Modified polysiloxane, preparation method and application thereof, and supercritical CO2 fracturing fluid

Through the preparation of modified polysiloxane, a highly dispersed polymer with high CO2 solubility and viscosity is formed, which solves the problem of insufficient solubility and viscosity of existing supercritical CO2 thickeners and significantly improves the efficiency of shale reservoirs. Oil and gas drive efficiency in the layer.

CN118725306APending Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310319053.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing supercritical CO2 thickeners have low carbon dioxide solubility and low viscosity, which affects their oil and gas development results in shale reservoirs.

Method used

Modified polysiloxane is used, which includes multiple polysiloxane macromolecular chains and multiple linking groups connecting different polysiloxane macromolecular chains. It is prepared through polymerization reaction and hydrosilylation reaction to form a product with good CO2 dissolution It is a polymer with high dispersion properties and viscosity, and toluene is added to supercritical CO2 to improve solubility and viscosity.

Benefits of technology

It improves the viscosity and solubility of supercritical CO2 fluid, enhances the ability of the thickener to dissolve CO2, and significantly improves the oil and gas driving efficiency and recovery rate in shale reservoirs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725306A_ABST
    Figure CN118725306A_ABST
Patent Text Reader

Abstract

The present invention relates to a modified polysiloxane, which is characterized in that the modified polysiloxane comprises a plurality of polysiloxane macromolecular chains and a plurality of linking groups for linking different polysiloxane macromolecular chains, the linking groups have a structure represented by a formula (1), * is a bond-linking position with Si phases contained in different polysiloxane macromolecular chains, and * is a bond-linking position with Si phases contained in different polysiloxane macromolecular chains. R1 and R2 are independently selected from C1-C3 alkylene groups, and the obtained modified polysiloxane can improve the viscosity of the supercritical CO2 fluid and the CO2 dissolving capacity. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of petroleum extraction fracturing fluid, and specifically relates to a modified polysiloxane and a preparation method and application thereof, as well as a supercritical CO2 fracturing fluid. Background Art

[0002] Supercritical CO2 fracturing technology can reduce the water sensitivity and water lock of underground reservoirs caused by hydraulic fracturing when transforming low-permeability shale reservoirs. It can reduce the friction resistance and formation damage of reservoir fractures and improve the rheological properties of crude oil in view of the low fluidity and high friction resistance of oil-based fracturing fluids. However, CO2 is a weak solvent and generally cannot be dissolved in high molecular weight, polar, and ionic compounds. In addition, due to its low viscosity, it has a series of problems such as poor sand carrying capacity, large filtrate capacity, and poor fracturing performance, which is not conducive to improving the sweep coefficient of CO2 fracturing fluids and the development of oil and gas in shale reservoirs.

[0003] The thickeners studied at present are mainly divided into fluorine-containing polymers, hydrocarbon polymers and silicon-containing polymers. Fluorine-containing polymer thickeners have good solubility and thickening properties, but their high cost and serious environmental pollution also restrict their field applications; low molecular hydrocarbons have good solubility, but poor thickening effect, long-chain high molecular hydrocarbons can be dissolved in CO2 under co-solvent conditions, but the effect of co-solvents on the formation cannot be ignored; silicon-containing polymers rely on the formation of Lewis acid hydrogen bonds between co-solvents and CO2, as well as the similar compatibility of co-solvents and siloxanes to improve solubility, and have low cohesive energy, good economy, and huge development potential.

