Phenolic cyanate ester resin as well as preparation method and application thereof

By adding an efficient catalyst and controlling the reaction conditions during the synthesis of phenolic cyanate ester resin, the problem of many by-products was solved, and a high-purity, high-temperature-resistant resin was obtained, which is suitable for the application of wave-transmitting composite materials.

CN118725219APending Publication Date: 2024-10-01THE RES INST FOR SPECIAL STRUCTURES OF AERONAUTICAL COMPOSITE AVIC

Patent Information

Application Number
CN202410935346.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

There are many by-products in the synthesis process of existing phenolic cyanate ester resin, resulting in insufficient product purity and difficulty in complete separation.

Method used

Add a high-efficiency catalyst to the reaction system, and control the raw material feed ratio, reaction temperature and time. Through low-temperature reaction and appropriate organic solvent extraction, the production of by-products is reduced and the purity of the resin is improved.

Benefits of technology

A phenolic cyanate resin with less by-products and high cross-linking density was obtained. It has high strength and high temperature resistance and is suitable for the development of wave-transmitting composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941152120000021
    Figure BDA0004941152120000021
  • Figure BDA0004941152120000041
    Figure BDA0004941152120000041
  • Figure FDA0004941152110000011
    Figure FDA0004941152110000011
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer resin materials and particularly relates to phenolic cyanate ester resin as well as a preparation method and application thereof. The preparation method comprises the following steps: firstly, taking phenolic resin and cyanogen bromide as raw materials, mixing the two raw materials in a reaction solvent, adding a catalyst into the reaction solvent, and reacting in a low-temperature environment to obtain a phenolic cyanate resin crude product; and (S2) dissolving the resin crude product obtained in the step (S1) with an organic solvent A, adding an organic solvent B for extraction, and finally removing the solvent to obtain the phenolic cyanate resin. The prepared resin has the characteristics of high strength and high temperature resistance, can be used as a resin matrix of a wave-transparent composite material, and has great application prospects in the fields of radar radomes, electromagnetic functional structures, high-performance copper-clad plates and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer resin materials, and specifically relates to a phenolic cyanate resin, a preparation method and an application thereof. Background Art

[0002] Cyanate is a high-performance resin matrix material with excellent comprehensive performance, good heat resistance, mechanical properties, dielectric properties and good process performance. Phenolic cyanate is one of them, which introduces cyanate functional group (-OCN) on the skeleton of linear phenolic formaldehyde, and after triazine cyclization curing reaction, forms stable structures such as triazine ring and aromatic heterocycle in the cured resin, has outstanding heat resistance and ablation resistance, and has potential important uses in aerospace, high technology and civil fire retardant materials. In the disclosed technology, patent CN110330612A discloses a synthesis process of phenolic cyanate resin, and the synthesis method is that methoxy-substituted phenolic cyanate and cyanogen chloride are carried out under triethylamine catalysis, and the reaction is easy to cause more by-products. Patent CN102558471A discloses a phenolic aralkyl cyanate resin and a synthesis method thereof, which is prepared with trialkylamine as a catalyst, but this method usually uses dichloromethane and chloroform as solvents, which is difficult to separate completely, and the by-product content is high. Summary of the invention

[0003] Purpose of the invention: The present invention provides a high temperature resistant, high strength phenolic cyanate resin for wave-transmitting composite materials and a preparation method thereof. To solve the problem of a large number of by-products in the current synthesis process of phenolic cyanate esters, the present invention promotes the main reaction and reduces the generation of by-products by adding a high-efficiency catalyst to the reaction system and controlling the feed ratio, reaction temperature and reaction time, thereby providing a resin basis for the development of wave-transmitting composite materials.

