before connecting the electron bridge molecule to the electron donor molecule, the preparation method further comprises the steps of: attaching a first protecting group to each of the first reactive groups; After the electron bridge molecule is connected to the electron donor molecule, the preparation method further comprises the steps of: attaching a second protecting group to each of the second reactive groups; Before respectively connecting at least one first crosslinkable group and at least one second crosslinkable group to each of the first reactive groups and each of the second reactive groups of the electron donor group-electron bridging group compound, the preparation method further comprises the steps of: The first protecting group and the second protecting group are removed.

15. The preparation method according to claim 14, characterized in that: The electron bridge molecule includes any one of isophorone, thiophene bridge and pyrrole bridge.

16. The preparation method according to claim 15, characterized in that: The first protecting group and the second protecting group are respectively derived from any one of tert-butyldimethylsilyl chloride and its derivatives, tert-butyldiphenylsilyl chloride and its derivatives, and dihydropyran derivatives.

17. The preparation method according to claim 16, characterized in that: The electron donor molecule has a structure of The first compound is prepared from a first crosslinkable group and a second crosslinkable group, wherein the electron bridge molecule is isophorone, the electron acceptor molecule is 2-(3-cyano-4-methyl-5-phenyl-5-(trifluoromethyl)furan-2(5H)-ethylidene)malononitrile, the first crosslinkable group and the second crosslinkable group are the same, and the preparation method comprises the following steps: A tert-butyldimethylsilyl group is generated on the hydroxyl group of the first compound to obtain a structure of a second compound; The second compound is reacted with isophorone in sodium ethoxide and 2-mercaptoethanol to obtain a compound having the structure A third compound; A tert-butyldimethylsilyl group is generated on the hydroxyl group of the third compound to obtain a structure of The fourth compound of The fourth compound is reacted with diethyl phosphate by Wittig-Hornor reaction to obtain a structure of The fifth compound; The nitrile group in the fifth compound is reduced by diisobutylaluminum hydride to obtain a structure of The sixth compound of The sixth compound is subjected to acid hydrolysis to remove the tert-butyldimethylsilyl group to obtain a structure of The seventh compound; The seventh compound and R 4 OH undergoes nucleophilic substitution reaction or Steglich esterification reaction to obtain the structure An eighth compound of The eighth compound is condensed with the electron acceptor molecule to obtain a product having a structure of The chromophore compound, Among them, the R 4 is the first cross-linkable group, and R 4 is the second cross-linkable group, R 4 Any one selected from anthracene group, maleimide group, acrylate group, azide group, alkynyl group, hydroxyl group, isocyanate group, furan group, mercapto group, olefin group, coumarin group, difluoroolefin group, styrene group and derivatives of these groups.

18. The preparation method according to claim 17, characterized in that: R 4 Any one selected from the following groups:

19. An electro-optical material, characterized in that: It comprises at least two chromophore compounds, at least two of the chromophore compounds are used for cross-linking reaction, and the chromophore compound is the chromophore compound according to any one of claims 1 to 9 or the chromophore compound prepared by the preparation method according to any one of claims 10 to 18.

20. The electro-optical material according to claim 19, characterized in that Comprising two chromophore compounds, when the first crosslinkable group and the second crosslinkable group on any one of the chromophore compounds are the same, the first crosslinkable group on one chromophore compound and the first crosslinkable group on the other chromophore compound are selected from any one of the following group combinations: anthracene group and maleimide group, azide group and alkynyl group, hydroxyl group and isocyanate group, anthracene group and acrylate group, furan group and maleimide group, thiol group and olefin group, coumarin group and coumarin group, difluoroolefin group and difluoroolefin group, and styrene group and styrene group, etc.

21. A film, characterized in that: The film is made of the electro-optical material according to claim 19 or 20.

22. An electro-optical glass, characterized in that: The invention comprises a glass substrate and a film located on the glass substrate, wherein the film is the film as claimed in claim 21.

23. An electro-optical device, characterized in that: Contains the film as claimed in claim 21, or contains the electro-optical glass as claimed in claim 22.