[0004] At present, the modification of silicon-containing polymers has become an important research direction of supercritical CO2 thickeners. CN107236091A provides a supercritical carbon dioxide thickener, the components of which are: (a) polydimethylsiloxane; (b) acrylate compounds; (c) styrene compounds; (d) initiator; (e) emulsifier; but its co-solvent dosage is large and its solubility is poor. CN108003349A provides a supercritical carbon dioxide thickener of siloxane polymer for fracturing, which is obtained by reacting an aromatic amide-terminated side chain modified siloxane polymer with a hydrogen-containing siloxane; the thickener has good thickening properties, but the test temperature and pressure are low, the solvent dosage is large, and the thickener's ability to dissolve in carbon dioxide needs to be further improved. Therefore, it is necessary to develop a modified polysiloxane to improve the solubility and viscosity of supercritical CO2 thickeners. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of low carbon dioxide solubility and viscosity of supercritical CO2 thickeners in the prior art, and to provide a modified polysiloxane, a preparation method and application thereof, and a supercritical CO2 fracturing fluid.

[0006] In order to achieve the above object, the first aspect of the present invention provides a modified polysiloxane, wherein the modified polysiloxane comprises: a plurality of polysiloxane macromolecular chains and a plurality of connecting groups connecting different polysiloxane macromolecular chains, wherein the connecting groups have a structure shown in formula (1),

[0007]

[0008] Among them, * is the position of bonding with Si contained in different polysiloxane macromolecular chains, R 1 and R 2 Each is independently selected from one of C1-C3 alkylene groups.

[0009] The second aspect of the present invention provides a method for preparing a modified polysiloxane, wherein the preparation method comprises the steps of:

[0010] (1) subjecting cyclic siloxane and chain siloxane to a polymerization reaction under the action of a first catalyst to obtain an intermediate product;

[0011] (2) subjecting the intermediate product to a hydrosilylation reaction under the action of an initiator and a second catalyst to obtain a modified polysiloxane.

[0012] The preparation method provided by the present invention can avoid the occurrence of high heat polymerization, so that the polymer generated by the reaction is in a highly dispersed state, and the stability of the dispersed state is very good, thereby improving the viscosity of the supercritical CO2 fluid and still having a good viscosity after being stored for 90 days.

[0013] The third aspect of the present invention provides a modified polysiloxane prepared by the preparation method of the present invention.

[0014] A fourth aspect of the present invention provides an application of the modified polysiloxane of the present invention in supercritical CO2 fracturing.

[0015] A fifth aspect of the present invention provides a supercritical CO2 fracturing fluid, wherein the fracturing fluid comprises the aforementioned modified polysiloxane as a thickener.

[0016] The supercritical CO2 fracturing fluid provided by the present invention has a volume ratio of toluene to modified polysiloxane of 1:1-6:1. The addition of toluene can effectively improve the solubility of modified polysiloxane in liquid CO2. Due to similar polarity, toluene and modified polysiloxane molecules interact with each other. In addition, there is a CH...O bond between CO2 and toluene molecules, and CO2 also forms a Lewis acid-base pair, which is combined with the branched CO2-philic group, that is, the structure shown in formula (1). These interactions jointly construct a three-dimensional network structure of modified polysiloxane-CO2.

[0017] Through the above technical scheme, the modified polysiloxane provided by the present invention contains a connecting group of the structure shown in formula (1), which has good CO2 solubility and can be dissolved in a variety of organic solvents. It can not only bond with the polysiloxane macromolecular chain, but also form a Lewis acid-base pair with CO2 when used as a thickener for supercritical CO2 fracturing fluid, so that a network structure with a certain strength can be formed between CO2 and the thickener. In addition to maintaining good chain flexibility of the modified polysiloxane under high temperature and high pressure, it also increases the bond energy between the carbon dioxide molecules and the thickener in the three-dimensional space, thereby enhancing the thickener's ability to dissolve CO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a fluid viscosity curve of a supercritical CO2 fracturing fluid prepared using the modified polysiloxane obtained in Example 1 at different thickener contents and different shear rates;

[0019] Figure 2 This is a viscosity change curve of the supercritical CO2 fracturing fluid prepared using the modified polysiloxane obtained in Example 1 at different temperatures and pressures;

[0020] Figure 3 This is the nuclear magnetic resonance T2 spectrum of the supercritical CO2 fracturing fluid made from the siloxane polymer obtained in Example 2 before and after it acts on the core;

