Oxime ester photoinitiator, light-cured resin composition and application

By introducing the thioxanthone structure into the oxime ester photoinitiator, the problems of small molecular fragments and poor sensitivity of the photoinitiator under ultraviolet light or mercury lamp in the existing technology are solved, and high sensitivity and good dissolution are achieved. properties, significantly improving the photocuring effect.

CN118724866APending Publication Date: 2024-10-01CHANGZHOU TRONLY ADVANCED ELECTRONICS MATERIALS CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310341491.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing oxime ester photoinitiators are prone to produce small molecular fragments under ultraviolet light or mercury lamp irradiation, and have poor sensitivity and solubility, resulting in poor curing effects of photocurable compositions.

Method used

An oxime ester photoinitiator with a specific structure is provided. The structure is a thioxanthone structure and is synthesized through Friedel-Crafts reaction, oximation reaction and esterification reaction to form a photoinitiator with high sensitivity and good solubility. Used in photocurable resin compositions, especially suitable under 365nm light conditions.

Benefits of technology

It improves the sensitivity and solubility of the photoinitiator, avoids the generation of small molecular fragments, and significantly improves the curing effect of the photocurable resin composition, especially under 365nm light conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724866A_ABST
    Figure CN118724866A_ABST
Patent Text Reader

Abstract

The invention provides an oxime ester photoinitiator, a light-cured resin composition and application of the oxime ester photoinitiator and the light-cured resin composition. The oxime ester photoinitiator has a structure as shown in a formula (I) or a geometric isomer thereof. Compared with the existing oxime ester photoinitiators, a parent structure with the structure as shown in the formula (I) is a thioxanthone structure, so that the stability of a main body is ensured, the absorption wavelength of the initiator is increased by introducing an aromatic ring substitution structure, the light sensitivity of the oxime ester photoinitiators is improved, and the photoinitiators can be applied to the field of photoinitiators. The introduction of the oxime ester structure ensures the photosensitive group of the initiator, the light sensitivity of the formed large conjugated structure product is improved, and the product has high photo-initiation activity (especially suitable for a photo-initiation system under 365nm illumination condition), and also has good solubility. When the light-cured resin composition is applied to the field of light curing of paint, coatings, printing ink, forming materials and the like, small molecular fragments are not generated, and the curing effect of the light-cured resin composition can be improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic chemistry, and in particular to an oxime ester photoinitiator, a photocurable resin composition and applications thereof. Background Art

[0002] Flat panel display technology is widely used in televisions, computers, mobile phones, vehicle-mounted equipment, aircraft and high-speed rail information display, etc. As people's requirements for display clarity and color reproduction gradually increase, flat panel displays have also developed from 1K and 2K to 4K and are moving towards 8K. In addition to relying on the design of microelectronic circuits, flat panel display photoresist is also a key material to achieve this function.

[0003] Flat panel display photoresist is composed of photoinitiators, resins, monomers, pigments, additives and other ingredients. The structures of resins and monomers of photoresists with different display clarity are not much different. The most important difference lies in the structure of the photoinitiator. The higher the clarity of the flat panel display, the higher the sensitivity of the photoresist initiator is required. Therefore, photoinitiator is a key raw material for high-definition flat panel display processing.

[0004] As OLED develops towards flexibility and thin layers, it is necessary to develop initiators of low-molecular-weight fragments. Although some low-molecular-weight fragment initiators have been developed in the early stage, it is difficult to balance the sensitivity and solubility.

[0005] Therefore, it is of great significance to study and develop an oxime ester compound with a new structure to solve the above problems. Summary of the invention

[0006] The main purpose of the present invention is to provide an oxime ester photoinitiator, a photocurable resin composition and an application thereof, so as to solve the problem that the oxime ester photoinitiators in the prior art are prone to produce small molecular fragments under ultraviolet light or mercury lamp irradiation, and have poor sensitivity and solubility, resulting in poor curing effect of the photocurable composition containing them.

[0007] In order to achieve the above object, the present invention provides an oxime ester photoinitiator on the one hand, wherein the oxime ester photoinitiator has a structure shown in formula (I):

[0008] or its geometric isomers,

[0009] R1, R2, R3, R4 and R5 are independently selected from R 11 , OR 11 , SR 11 , COR 11 ,CONR 12 R 13 or CN, R 11 , R12 and R 13 are independently selected from hydrogen atoms, substituted or unsubstituted groups: C1 to C 20 Alkyl, C6~C 30 Aryl, C7~C 30 Arylalkyl, C2~C 20 Heterocyclic group, C4~C 20 Heteroaryl, C3~C 20 Cycloalkyl, C3~C 20 Cycloalkylalkyl, or C3~C 20 A is selected from C1~C 20 Straight or branched alkyl, C3~C 20 Cycloalkyl, C4~C 20 Cycloalkylalkyl or C4~C 20 alkylcycloalkyl; n represents any integer from 1 to 5; optionally, two adjacent groups among R1, R2, R3, R4 and R5 are connected to form a ring.

[0010] In order to achieve the above objectives, another aspect of the present invention further provides a photocurable resin composition, which includes a photoinitiator, an alkali-soluble resin and a polymerizable monomer, wherein the photoinitiator includes the above-mentioned oxime ester photoinitiator provided in the present application.

[0011] Another aspect of the present invention provides an application of the above-mentioned oxime ester photoinitiator provided in the present application, or the above-mentioned photocurable resin composition provided in the present application in paints, coatings, inks and molding materials.