[0004] Technical solution: On the one hand, the present invention provides a method for preparing a phenolic cyanate ester resin, comprising the following steps:

[0005] Step S1, using phenolic resin and cyanogen bromide as raw materials, mixing the two raw materials in a reaction solvent, adding a catalyst thereto, reacting under a low temperature environment, and obtaining a crude phenolic cyanate resin;

[0006] Step S2, dissolving the crude resin obtained in step S1 with organic solvent A, then adding organic solvent B for extraction, and finally removing the solvent to obtain phenolic cyanate ester resin;

[0007] The reaction equation is:

[0008]

[0009] Where n=2~7.

[0010] Furthermore, in step S1, using phenolic resin and cyanogen bromide as raw materials, 10 to 25 parts of phenolic resin and 10 to 30 parts of cyanogen bromide are mixed in a reaction solvent, a catalyst is added, and the mixture is reacted at a temperature range of -20°C to -5°C for 5 to 15 hours to obtain a crude phenolic cyanate resin.

[0011] Furthermore, the reaction solvent is one of acetone, tetrahydrofuran, dioxane and dimethylformamide.

[0012] Furthermore, the catalyst is one or both of trialkylamine and triethylamine.

[0013] Furthermore, solvent A is one or both of dichloromethane and dichloroethane.

[0014] Furthermore, solvent B is one or both of butanone and toluene.

[0015] On the other hand, the present invention also provides a phenolic cyanate ester resin, which is synthesized by the above preparation method and has the structural formula:

[0016] Among them, n=2~7.

[0017] The phenolic cyanate resin as described above can be used in radar antenna covers, electromagnetic functional structures, and copper-clad laminates as a resin matrix for wave-transmitting composite materials.

[0018] Beneficial technical effects: The present invention reacts a low molecular weight phenolic resin with cyanogen bromide, controls the raw material feed ratio, reaction temperature, reaction time, and adds a high-efficiency catalyst to promote the main reaction and reduce the occurrence of side reactions, and obtains a crude product with less by-products and high crosslinking density. The crude product is purified by extraction with a suitable organic solvent to obtain a resin monomer with high purity.

[0019] In the material composition of the present invention, the amount of phenolic resin is 10 to 25 parts, and the amount of cyanogen bromide is 10 to 30 parts. The reaction temperature is -20°C to -5°C, and the reaction time is 5 to 15h. Through a large number of experimental explorations and analyses, it is found that side reactions are prone to occur in the synthesis of phenolic cyanate resins, resulting in insufficient product purity. By lowering the reaction temperature (-20°C to -5°C) and increasing the amount of cyanogen bromide, side reactions can be effectively reduced and the degree of cyanate reaction can be increased. Therefore, in the present invention, on the basis of the stoichiometric ratio, the method of using cyanogen bromide in excess of phenolic resin is adopted; at the same time, the molecular weight of the phenolic resin should not be too large. If the molecular weight is too large, it will affect the reaction activity and is not conducive to the reaction. Finally, the preferred molecular formula of the present invention is n=2 to 7.

[0020] In addition, in the preparation process of the present invention, after the catalytic reaction in S1, a crude phenolic cyanate resin is obtained, which contains impurities such as imine carbonate and diethyl cyanamide by-products, unreacted raw materials, catalysts, etc.; therefore, it is purified in step S2. The difficulty of the purification process is that it is not easy to find a suitable extraction solvent that can effectively separate the resin monomer from the impurities. By comparing and analyzing the solubility of the phenolic cyanate resin monomer and other impurities, and testing commonly used organic solvents, the preferred solvent A of the present invention is one or both of dichloromethane and dichloroethane, and the solvent B is one or both of butanone and toluene.

[0021] After the triazine cyclization polymerization reaction, stable structures such as triazine rings and aromatic rings exist in the structure of the phenolic cyanate resin. Therefore, the resin has high strength and high temperature resistance. It can be used as a resin matrix for wave-transmitting composite materials and has great application prospects in radar antenna covers, electromagnetic functional structures, high-performance copper clad laminates and other fields. DETAILED DESCRIPTION

[0022] The present invention is further described below in conjunction with implementation cases, which are only some implementation cases or certain specific implementation forms of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] The problem that the current method for preparing phenolic cyanate resin is difficult to control side reactions leading to insufficient product purity is addressed. To improve these deficiencies, the present invention uses phenolic resin as a raw material, reacts it with cyanogen bromide, uses a high-efficiency catalyst to promote the main reaction, reduces the generation of side products, and thus obtains a phenolic cyanate resin with stable performance.