[0021] Figure 4 This is the nuclear magnetic resonance T2 spectrum of the supercritical CO2 fracturing fluid made from the modified polysiloxane obtained in Example 2 before and after it acts on the core. DETAILED DESCRIPTION

[0022] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0023] The first aspect of the present invention provides a modified polysiloxane, wherein the modified polysiloxane comprises: a plurality of polysiloxane macromolecular chains and a plurality of connecting groups connecting different polysiloxane macromolecular chains, wherein the connecting groups have a structure as shown in formula (1),

[0024]

[0025] Among them, * is the position of bonding with Si contained in different polysiloxane macromolecular chains, R 1 and R 2Each is independently selected from C1-C3 alkylene.

[0026] The modified polysiloxane of the present invention has the ability to increase the viscosity of supercritical CO2 fluid. The chemical composition and structure of the modified polysiloxane of the present invention can be schematically illustrated as follows, N is the number of schematic structural units. Different polysiloxane macromolecular chains may have different numbers of structural units. The spatial network structure formed by multiple polysiloxane macromolecular chains and multiple connecting groups connecting different polysiloxane macromolecular chains increases the bond energy between carbon dioxide molecules and thickeners in the three-dimensional space, and enhances the ability of the thickener to dissolve CO2.

[0027] The modified polysiloxane provided by the present invention has a -C-Si- bond, which is derived from the covalent bond formed by the C marked with * in formula (1) and the Si contained in the polysiloxane macromolecular chain, and can realize a three-dimensional network structure composed of multiple polysiloxane macromolecular chains and multiple connecting groups connecting different polysiloxane macromolecular chains. This structure can also be characterized and determined by infrared spectroscopy.

[0028] In the present invention, a CO2-philic short chain, i.e., the structure shown in formula (1), is introduced between polysiloxane macromolecular chains to form a spatial network structure, which can not only improve the interaction between modified polysiloxane molecules and increase the viscosity of the modified polysiloxane solution, but also ensure sufficient modified polysiloxane-CO2 interaction and enhance the solubility in CO2.

[0029] According to the present invention, the weight ratio of the polysiloxane macromolecular chain to the connecting group is 1-2:1.

[0030] According to the present invention, the polysiloxane macromolecular chain has a structural unit represented by formula (2):

[0031]

[0032] Wherein, R' and R" are end-capping groups, R1, R2, R3 and R4 are each independently selected from at least one of a C1-C3 alkyl group and a hydrogen group, and the end-capping groups R' and R" are each independently selected from at least one of a hydrogen group and a C1-C3 alkyl group.

[0033] According to the present invention, the weight average molecular weight of the modified polysiloxane is 16000-18000 g / mol.

[0034] The second aspect of the present invention provides a method for preparing a modified polysiloxane, wherein the preparation method comprises the steps of:

[0035] (1) subjecting cyclic siloxane and chain siloxane to a polymerization reaction under the action of a first catalyst to obtain an intermediate product;

[0036] (2) subjecting the intermediate product to a hydrosilylation reaction with a monomer represented by formula (3) under the action of a second catalyst to obtain a modified polysiloxane;

[0037]

[0038] In formula (3), R 1 and R 2 Each is independently selected from at least one of C1-C3 alkylene groups.

[0039] In the present invention, the Si-O bond of the cyclic siloxane is broken under the action of the first catalyst, and after the ring opening, a covalent bond is formed with Si in the chain siloxane to generate a polysiloxane macromolecular chain of the structure shown in formula (2); under the action of the second catalyst, the C=C double bond in the monomer of the structure shown in formula (3) is opened, and a covalent bond is formed with Si contained in the polysiloxane macromolecular chain, so that a three-dimensional network structure composed of multiple polysiloxane macromolecular chains and multiple connecting groups connecting different polysiloxane macromolecular chains can be realized, thereby obtaining a modified polysiloxane.