[0012] By applying the technical solution of the present invention, compared with the existing oxime ester photoinitiators, the parent structure of the structure shown in the above formula (I) provided by the present application is a thioxanthone structure, which ensures the stability of the main body, and the introduction of the aromatic ring substitution structure increases the absorption wavelength of the initiator, improves the sensitivity of the oxime ester photoinitiator, and the introduction of the oxime ester structure ensures the photosensitive group of the initiator. Due to the formation of a large conjugated structure, the product sensitivity is improved, has a high photoinitiator activity (especially suitable for photoinitiator systems under 365nm illumination conditions), and also has good solubility. It is applied in the field of photocuring of paints, coatings, inks and molding materials, not only does it not produce small molecule fragments, but it can also improve the curing effect of the photocurable resin composition. The oxime ester photoinitiator of the above specific structure is particularly suitable for photocuring under 365nm illumination conditions. DETAILED DESCRIPTION

[0013] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0014] As described in the background art, existing oxime ester photoinitiators are prone to produce small molecular fragments under ultraviolet light or mercury lamp irradiation, and are difficult to have excellent photosensitivity and poor solubility, resulting in poor curing effect of photocurable compositions containing them. In order to solve the above technical problems, the present application provides an oxime ester compound, which has a structure shown in formula (I):

[0015] or its geometric isomers,

[0016] R1, R2, R3, R4 and R5 are independently selected from but not limited to R 11 , OR 11 , SR 11 , COR 11 ,CONR 12 R 13 or CN, R 11 , R 12 and R 13 Each independently includes but is not limited to hydrogen atoms, substituted or unsubstituted groups: C1~C 20 Alkyl, C6~C 30 Aryl, C7~C 30 Arylalkyl, C2~C 20 Heterocyclic group, C4~C 20 Heteroaryl, C3~C 20 Cycloalkyl, C3~C 20 Cycloalkylalkyl, or C3~C 20 A includes but is not limited to C1~C 20 Straight or branched alkyl, C3~C 20 Cycloalkyl, C4~C 20 Cycloalkylalkyl or C4~C 20 alkylcycloalkyl; n represents any integer from 1 to 5; optionally, two adjacent groups among R1, R2, R3, R4 and R5 are connected to form a ring.

[0017] Compared with the existing oxime ester photoinitiators, the parent structure of the structure shown in the above formula (I) provided by the present application is a thioxanthone structure, which ensures the stability of the main body, and the introduction of the aromatic ring substitution structure increases the absorption wavelength of the initiator, improves the sensitivity of the oxime ester photoinitiator, and the introduction of the oxime ester structure ensures the photosensitive group of the initiator. Due to the formation of a large conjugated structure, the product sensitivity is improved, has a high photoinitiator activity (especially suitable for photoinitiator systems under 365nm illumination conditions), and also has good solubility. It is applied in the field of photocuring of paints, coatings, inks and molding materials, not only does it not produce small molecule fragments, but it can also improve the curing effect of the photocurable resin composition. The oxime ester photoinitiator of the above specific structure is particularly suitable for photocuring under 365nm illumination conditions.

[0018] In a preferred embodiment, R 11 , R 12 and R 13 The substituents in each independently include but are not limited to OR 21 , COR 21 , SR 21 NR 22 R 23 ,CONR 22 R 23 、-NR 22 -OR 23 、-NCOR 22 -OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 、CN、halogen atom、-CR 21 =CR 22 R 23 、-CO-CR 21 =CR 22 R 23 , carboxyl, or epoxy; R 21 , R 22 and R 23 Each independently includes but is not limited to hydrogen atoms, C1~C 20 Alkyl, C6~C 30 Aryl, C7~C 30 Arylalkyl, or C2~C 20 and / or, R 21 , R 22 and R 23 The aliphatic carbon chains in the compound are independently interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds or iminoformate bonds.

[0019] Compared with other types, R 11 , R 12 and R 13 Limiting the substituents in the above-mentioned range is beneficial to improving the sensitivity of the oxime ester photoinitiator, thereby improving its photoinitiator activity and curing efficiency; it is also beneficial to inhibiting the generation of small molecular fragments under ultraviolet light. At the same time, compared with the uninterrupted aliphatic carbon chain, the R 21 , R 22 and R 23 Further limiting the aliphatic carbon chain in the above-mentioned range is beneficial to further improve the sensitivity of the oxime ester photoinitiator, further inhibit the generation of small molecule fragments under ultraviolet light, and is also beneficial to improve the solubility of the oxime ester photoinitiator.

[0020] In a preferred embodiment, R 11 , R 12 and R 13 The aliphatic carbon chains in are independently interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds or imidocarboxylate bonds. 11 , R 12 and R 13 Further limiting the aliphatic carbon chain in the above-mentioned range is beneficial to further improve the sensitivity of the oxime ester photoinitiator, further inhibit the generation of small molecule fragments under ultraviolet light, and is also beneficial to improve the solubility of the oxime ester photoinitiator.

[0021] In a preferred embodiment, when R 11 , R 12 , R 13 Independently include but are not limited to C1~C 20 Alkyl, C7~C 30 Arylalkyl, C3~C 20 Cycloalkyl, C3~C 20 Cycloalkylalkyl, or C3~C 20 When the alkylcycloalkyl group is an alkyl group, the alkyl groups are independently substituted by side chains or terminated with unsaturated bonds. 11 , R 12 and R 13 Limiting the substituents in the above-mentioned range is beneficial to further improve the sensitivity of the oxime ester photoinitiator, thereby further improving its photoinitiator activity, thereby further improving the curing efficiency; and at the same time, it is beneficial to further inhibit the generation of small molecule fragments under ultraviolet light.

[0022] In a preferred embodiment, when R 21 , R22 and R 23 Independently include but are not limited to C1~C 20 Alkyl, or C7~C 30 When the alkyl group is an arylalkyl, the alkyl part thereof is independently substituted by a side chain or terminated with an unsaturated bond; preferably, the side chain is a C3-C6 cycloalkyl group, and when the unsaturated bond is terminated, specifically, the carbon-carbon double bond is terminated. 21 , R 22 and R 23 Limiting the substituents in the above-mentioned range is beneficial to further improve the sensitivity of the oxime ester photoinitiator, thereby further improving its photoinitiator activity, thereby further improving the curing efficiency; and at the same time, it is beneficial to further inhibit the generation of small molecule fragments under ultraviolet light.