[0024] In a specific implementation process, 10 to 25 parts of phenolic resin and 10 to 30 parts of cyanogen bromide are mixed in a reaction solvent, a catalyst is added, and the mixture is reacted at a temperature range of -20°C to -5°C for 5 to 15 hours to obtain a crude phenolic cyanate resin; the crude resin is first dissolved in solvent A, then solvent B is added for extraction, and finally the solvent is removed to obtain a phenolic cyanate resin;

[0025] The specific reaction equation is:

[0026]

[0027] Where n=2~7.

[0028] The cyanate resin is a phenolic cyanate resin having the following molecular structure:

[0029] Among them, among them, n=2~7.

[0030] Example 1

[0031] 10 parts of phenolic resin and 15 parts of cyanogen bromide were dissolved in acetone, trialkylamine was added as a catalyst, and the crude resin was obtained after 6 hours of reaction. The crude resin was dissolved in dichloromethane, and butanone was added to the solution for extraction. After separation, butanone was removed by reduced pressure distillation to obtain a phenolic cyanate resin.

[0032] The glass transition temperature of the prepared phenolic cyanate resin cured product is 385°C, and the bending strength is 95 MPa. The test results of the vector network analyzer show that its dielectric constant is 2.90 and the loss tangent is 0.008 at 10 GHz.

[0033] Example 2

[0034] 15 parts of phenolic resin and 20 parts of cyanogen bromide were dissolved in acetone, triethylamine was added as a catalyst, and the crude resin was obtained after 8 hours of reaction. The crude resin was dissolved in ethylene dichloride, and toluene was added to the solution for extraction. After separation, toluene was removed by vacuum distillation to obtain a phenolic cyanate resin.

[0035] The glass transition temperature of the prepared phenolic cyanate resin cured product is 390°C, and the bending strength is 100 MPa. The test results of the vector network analyzer show that its dielectric constant is 2.90 and the loss tangent is 0.007 at 10 GHz.

[0036] Example 3

[0037] 10 parts of phenolic resin and 13 parts of cyanogen bromide were dissolved in tetrahydrofuran, trialkylamine was added as a catalyst, and the crude resin was obtained after the reaction for 10 hours. The crude resin was dissolved in dichloromethane, and butanone was added to the solution for extraction. After separation, butanone was removed by reduced pressure distillation to obtain a phenolic cyanate resin.

[0038] The glass transition temperature of the prepared phenolic cyanate resin cured product is 387°C, the bending strength is 96 MPa, and the vector network analyzer test results show that its dielectric constant is 2.95 and the loss tangent is 0.008 at 10 GHz.

[0039] Example 4

[0040] 10 parts of phenolic resin and 18 parts of cyanogen bromide were dissolved in dimethylformamide, triethylamine was added as a catalyst, and the crude resin was obtained after 9 hours of reaction. The crude resin was dissolved in ethylene dichloride, and toluene was added to the solution for extraction. After separation, toluene was removed by vacuum distillation to obtain a phenolic cyanate resin.

[0041] The glass transition temperature of the prepared phenolic cyanate resin cured product is 385°C, the bending strength is 95 MPa, and the vector network analyzer test results show that its dielectric constant is 2.92 and the loss tangent is 0.008 at 10 GHz.

[0042] Example 5

[0043] 15 parts of phenolic resin and 18 parts of cyanogen bromide were dissolved in dioxane, triethylamine was added as a catalyst, and the crude resin was obtained after the reaction for 12 hours. The crude resin was dissolved in ethylene dichloride, and butanone was added to the solution for extraction. After separation, butanone was removed by reduced pressure distillation to obtain a phenolic cyanate resin.