[0040] In the present invention, step (1) further comprises a solvent, wherein the solvent is selected from at least one of toluene and ethylene glycol dimethyl ether.

[0041] According to the present invention, the cyclic siloxane in step (1) is selected from the general formula C 2n H 6n O n Si n The compound shown, wherein n≥8, preferably octamethylcyclotetrasiloxane;

[0042] According to the present invention, the chain siloxane in step (1) is selected from at least one of 1,1,3,3-tetramethyldisiloxane, 1,1,3,3-tetraethyldisiloxane, 1,1,3,3-tetrapropyldisiloxane and 1,3-dichlorotetramethyldisiloxane, preferably 1,1,3,3-tetramethyldisiloxane.

[0043] According to the present invention, the mass ratio of the cyclic siloxane to the chain siloxane is 8-16:1, preferably 10-15:1.

[0044] In the present invention, two types of siloxanes, cyclic siloxane and chain siloxane, are first subjected to a ring-opening polymerization reaction to obtain a polysiloxane macromolecular chain having a structure represented by formula (2), which is conducive to the subsequent introduction of CO2-philic short chains. The preparation of modified polysiloxane can avoid the occurrence of high polymerization conditions, so that the polymer generated by the reaction is in a highly dispersed state. Moreover, the stability of this dispersed system is very good, thereby improving the viscosity capacity of the supercritical CO2 fluid.

[0045] According to the present invention, the monomer shown in formula (3) is selected from at least one of diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and ethylene glycol dimethacrylate, preferably diethylene glycol dimethacrylate. Diethylene glycol dimethacrylate has good CO2 solubility and is soluble in a variety of organic solvents. It can be bonded to the polysiloxane macromolecular chain and, when used as a thickener for supercritical CO2 fracturing fluid, it forms a Lewis acid-base pair with CO2, thereby forming a network structure with a certain strength between CO2 and the thickener, which allows the modified polysiloxane to maintain good chain flexibility under high temperature and high pressure, and also increases the bond energy between the carbon dioxide molecules and the thickener in the three-dimensional space, thereby enhancing the thickener's ability to dissolve CO2.

[0046] According to the present invention, the mass ratio of the intermediate product to the monomer represented by formula (3) is 2.5-3.5:1, preferably 2.8-3.3:1.

[0047] According to the present invention, the first catalyst is selected from at least one of tetramethylammonium hydroxide and potassium hydroxide. Preferably, the mass ratio of the first catalyst to the cyclic siloxane is 0.00050-0.00060:1; the second catalyst is at least one of chloroplatinic acid and tetrakis(triphenylphosphine)palladium. Preferably, the mass ratio of the second catalyst to the intermediate product is 0.000015-0.000020:1.

[0048] According to the present invention, in the preparation method, the conditions of the polymerization reaction include: a reaction temperature of 100-120° C. and a reaction time of 6-10 hours, preferably, a reaction temperature of 110° C. and a reaction time of 8 hours.

[0049] According to the present invention, in the preparation method, the conditions of the hydrosilylation reaction include: a reaction temperature of 90-100° C. and a reaction time of 3-5 hours, preferably, a reaction temperature of 97° C. and a reaction time of 4 hours.

[0050] In the present invention, the preparation method further comprises removing the solvent, the first catalyst and the low molecular weight compound after the reaction in step (1) is completed. This is because the presence of the solvent and the low molecular weight compound will affect the polymerization mode and degree of polymerization in the second step, and the molecular weight will not meet the requirements, and its performance will also be reduced accordingly. The reaction conditions for removing the solvent and the first catalyst are: temperature 130°C, time 2 hours; the reaction conditions for removing the low molecular weight compound are: temperature 145°C, vacuum drying for 2 hours.

[0051] In the present invention, in the preparation method, in step (2), the intermediate product and the initiator are mixed evenly, and then the second catalyst is added, wherein the mixing conditions are a temperature of 82° C., a rotation speed of 500 r / min, and a stirring time of 25 min.