[0023] In a preferred embodiment, R1, R2, R3, R4 and R5 independently include but are not limited to C1 to C 20 A straight or branched alkyl group; and / or, R5 includes but is not limited to C1 to C 20 Straight or branched alkyl, C3~C 10 Cycloalkyl, C4~C 20 Cycloalkylalkyl, C4~C 20 Alkylcycloalkyl, C6~C 20 Aryl or C4~C 20 Compared with other types, limiting R1, R2, R3, R4 and R5 within the above-mentioned range is conducive to improving the sensitivity of the oxime ester photoinitiator, thereby improving its photoinitiating activity and curing efficiency; at the same time, it is conducive to inhibiting the generation of small molecular fragments under ultraviolet light irradiation.

[0024] In a preferred embodiment, R1 is a hydrogen atom, R2 and R4 independently include but are not limited to methyl, ethyl or isopropyl; R3 is a hydrogen atom, R5 includes but is not limited to methyl, ethyl, phenyl, thienyl, cyclohexyl; A includes but is not limited to n is 1 or 2. Compared with other types, using the above types of R1, R2, R3, R4, R5, A and limiting n to 1 or 2 is beneficial to further improve the sensitivity of the oxime ester photoinitiator, thereby further improving its photoinitiating activity, thereby further improving the curing efficiency; at the same time, it is beneficial to further inhibit the generation of small molecular fragments under ultraviolet light irradiation.

[0025] In a preferred embodiment, the oxime ester photoinitiator includes but is not limited to one or more compounds having the following structure:

[0026]

[0027]

[0028] The chemical structure of the above-mentioned compound is more stable and it is more difficult to produce small molecule fragments; at the same time, the compound with the above-mentioned structure has higher sensitivity and higher photoinitiator activity, and is particularly suitable for photocuring under 365nm light conditions.

[0029] The second aspect of the present application provides a preferred method for synthesizing oxime ester compounds, which comprises the following steps:

[0030] S1, in a second solvent, allowing the first reactant and the second reactant to undergo a Friedel-Crafts reaction in the presence of a Lewis acid to obtain a first intermediate;

[0031]

[0032] S2, in a third solvent, allowing the first intermediate to undergo an oximation reaction with hydroxylamine hydrochloride to obtain a second intermediate;

[0033]

[0034] S3, in a fourth solvent, allowing the second intermediate to undergo an esterification reaction with an acylating agent under the action of a base to obtain the above-mentioned oxime ester photoinitiator provided in the present application;

[0035]

[0036] Wherein, X is a halogen, and R1, R2, R3, R4, R5, A and n have the same definitions as above.

[0037] In a second solvent, a first reactant containing a thioxanthone structure and a second reactant containing an aromatic ring structure undergo a Friedel-Crafts reaction to obtain a first intermediate; in a third solvent, the first intermediate obtained above undergoes an oximation reaction with hydroxylamine hydrochloride to obtain a second intermediate containing a -C=N-OH structure; in a fourth solvent, the second intermediate undergoes an esterification reaction with an acylating agent under the action of a base to make the second intermediate structure Transformed into Thus, the oxime ester photoinitiator represented by formula (I) in the present application is obtained. The oxime ester photoinitiator prepared by the above method has high sensitivity and solubility and almost no small molecular fragments are generated under ultraviolet light irradiation. In addition, the above preparation method is simple and the raw material cost is controllable.

[0038] In a preferred embodiment, the molar ratio of the first reactant to the second reactant is (1-1.3): (1-1.3). The molar ratio of the first reactant to the second reactant includes but is not limited to the above range, and limiting it within the above range is beneficial to increasing the generation rate of the first intermediate, thereby facilitating the yield of the target product obtained subsequently.

[0039] In a preferred embodiment, the temperature of the Friedel-Crafts reaction is -10 to 10° C. The temperature of the Friedel-Crafts reaction includes but is not limited to the above range, and limiting it within the above range is beneficial to suppressing the occurrence of side reactions, thereby facilitating improving the yield and purity of the first intermediate.

[0040] The Lewis acid in the present application may be a commonly used type in the art. In a preferred embodiment, the Lewis acid includes but is not limited to one or more of the group consisting of aluminum chloride, zinc chloride, magnesium chloride, lithium chloride, and calcium chloride.

[0041] In a preferred embodiment, the molar ratio of the first intermediate to hydroxylamine hydrochloride is (1-1.5): (1-1.5). The molar ratio of the first intermediate to hydroxylamine hydrochloride includes but is not limited to the above range, and limiting it within the above range is beneficial to increase the generation rate of the second intermediate, thereby facilitating the yield of the target product obtained subsequently.

[0042] In a preferred embodiment, the oximation reaction is carried out under heating reflux, and the temperature of the oximation reaction is preferably 50 to 120° C. The temperature of the oximation reaction includes but is not limited to the above range, and limiting it within the above range is conducive to suppressing the occurrence of side reactions, thereby facilitating the improvement of the yield and purity of the second intermediate.

[0043] In a preferred embodiment, the molar ratio of the second intermediate to the acylating agent is (1-1.5): (1-1.5). The molar ratio of the second intermediate to the acylating agent includes but is not limited to the above range, and limiting it within the above range is beneficial to improving the utilization rate of raw materials and the generation rate of oxime lipid photoinitiators.

[0044] In a preferred embodiment, the temperature of the esterification reaction is -10 to 60° C. The temperature of the esterification reaction includes but is not limited to the above range, and limiting it within the above range is beneficial to improving the efficiency of the esterification reaction, and is beneficial to suppressing the occurrence of side reactions, thereby helping to improve the generation rate and purity of the oxime lipid photoinitiator.

[0045] In order to further improve the generation rate and purity of the oxime lipid photoinitiator, preferably, the temperature of the esterification reaction is 0 to 25°C.