[0044] The glass transition temperature of the prepared phenolic cyanate resin cured product is 390°C, the bending strength is 93 MPa, and the vector network analyzer test results show that its dielectric constant is 2.97 and the loss tangent is 0.007 at 10 GHz.

[0045] Example 6

[0046] 10 parts of phenolic resin and 16 parts of cyanogen bromide were dissolved in acetone, trialkylamine was added as a catalyst, and the crude resin was obtained after 7 hours of reaction. The crude resin was dissolved in dichloromethane, and toluene was added to the solution for extraction. After separation, toluene was removed by vacuum distillation to obtain a phenolic cyanate resin.

[0047] The glass transition temperature of the prepared phenolic cyanate resin cured product is 383°C, the bending strength is 92 MPa, and the vector network analyzer test results show that its dielectric constant is 2.95 and the loss tangent is 0.007 at 10 GHz.

[0048] The present invention adopts the phenol-cyanogen bromide method to synthesize a phenolic cyanate resin with high temperature resistance, high strength and good dielectric properties; the phenolic cyanate resin can be used as a resin matrix of a wave-transmitting composite material and has great application prospects in the fields of radar antenna covers, high-performance copper-clad laminates, etc.

[0049] Those skilled in the art will appreciate that, unless otherwise specifically defined, all technical terms used above have the same meanings as those generally understood by ordinary technicians in the field to which the present invention belongs; all the above specific implementation methods and specific cases further illustrate the purpose, technical solutions and beneficial technical effects of the present invention in detail. It should also be understood that the above description is only some specific implementation methods and cases of the present invention, and is not intended to limit the present invention. On the contrary, any other modifications, equivalent substitutions, improvements, etc. made within the design ideas and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a phenolic cyanate ester resin, characterized in that: The following steps are involved: Step S1, using phenolic resin and cyanogen bromide as raw materials, mixing the two raw materials in a reaction solvent, adding a catalyst thereto, reacting under a low temperature environment, and obtaining a crude phenolic cyanate resin; Step S2, dissolving the crude resin obtained in step S1 with organic solvent A, then adding organic solvent B for extraction, and finally removing the solvent to obtain phenolic cyanate ester resin; The reaction equation is: Where n=2~7.

2. The method for preparing a phenolic cyanate ester resin according to claim 1, wherein: In step S1, phenolic resin and cyanogen bromide are used as raw materials, 10 to 25 parts of phenolic resin and 10 to 30 parts of cyanogen bromide are mixed in a reaction solvent, a catalyst is added, and the mixture is reacted at a temperature range of -20°C to -5°C for 5 to 15 hours to obtain a crude phenolic cyanate resin.

3. The method for preparing a phenolic cyanate ester resin according to claim 2, wherein: The reaction solvent is one of acetone, tetrahydrofuran, dioxane and dimethylformamide.

4. The method for preparing a phenolic cyanate ester resin according to claim 2, wherein: The catalyst is one or both of trialkylamine and triethylamine.

5. The method for preparing a phenolic cyanate ester resin according to claim 1, wherein: Solvent A is one or both of dichloromethane and dichloroethane.

6. The method for preparing a phenolic cyanate ester resin according to claim 1, wherein: Solvent B is one or both of butanone and toluene.

7. A phenolic cyanate resin synthesized by the preparation method according to any one of claims 1 to 6, and having the structural formula: in, n=2~7。 8. A phenolic cyanate resin which can be used as a resin matrix for wave-transmitting composite materials in radar antenna covers, electromagnetic functional structures, and copper-clad laminates.

Citation Information

Patent Citations

  • Phenolic aralkyl cyanate resin and synthesis method thereof

    CN102558471A

  • Production process of phenolic cyanate resin

    CN110330612A

Cited By

  • Preparation method of flame-retardant cyanate resin adhesive

    CN119614114A

  • Preparation method of flame retardant cyanate ester resin adhesive

    CN119614114B