[0052] In the present invention, the preparation method, after the hydrosilation reaction in step (2) is completed, in order to improve the purity of the product, further comprises filtering and separating to remove the second catalyst, and vacuum distilling to remove small molecular compounds and low boiling point impurities.

[0053] The third aspect of the present invention provides a modified polysiloxane prepared by the preparation method of the present invention.

[0054] A fourth aspect of the present invention provides an application of the modified polysiloxane of the present invention in supercritical CO2 fracturing.

[0055] A fifth aspect of the present invention provides a supercritical CO2 fracturing fluid, wherein the fracturing fluid comprises the aforementioned modified polysiloxane as a thickener.

[0056] The supercritical CO2 fracturing fluid provided by the present invention has a volume ratio of toluene to modified polysiloxane of 1:1-6:1. The addition of toluene can effectively improve the solubility of modified polysiloxane in liquid CO2. Due to similar polarity, toluene and modified polysiloxane molecules interact with each other. In addition, there is a CH...O bond between CO2 and toluene molecules, and CO2 also forms a Lewis acid-base pair, which is combined with the branched CO2-philic group, that is, the structure shown in formula (1). These interactions jointly construct a three-dimensional network structure of modified polysiloxane-CO2.

[0057] The present invention will be described in detail below through examples.

[0058] Example 1

[0059] Step 1: Add 10 mL of toluene (mass fraction 99.8%) solution into a three-necked flask, then add 43.5 g of octamethylcyclotetrasiloxane, 3.6 g of 1,1,3,3-tetramethyldisiloxane, and then add 0.025 g of tetramethylammonium hydroxide, stir and heat to 110° C. to carry out ring-opening polymerization reaction for 8 hours;

[0060] Step 2: After the reaction is completed, a condenser and a collecting bottle are added to the three-necked flask, and the temperature is continued to be raised to 130° C. and maintained for 2 hours to remove toluene and tetramethylammonium hydroxide; then the temperature is continued to be raised to 145° C. and vacuum dried for 2 hours to remove low molecular weight compounds to obtain an intermediate product;

[0061] Step 3, pour 20g of the intermediate product and 6.5g of diethylene glycol dimethacrylate (mass fraction 95%) into a three-necked flask, heat to 82°C, adjust the rotation speed to 500r / min, and stir for 25min; drop 0.00035g of chloroplatinic acid (mass fraction 8%) as a catalyst, and raise the system temperature to 97°C, react for 4 hours, filter and separate the chloroplatinic acid, and vacuum distill to remove small molecular compounds and low-boiling impurities, and cool to room temperature to obtain the supercritical CO2 thickener product of the present invention.

[0062] The thickening effect of the modified polysiloxane thickener system prepared in Example 1 of the present invention after mixing with supercritical CO2 was tested using a HAAKE Viscotester iQ rheometer series high temperature and high pressure rheometer with a double-phase rotor. Figure 1 and Figure 2 shown.

[0063] Depend on Figure 1 It can be seen that when the thickener is added at 0.5%, the viscosity after shearing changes slightly, indicating that no effective three-dimensional network structure has been formed. When the thickener is added at more than 1.5%, the number of polymer molecular chains forming a tight network structure increases, which is manifested as a sudden increase in the consistency coefficient, indicating that the hydrogen bonds in the system grow exponentially, and the main chains will also entangle with each other to form a tight structure, and destroying these structures requires a lot of energy, which is difficult to destroy by shearing.

[0064] Depend on Figure 2 It can be seen that the apparent viscosity of the thickened CO2 fluid decreases in stages with increasing temperature. When the temperature is between 50℃-70℃, the viscosity decreases slightly at different pressures, ranging from 15.93% to 21.35%, and the higher the pressure, the smaller the decrease; but when the temperature is between 70-85℃, the viscosity decreases significantly, and compared with 70℃, the decrease at different pressures is between 39.51% and 46.26%, and the higher the pressure, the greater the decrease.