[0046] The second solvent, the third solvent and the fourth solvent used in the present application can be respectively used in the common types in the art, without special limitation. In a preferred embodiment, the second solvent includes but is not limited to one or more of the group consisting of dichloromethane, dichloroethane and toluene; the third solvent is a mixture of alcohol and water, preferably a mixture of ethanol and water; the fourth solvent includes but is not limited to one or more of the group consisting of diethyl ether, acetonitrile, tert-butyl methyl ether, tetrahydrofuran, vinyl acetate, toluene, xylene, acetone, methyl ethyl ketone, dichloromethane, chloroform, chlorobenzene, dimethylacetamide, and dimethylformamide.

[0047] In a preferred embodiment, the acylating agent includes but is not limited to acyl halide compounds or acid anhydride compounds; preferably cyclohexanecarbonyl chloride, 2-propylpentanoyl chloride, 3,5,5-trimethylhexanoyl chloride, 3-chloropropionyl chloride, 5-chlorovaleryl chloride, 3-chloropivaloyl chloride, 6-bromohexanoyl chloride, methoxyacetyl chloride, ethoxyacetyl chloride, butoxyacetyl chloride, 3-(methylthio)propionyl chloride, 2-butoxyethoxyacetyl chloride, benzoyl chloride, toluoyl chloride, 3,5-dimethylbenzoyl chloride, 4-methoxybenzoyl chloride, 4-cyanobenzoyl chloride, 4-nitrobenzoyl chloride, 4-phenylbenzoyl chloride, chlorobenzoyl chloride, phenylacetyl chloride, phenylpropionyl chloride, chlorophenylacetyl chloride, 4-phenylbutyryl chloride, 6-phenylhexanoyl chloride, nitrophenylacetyl chloride, phenoxyacetyl chloride, phenoxypropionyl chloride, chlorophenoxyacetyl chloride, nitrophenoxyacetyl chloride, 2-thiophenecarbonyl chloride, thiophene-2-acetyl chloride, chloronicotinoyl chloride, 2-furoyl chloride, quinolinecarbonyl chloride, naphthoyl chloride, 2-ethoxy-1-naphthoyl chloride, anthracenecarbonyl chloride; preferably acetic anhydride, propionic anhydride, capric anhydride, stearic anhydride, isobutyric anhydride, tert-valeric anhydride, 4-methoxyphenylacetic anhydride.

[0048] The base used in the present application can be any commonly used type in the art, without particular limitation. In a preferred embodiment, the base includes but is not limited to one or more of the group consisting of triethylamine, pyridine, diisopropylethylamine, potassium hydroxide, sodium hydroxide and sodium hydride.

[0049] In a preferred embodiment, a catalyst is also added during the esterification reaction; preferably, the catalyst is one or more of the group consisting of 4-dimethylaminopyridine, dicyclohexyldiimine and pyridine.

[0050] The third aspect of the present application also provides a photocurable resin composition, which includes a photoinitiator, an alkali-soluble resin and a polymerizable monomer, wherein the photoinitiator includes the above-mentioned oxime ester photoinitiator provided in the present application.

[0051] The above-mentioned oxime ester photoinitiator provided in the present application has high sensitivity, solubility and is less likely to produce small molecule fragments under ultraviolet light. When applied to the photocuring fields such as paints, coatings, inks and molding materials, not only will small molecule fragments not be produced, but also the curing effect of the photocurable resin composition can be improved. The above-mentioned oxime ester photoinitiator with a specific structure is particularly suitable for photocuring under 365nm light conditions.

[0052] In a preferred embodiment, the photocurable resin composition includes 1 to 10 parts of oxime ester photoinitiator and 10 to 200 parts of alkali-soluble resin, based on the amount required for 100 parts by weight of the polymerizable monomer. Compared with other dosage ranges, limiting the dosage of oxime ester photoinitiator, alkali-soluble resin and polymerizable monomer to the above ranges is conducive to improving the compatibility of oxime ester photoinitiator, alkali-soluble resin and polymerizable monomer; it is also conducive to further improving the photocuring effect of the photocurable resin composition; it is also conducive to inhibiting the generation of small molecule fragments, thereby reducing the occurrence of light-emitting device failures.

[0053] In order to further improve the compatibility of the oxime ester photoinitiator, the alkali-soluble resin and the polymerizable monomer, and further exert the photocuring effect of the photocurable resin composition, preferably, based on the amount required for 100 parts by weight of the polymerizable monomer, the photocurable resin composition also includes 0 to 300 parts of the first solvent.

[0054] In a preferred embodiment, the polymerizable monomer includes but is not limited to dipentaerythritol hexaacrylate.

[0055] In a preferred embodiment, the alkali-soluble resin includes but is not limited to benzyl methacrylate and methyl methacrylate.

[0056] The present application has no particular limitation on the type of the first solvent, as long as it can effectively dissolve other components of the composition. In a preferred embodiment, the first solvent includes but is not limited to butanone.

[0057] In an optional embodiment, the photocurable resin composition of the present application further includes inorganic compounds, colorants and other components, and those skilled in the art can add them according to corresponding needs.

[0058] The fourth aspect of the present application also provides an application of the above-mentioned oxime ester photoinitiator or the above-mentioned photocurable resin composition provided by the present application in paints, coatings, inks and molding materials, without special limitations.

[0059] The above-mentioned oxime ester photoinitiator provided in the present application has high sensitivity, solubility and is less likely to produce small molecule fragments under ultraviolet light. When applied to the photocuring fields such as paints, coatings, inks and molding materials, not only will small molecule fragments not be produced, but also the curing effect of the photocurable resin composition can be improved. The above-mentioned oxime ester photoinitiator with a specific structure is particularly suitable for photocuring under 365nm light conditions.

[0060] The above-mentioned oxime ester photoinitiator provided in the present application can be used in the fields of paints, coatings, inks and molding materials, including but not limited to: coatings applied on substrates such as plastics, metals, glass, ceramics, wood, walls, etc.; photocurable adhesives, photodecomposable coatings; printing inks such as screen printing, offset printing, gravure printing, etc.; photocurable inks for inkjet printing and 3D printing; film materials such as hard coating agents, anti-fouling films, anti-reflection films, impact buffer films, interlayer insulating films, light extraction films, brightening films, and sealing films; optical components such as lenses, lens arrays, optical waveguides, light guide plates, light diffusers, and diffraction elements; optical molding resins such as color filters and black matrices (light-shielding films); optical recording media such as holographic imaging materials; photoresists for electronic circuits and semiconductor manufacturing; optical spacers; rib walls; materials for nanoimprinting; quantum dots; OLEDs, etc.

[0061] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0062] (I) Synthesis of oxime lipid photoinitiators

[0063] Synthesis Example 1

[0064] A method for synthesizing an oxime lipid photoinitiator (compound 1), comprising:

[0065] (1) Preparation of the first intermediate 1a, the synthetic route is as follows:

[0066]

[0067] In a 250mL three-necked flask, 12.7g (0.05mol) of the first reactant 1a and 20mL of dichloromethane were added, stirred to dissolve, and then 6.7g of aluminum chloride was added. The mixture was cooled to 0°C with ice water, and a mixed solution of 10.7g (0.05mol) of the second reactant 1b and 20mL of dichloromethane was added dropwise. The temperature of the Friedel-Crafts reaction was controlled to be 0-5°C. After the addition was completed, the reaction was continued for 1h. The reaction was controlled to end by HPLC, and the reaction solution was slowly poured into 100g of ice water for hydrolysis. After stirring for 1h, the reaction solution was allowed to stand for stratification, the water layer was removed, and the mixture was washed 3 times with 50mL of water respectively. After the organic layer was concentrated, 41.4g of the first intermediate 1a as a yellow oil was obtained with a yield of 95.9% and a purity of 98.06%.

[0068] It should be noted that the first reactant 1a used in this Synthesis Example 1 was purchased from BASF with the brand name ITX, and the second reactant 1b was purchased from Jiaying Photosensitive Materials with the CAS number 80144-02-1.

[0069] (2) Preparation of the second intermediate 1b, the synthetic route is as follows:

[0070]

[0071] 8.6 g (0.02 mol) of the first intermediate 1a, 20 mL of methanol, 1.4 g (0.2 mol) of hydroxylamine hydrochloride and 1.6 g of ammonium acetate were added to a 100 mL reaction bottle, stirred and refluxed for 5 h under heating, and the reaction was controlled to end by HPLC. The reaction was stopped and cooled to room temperature, and then 20 mL of dichloromethane and 20 mL of water were added to the reaction bottle. After continuing to stir for half an hour, the layers were allowed to stand and the organic phase of the lower layer was separated. The organic phase was washed with water until neutral, concentrated, and post-treated to obtain a yellow oil (second intermediate 1b), which was directly used for the next step without purification.

[0072] (3) Preparation of compound 1, the synthetic route is as follows:

[0073]

[0074] Add the second intermediate 1b obtained in step (2) and 20 mL of dichloromethane to a 100 mL reaction bottle, stir to dissolve, add the catalyst 4-dimethylaminopyridine DMAP, add 4 g of acetic anhydride dropwise, drip it for 0.5 h, and continue stirring at room temperature for 2 h. When the reaction is completed by HPLC control, add 30 mL of water to the reaction solution, stir for 10 min, stand and separate the water layer, wash the organic phase with water (30 mL × 3), concentrate, and purify the obtained brown oil by column chromatography (the eluent is ethyl acetate and n-hexane in a weight ratio of 1:50) to obtain 7.8 g of light yellow solid, namely compound 1, with a purity of 98.61%.

[0075] The structure of compound 1 was determined by H-NMR 1 H-NMR (400MHz, Chloroform-d) confirmed that the characterization results are as follows:

[0076] δ8.0012, (J=1.5Hz, 1H), 7.7413 (d, J=7.5Hz, 1H), 7.6824 (dd, J=7.6, 1.5Hz, 1H), 7.510 9-7.5711 (m, 2H), 7.4832 (dd, J=1.4, 0.7Hz, 1H), 7.3123-7.3922 (m, 2H), 7.1916 (td, J= 7.4, 1.5Hz, 1H), 7.0909 (dd, J=7.5, 1.6Hz, 1H), 4.1807 (t, J=7.1Hz, 2H), 3.5735 (t, J=7 .1Hz, 2H), 3.3850 (s, 3H), 3.12-3.0327 (m, 1H), 2.1528 (s, 3H), 1.2709 (d, J=6.8Hz, 6H).

[0077] Synthesis Example 2

[0078] A method for synthesizing an oxime lipid photoinitiator (compound 2), comprising:

[0079] (1) Preparation of the first intermediate 2a, the synthetic route is as follows:

[0080]

[0081] 8.5 g (0.05 mol) of the first reactant 2a and 50 mL of dichloromethane were added to a 250 mL three-necked flask, stirred to dissolve, and then 6.7 g of aluminum chloride was added. The mixture was cooled to 0°C with ice water, and a mixed solution of 11.4 g (0.05 mol) of the second reactant 2b and 20 mL of dichloromethane was added dropwise. The temperature of the Friedel-Crafts reaction was controlled to be 0-5°C. After the addition was completed, the reaction was continued for 1 h. The reaction was controlled to end by HPLC, and the reaction solution was slowly poured into 100 g of ice water for hydrolysis. After stirring for 1 h, the reaction solution was allowed to stand to separate the water layer, and washed 3 times with 50 mL of water respectively. After the organic layer was concentrated, 21.8 g of the first intermediate 2a as a yellow oil was obtained with a yield of 95.1% and a purity of 98.06%.

[0082] It should be noted that the first reactant 2a used in this Synthesis Example 2 was purchased from Hubei Biaoyue Biological and the brand is photoinitiator DETX, and the second reactant 2b was purchased from Cyanamid Company and the CAS number is 35535-52-5.