[0065] When the temperature is the same, the pressure of the thickener CO2 fluid is gradually increased, and the viscosity of the system gradually increases. When the temperature is within 70°C, the viscosity of the thickener CO2 fluid at 12MPa is 6% to 10% higher than that at 10MPa, and the viscosity change is not significant; when the pressure exceeds 12MPa, the viscosity of the system increases significantly, with a relative increase of 20%-32%; when the pressure increases to 18MPa, the viscosity can be increased by up to 40.12%, indicating that the new silicone thickener has a more significant viscosity-increasing effect under high pressure.

[0066] Example 2

[0067] The changes of crude oil inside the core are characterized by nuclear magnetic resonance technology, and the oil displacement effects of the siloxane polymer and the modified polysiloxane thickener system synthesized by the present invention in the core are compared, comprising the following steps:

[0068] S1. After measuring the dry weight, length and diameter of two parallel core samples, the cores are cracked, split and filled with sand;

[0069] S2, dry and vacuum the two parallel core samples for 12 hours, then inject the formation crude oil, pressurize and saturate for 12 hours, take out the cores for nuclear magnetic resonance testing, and obtain the saturated oil T2 spectrum; measure the wet weight of the cores and calculate the saturated oil volume;

[0070] S3. Place two parallel core samples of saturated crude oil into a core holder, connect the confining pressure loading device, open the thermostat, start the displacement pump, and pressurize and inject the same amount of supercritical CO2+siloxane polymer and supercritical CO2+modified polysiloxane thickener respectively;

[0071] S4, close the injection pump and valve to put the entire core in a "well-simmering" state;

[0072] S5. After a period of "well soaking", flowback is carried out, and the flowback pressure decreases by 5MPa / min, and the amount of liquid discharged is measured;

[0073] S6. After the experiment, the core is placed in a nuclear magnetic resonance device for experiment to test the distribution of crude oil in different pore sizes, so as to analyze the utilization degree of crude oil in the matrix-fracture and calculate the recovery factor;

[0074] The recovery factor is calculated as:

[0075]

[0076] Where R is the recovery factor, dimensionless; T o is the total signal amount under saturated oil state, dimensionless; Tr is the total signal amount after the experiment, dimensionless.

[0077] The results are as follows Figure 3 and Figure 4 From the NMR curves, the pore structure and pore distribution range of the two cores are consistent, and they can be used as parallel core samples for comparative analysis. The right peak near 1μm is the fracture pore, while the left peak is the core matrix pore.

[0078] By comparing the signal changes within the NMR T2 relaxation time, the changes in crude oil in the matrix pores and fracture pores can be quantitatively characterized. The extent of crude oil production in the core by different CO2 thickeners is shown in Table 1:

[0079] Table 1 Comparison of crude oil recovery efficiency of different thickeners in different pores

[0080] Oil recovery efficiency <![CDATA[CO2 + silicone polymer]]> <![CDATA[CO2+-modified polysiloxane thickener]]> Matrix pore utilization ratio / % 10.32 11.28 Fracture pore utilization ratio / % 18.38 29.65 Total oil recovery efficiency / % 28.70 40.93

[0081] It can be seen from the results in Table 1 that the use of the modified polysiloxane thickener of the present invention can not only greatly improve the oil displacement efficiency in the fracture pores, but also improve the degree of crude oil mobilization in the matrix pores. This shows that after entering the fracture pores, the CO2+modified polysiloxane thickener fluid can still maintain a good spatial network structure, expand the scope of action, allow CO2 to enter deeper and more pores, and have a more obvious oil displacement effect.