[0083] (2) Preparation of the second intermediate B.1, the synthetic route is as follows:

[0084]

[0085] 9.5 g (0.02 mol) of the first intermediate 2a, 20 mL of methanol, 1.4 g (0.02 mol) of hydroxylamine hydrochloride and 1.6 g of ammonium acetate were added to a 100 mL reaction bottle, and the mixture was stirred and refluxed for 5 h under heating. The reaction was controlled to be complete by HPLC. The reaction was stopped and cooled to room temperature. Then 20 mL of dichloromethane and 20 mL of water were added to the reaction bottle. After stirring for half an hour, the mixture was allowed to stand for stratification, and the organic phase of the lower layer was separated. The organic phase was then washed with water until neutral, concentrated, and post-treated to obtain a yellow oil, which was directly used for the next step without purification.

[0086] (3) Preparation of compound 2, the synthetic route is as follows:

[0087]

[0088] Add the second intermediate B.1 obtained in step (2) and 20 mL of dichloromethane to a 100 mL reaction bottle, stir to dissolve, add 0.5 g of triethylamine, add 1.6 g of acetyl chloride dropwise, drip for 10 min, and continue stirring at room temperature for 2 h. After the reaction is completed by HPLC control, add 30 mL of water to the reaction solution, stir for 10 min, stand for stratification, wash the organic phase with water (30 mL each time, 3 times in total), concentrate, and purify the obtained brown oil by column chromatography (the eluent is ethyl acetate and n-hexane in a weight ratio of 1:50) to obtain 9.2 g of light yellow solid, i.e., compound 2, with a purity of 98.61%.

[0089] The structure of compound 2 was determined by H-NMR spectroscopy 1 H-NMR (400MHz, Chloroform-d) confirmed that the characterization results are as follows:

[0090] δ7.7222 (dd, J=7.4Hz, 2H), 7.6712 (dd, J=7.6, 1.5Hz, 1H), 7.4909 (d, J=7.5Hz, 1H), 7.3416 (dt, J=1.9, 1.0H z, 1H), 7.2232 (dq, J=1.7, 1.0Hz, 1H), 6.6933 (dd, J=7.5, 1.5Hz, 1H), 6.6112 (d, J=1.5Hz, 1H), 4.1218 (q, J= 8.0Hz, 2H), 4.0341 (q, J=8.0Hz, 2H), 2.7528 (qt, J=8.0, 1.0Hz, 2H), 2.6717 (qd, J=8.1, 1.1Hz, 2H), 2.1570 ( s, 3H), 1.4609 (t, J=8.0Hz, 3H), 1.4137 (t, J=8.0Hz, 3H), 1.2470 (t, J=8.0Hz, 3H), 1.2023 (t, J=8.0Hz, 3H).

[0091] Synthesis Examples 3 to 10

[0092] The difference from Example 1 is that different types of first reactants and second reactants are used to prepare the following compounds 3 to 10, respectively. The chemical structural formulas and corresponding H-NMR characterization data of compounds 3 to 10 are shown in Table 1. The preparation methods are the same as those of Example 1.

[0093] Table 1

[0094]

[0095]

[0096] (II) Preparation of photosensitive resin composition

[0097] The oxime ester photoinitiators prepared in all the above embodiments were used to prepare the photocurable resin composition, wherein the acrylate copolymer was a copolymer of benzyl methacrylate, methacrylic acid and methyl methacrylate in a molar ratio of 70:10:20, and Mw was 10,000.

[0098] In the above-mentioned photocurable resin composition, the photoinitiator is the oxime ester photoinitiator compounds 1 to 12 mentioned above in the present application or a similar photoinitiator known in the prior art for comparison. The amounts of each component used in Examples 1 to 8 and Comparative Examples 1 and 2 of the present application are shown in Table 1, and the amounts of each component used in Examples 9 to 15 are shown in Table 2.

[0099] Table 2

[0100]

[0101]

[0102] It should be noted that the above compound B is prepared by the following preparation method, including: (1) preparation of intermediate B.1, the synthesis route of which is as follows:

[0103]

[0104] To a 500mL four-necked flask, add 19.9g (0.1mol) of raw material B.1, 200mL of dichloromethane and 25.7g of aluminum chloride. Under nitrogen protection, control the temperature at 0-10°C and add dropwise 27.7g of benzoyl chloride into the four-necked flask. Monitor the progress of the reaction by TLC. After the reaction is completed, the reaction solution is obtained. Slowly add the reaction solution into a dilute hydrochloric acid solution to quench it. Separate the organic layer, wash the organic layer with water, desolventize and purify to obtain 21.2g of intermediate B.1. The yield is 70.0% and the purity is 99.0%.

[0105] (2) Preparation of intermediate B.2, the synthetic route is as follows:

[0106]

[0107] Add 15.2g (0.05mol) of intermediate B.1, 200mL of dichloromethane, 22.8g (0.20mol) of isoamyl nitrite and 20.6g (0.21mol) of 37% concentrated hydrochloric acid to a 500mL reaction bottle, stir for 4h at 20-25℃, stop the reaction and obtain the product system, add 100mL of water to the product system, continue stirring for 20min, let stand for stratification, separate the lower organic phase, wash the organic phase with water until neutral and concentrate. Add 100mL of methanol to the concentrate, stir well at room temperature for 6-8h, precipitate solid, rinse the filter cake obtained by filtration with methanol, dry the obtained solid in a 60℃ forced air oven for 5h, and obtain 10.4g of intermediate B.2, with a yield of 62.7% and a purity of 95.5%.

[0108] (3) Preparation of compound B (modified oxime ester compound), the synthetic route is as follows:

[0109]

[0110] To a 250 mL reaction bottle, add 10.4 g of intermediate B.2 (0.03 mol), 100 mL of dichloromethane, and 6.1 g of acetic anhydride (0.06 mol), stir at room temperature to dissolve, monitor the reaction progress by TLC, and obtain a reaction solution after the reaction is completed. Remove dichloromethane from the reaction solution and slurry it with a mixture of acetone and methanol in a volume ratio of 1:1 to obtain 10.7 g of compound B (modified oxime ester compound), with a yield of 95.4% and a purity of 95.8%.

[0111] Embodiment 11

[0112] The difference from Example 1 is that the weight portion of Compound 1 (oxime ester photoinitiator) is 1 part, and the amounts of other components are the same as those in Example 1.

[0113] Example 12

[0114] The difference from Example 1 is that the weight proportion of Compound 1 (oxime ester photoinitiator) is 10 parts, and the amounts of other components are the same as those in Example 1.

[0115] Example 13

[0116] The difference from Example 1 is that the weight portion of Compound 1 (oxime ester photoinitiator) is 0.5 parts, and the amounts of other components are the same as those in Example 1.

[0117] Embodiment 14

[0118] The difference from Example 1 is that the weight portion of the acrylic ester copolymer (alkali-soluble resin) is 10 parts, and the amounts of other components are the same as those in Example 1.

[0119] Embodiment 15

[0120] The difference from Example 1 is that the weight portion of the acrylic ester copolymer (alkali-soluble resin) is 300 parts, and the amounts of other components are the same as those in Example 1.

[0121] Example 16

[0122] The difference from Example 1 is that the weight portion of dipentaerythritol hexaacrylate (polymerizable monomer) is 20 parts, and the amounts of other components are the same as those in Example 1.

[0123] Embodiment 17

[0124] The difference from Example 1 is that the weight portion of dipentaerythritol hexaacrylate (polymerizable monomer) is 500 parts, and the amounts of other components are the same as those in Example 1.

[0125] Table 3

[0126]

[0127] (III) Performance evaluation test of photocurable resin composition

[0128] (1) Sensitivity test

[0129] The above-mentioned photocurable resin composition was stirred in the dark and coated on the PET film with a 6# wire rod to form a coating with a wet film thickness of about 5 μm. The coating was exposed with a mercury lamp (RW-LED-YT200g1) to give 100 mJ / cm 2 The energy was applied to observe the curing film formation and the finger touch method was used for evaluation. The test results are shown in Tables 4 and 5 respectively.

[0130] The evaluation criteria are as follows: 1: Oily, not solid; 2: Oily on the surface, solidified at the bottom; 3: Sticky on the surface, with heavy fingerprints after touch; 4: Basically dry on the surface, slightly astringent after touch, with light fingerprints; 5: Completely solidified, smooth surface, with no fingerprints after touch.

[0131] Table 4

[0132]

[0133] Table 5

[0134] Embodiment 11 Example 12 Example 13 Embodiment 14 Embodiment 15 Example 16 Embodiment 17 Curing conditions 4 5 1 5 4 5 4

[0135] (2) Small molecule fragments (outgas)

[0136] Using the GC-MS test method, 5 g of the sample film prepared in the same manner as above was taken and cut into a suitable size and placed in a headspace bottle for standby use. Headspace sampling was used to observe whether small molecular fragments (outgas) were produced (except for carbon dioxide and self-contained solvent peaks). The test results of Examples 1 to 17 of the present application and Comparative Examples 1 and 2 are shown in Tables 6 and 7.

[0137] The equipment and test conditions used are as follows:

[0138] Agilent 7890B gas chromatograph, chromatographic column: Agilent HP-5ms column; vaporization temperature: 280°C; program temperature rise: 60°C for 3 min, 20°C / min heating rate, 280°C for 10 min;

[0139] Agilent 7697A headspace sampler, headspace conditions: heating box: 110°C; quantitative loop: 120°C; transfer line: 140°C; equilibrium time: 30 min;

[0140] Agilent 7010B mass spectrometer, mass spectrometry conditions: ion source temperature: 280°C; electron energy: 70 eV; scanning range (m / z): 30-400.

[0141] Table 7

[0142]

[0143] Table 8

[0144]

[0145] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0146] (1) According to Table 2, the difference between each embodiment and the comparative example is only the different types of photoinitiators used. Combined with the sensitivity test results in Table 4, it can be seen that the curing efficiency of the photocurable compositions prepared in comparative examples 1 to 3 under the irradiation of a mercury lamp is respectively worse than that of embodiments 1 to 10, and can only achieve basic surface dryness, slightly astringent after touch, and light fingerprints; at the same time, the curing efficiency under the irradiation of a mercury lamp is very low, so curing cannot be achieved, and the surface is sticky when touched by fingers. The photocurable resin compositions prepared in embodiments 1 to 10 can achieve a completely cured effect under the irradiation of a mercury lamp, and the surface is smooth, and there are no fingerprints after touch. This shows that the above-mentioned oxime ester photoinitiator with a specific structure provided in the present application can improve the curing efficiency of the photocurable resin composition under the irradiation of a mercury lamp, which shows that the above-mentioned oxime ester photoinitiator has good sensitivity.

[0147] By comparing Example 1 and Comparative Example 3, it can be seen that the oxime ester photoinitiator provided in the present application has a conjugated structure formed due to the introduction of an aromatic ring structure in its chemical structure, which, on the one hand, gives it a stable structure, and on the other hand, enables it to absorb light in a longer wavelength range, thereby increasing its sensitivity and improving the photocuring effect of the photocurable resin composition.

[0148] Comparing Examples 1, 11 to 13, it can be seen that the amount of photoinitiator in Example 13 is significantly lower than the preferred range of the present application, and the wet film after coating in this example is difficult to cure under the irradiation of a mercury lamp; while the wet films in Examples 1, 11 and 12 can achieve basic surface drying or complete curing; in addition, no small molecule fragments are generated in Examples 1, 11 to 13. Comparing Examples 1, 14 and 15, it can be seen that the amount of acrylate copolymer in Example 15 is significantly higher than the preferred range of the present application, and the curing rate of the wet film after coating in this example under the irradiation of a mercury lamp is lower than that of Examples 1 and 14; in addition, no small molecule fragments are generated in Examples 1, 14 and 15. Comparing Examples 1, 16 and 17, it can be seen that the amount of dipentaerythritol hexaacrylate in Example 17 is significantly higher than the preferred range of the present application, and the curing rate of the wet film after coating in this example under the irradiation of a mercury lamp is lower than that of Examples 1 and 16; in addition, no small molecule fragments are generated in Examples 1, 16 and 17.