[0082] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A modified polysiloxane, It is characterized in that The modified polysiloxane comprises: a plurality of polysiloxane macromolecular chains and a plurality of connecting groups connecting different polysiloxane macromolecular chains, wherein the connecting groups have a structure as shown in formula (1), Among them, * is the position of bonding with Si contained in different polysiloxane macromolecular chains, R 1 and R 2 Each independently selected from C 1 -C 3 of alkylene.

2. The modified polysiloxane according to claim 1, It is characterized in that The weight ratio of the polysiloxane macromolecular chain to the connecting group is 1-2:

1.

3. The modified polysiloxane according to claim 1, It is characterized in that The polysiloxane macromolecular chain has a structural unit represented by formula (2): Wherein, R′ and R″ are end-capping groups, R 1 , R 2 , R 3 and R 4 Each independently selected from C 1 -C 3 At least one of an alkyl group or a hydrogen group.

4. The modified polysiloxane according to claim 3, It is characterized in that The end-capping groups R' and R" are each independently selected from hydrogen, C 1 -C 3 At least one of the alkyl groups.

5. The modified polysiloxane according to claim 1, It is characterized in that The weight average molecular weight of the modified polysiloxane is 16000-18000 g / mol.

6. A method for preparing modified polysiloxane, It is characterized in that The preparation method comprises the steps of: (1) subjecting cyclic siloxane and chain siloxane to a polymerization reaction under the action of a first catalyst to obtain an intermediate product; (2) subjecting the intermediate product to a hydrosilylation reaction with a monomer represented by formula (3) under the action of a second catalyst to obtain a modified polysiloxane; In formula (3), R 1 and R 2 Each independently selected from C 1 -C 3 At least one of the alkylene groups.

7. The preparation method according to claim 6, It is characterized in that The cyclic siloxane in step (1) is selected from the general formula C 2n H 6n O n Si n The compound shown, wherein n≥8, preferably octamethylcyclotetrasiloxane; And / or, the chain siloxane in step (1) is at least one selected from 1,1,3,3-tetramethyldisiloxane, 1,1,3,3-tetraethyldisiloxane, 1,1,3,3-tetrapropyldisiloxane, preferably 1,1,3,3-tetramethyldisiloxane.

8. The preparation method according to claim 6 or 7, It is characterized in that The mass ratio of the cyclic siloxane to the chain siloxane is 8-16:1, preferably 10-15:

1.

9. The preparation method according to any one of claims 6 to 8, It is characterized in that The monomer represented by formula (3) is at least one selected from diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and ethylene glycol dimethacrylate, preferably diethylene glycol dimethacrylate; Preferably, the mass ratio of the intermediate product to the monomer represented by formula (3) is 2.5-3.5:1, preferably 2.8-3.3:

1.

10. The preparation method according to any one of claims 6 to 9, It is characterized in that The first catalyst is selected from at least one of tetramethylammonium hydroxide and potassium hydroxide. Preferably, the mass ratio of the first catalyst to the cyclic siloxane is: 0.00050-0.00060:1; And / or, the second catalyst is at least one of chloroplatinic acid and tetrakis(triphenylphosphine)palladium. Preferably, the mass ratio of the second catalyst to the intermediate product is: 0.000015-0.000020:

1.

11. The preparation method according to any one of claims 6 to 10, It is characterized in that The polymerization reaction conditions include: reaction temperature of 100-120° C., reaction time of 6-10 hours, preferably, reaction temperature of 110° C., reaction time of 8 hours. And / or, the conditions of the hydrosilylation reaction include: reaction temperature of 90-100° C., reaction time of 3-5 hours, preferably, reaction temperature of 97° C., reaction time of 4 hours.

12. A modified polysiloxane obtained by the preparation method according to any one of claims 6 to 11.

13. A modified polysiloxane according to any one of claims 1 to 5 and 12 in supercritical CO 2 Application in fracturing.

14. A supercritical CO 2 Fracturing fluid, It is characterized in that The fracturing fluid comprises the modified polysiloxane according to any one of claims 1 to 5 and 12 as a thickener.