[0149] It can be seen that, compared with other ranges, limiting the amount of oxime ester photoinitiator, alkali-soluble resin and polymerizable monomer within the preferred range of the present application is beneficial to improving the compatibility of oxime ester photoinitiator, alkali-soluble resin and polymerizable monomer; it is beneficial to improving the curing rate and curing effect of the photocurable resin composition (especially improving the photocuring effect under 385nm light conditions).

[0150] (2) From the test results in Table 7 and Table 8, it can be seen that small molecule fragments were produced in Comparative Examples 1 and 2, while no small molecule fragments were produced in Examples 1 to 17. This shows that compared with other types of photoinitiators, the oxime ester photoinitiator provided in the present application is not easy to produce small molecule fragments.

[0151] In summary, the oxime ester photoinitiator with a specific structure provided in the present application can be applied to a conventional ultraviolet light curing system and can be cured well under a mercury lamp. Compared with other types of photoinitiators, the oxime ester photoinitiator provided in the present application is not easy to produce small molecule fragments and has the characteristics of low outgas.

[0152] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0153] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An oxime ester photoinitiator, characterized in that: The oxime ester photoinitiator has a structure shown in formula (I): or its geometric isomers, R1, R2, R3, R4 and R5 are independently selected from R 11 , OR 11 , SR 11 , COR 11 ,CONR 12 R 13 or CN, the R 11 , the R 12 and the R 13 are independently selected from hydrogen atoms, substituted or unsubstituted groups: C1 to C 20 Alkyl, C6~C 30 Aryl, C7~C 30 Arylalkyl, C2~C 20 Heterocyclic group, C4~C 20 Heteroaryl, C3~C 20 Cycloalkyl, C3~C 20 Cycloalkylalkyl, or C3~C 20 of alkylcycloalkyl; A is selected from C1~C 20 Straight or branched alkyl, C3~C 20 Cycloalkyl, C4~C 20 Cycloalkylalkyl or C4~C 20 of alkylcycloalkyl; n represents any integer from 1 to 5; Optionally, two adjacent groups among the R1, the R2, the R3, the R4 and the R5 are connected to form a ring.

2. The oxime ester photoinitiator according to claim 1, characterized in that: The R 11 , the R 12 and the R 13 The substituents in are independently selected from OR 21 , COR 21 , SR 21 NR 22 R 23 ,CONR 22 R 23 、-NR 22 -OR 23 、-NCOR 22 -OCOR 23 、-C(=N-OR 21 )-R 22 、-C(=N-OCOR 21 )-R 22 、CN、halogen atom、-CR 21 =CR 22 R 23 、-CO-CR 21 =CR 22 R 23 , carboxyl, or epoxy; The R 21 , the R 22 and the R 23 are independently selected from hydrogen atoms, C1 to C 20 Alkyl, C6~C 30 Aryl, C7~C 30 Arylalkyl, or C2~C 20 and / or, The R 21 , the R 22 and the R 23 The aliphatic carbon chains in the compound are independently interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds or iminoformate bonds.

3. The oxime ester photoinitiator according to claim 1 or 2, characterized in that: The R 11 , the R 12 and the R 13 The aliphatic carbon chains in the compound are independently interrupted 1 to 5 times by unsaturated bonds, ether bonds, thioether bonds, ester bonds, thioester bonds, amide bonds or iminoformate bonds.

4. The oxime ester photoinitiator according to any one of claims 1 to 3, characterized in that: When the R 11 , the R 12 , the R 13 Each independently selected from C1 to C 20 Alkyl, C7~C 30 Arylalkyl, C3~C 20 Cycloalkyl, C3~C 20 Cycloalkylalkyl, or C3~C 20 When the alkylcycloalkyl group is an alkyl group, the alkyl groups are independently substituted by side chains or terminated with unsaturated bonds; When the R 21 , the R 22 and the R 23 Each independently selected from C1 to C 20 Alkyl, or C7~C 30 When the arylalkyl group is an arylalkyl group, the alkyl parts thereof are independently substituted by side chains or terminated with unsaturated bonds; preferably, the side chains are C3-C6 cycloalkyl groups, and when terminated with unsaturated bonds, specifically with carbon-carbon double bonds.

5. The oxime ester photoinitiator according to claim 4, characterized in that: The R1, R2, R3, R4 and R5 are independently selected from C1 to C 20 A straight or branched alkyl group; and / or The R5 is selected from C1~C 20 Straight or branched alkyl, C3~C 10 Cycloalkyl, C4~C 20 Cycloalkylalkyl, C4~C 20 Alkylcycloalkyl, C6~C 20 Aryl or C4~C 20 The heteroaryl group.

6. The oxime ester photoinitiator according to any one of claims 1 to 5, characterized in that: R1 is a hydrogen atom, R2 and R4 are independently selected from methyl, ethyl or isopropyl; R3 is a hydrogen atom, R5 is selected from methyl, ethyl, phenyl, thienyl, cyclohexyl; A is selected from The n is 1 or 2.

7. The oxime ester photoinitiator according to claim 6, characterized in that: The oxime ester photoinitiator is selected from one or more compounds having the following structure:

8. A photocurable resin composition, characterized in that: The photocurable resin composition comprises a photoinitiator, an alkali-soluble resin and a polymerizable monomer, wherein the photoinitiator comprises the oxime ester photoinitiator according to any one of claims 1 to 7.

9. The photocurable resin composition according to claim 8, characterized in that: The photocurable resin composition comprises 1 to 10 parts of the oxime ester photoinitiator and 10 to 200 parts of an alkali-soluble resin based on 100 parts by weight of the polymerizable monomer; Preferably, the photocurable resin composition further comprises 0 to 300 parts of a first solvent based on 100 parts by weight of the polymerizable monomer.

10. Use of the oxime ester photoinitiator according to any one of claims 1 to 7, or the photocurable resin composition according to claim 8 or 9 in paints, coatings, inks and molding materials.

Citation Information

Cited By