Flexible composite dielectric film material, preparation method and application thereof
By using SAZn particles in polyvinylidene fluoride materials to increase the content of polar beta phase crystals, the problems of material hygroscopicity and high loss are solved, and a flexible composite dielectric film material with high dielectric constant and low loss is achieved, which is suitable for high-temperature applications. frequency and high energy density applications, and simplifies the production process.
Patent Information
- Application Number
- CN202410827894.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-01
AI Technical Summary
The hygroscopicity of small organic molecules in existing polyvinylidene fluoride composite materials is too strong, resulting in large ion leakage, high material loss, low energy storage efficiency, and the process of increasing the dielectric constant is complex, high-cost, and difficult to process.
SAZn particles are used as wide bandgap coordination polymers, and flexible composite dielectric film materials are prepared by mixing polyvinylidene fluoride particles with N,N-dimethylformamide solution, adding SAZn particles and conducting ultrasonic dispersion. Increase the polar beta phase crystal content of PVDF, reduce the dielectric loss of the material and increase the energy storage density.
The dielectric constant is significantly increased, the dielectric loss is reduced, the energy storage density and efficiency are improved, and the material shows good stability under high-frequency electric fields and high temperatures. It is suitable for embedded capacitors and pulse power devices, and the process is simple and cycle-friendly. Short, suitable for mass production.
Smart Images

Figure CN118725366A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a flexible composite dielectric film material, a preparation method and an application thereof. Background Art
[0002] With the rapid development of new energy and modern electronic industries, capacitors are increasingly showing their important position in many fields such as smart grids, hybrid vehicles, electronic equipment, wind power conversion devices, etc. The development of new dielectric materials has become an important development field in the electronic power materials industry. Polymer film dielectric materials are widely used due to their light weight, flexibility, excellent mechanical properties, high dielectric breakdown strength, low dielectric loss and good processing performance, such as the commercialized biaxially oriented polypropylene (BOPP) dielectric film capacitors. However, since BOPP's long-term working conditions are mostly 150kV / mm and below electric fields, and the energy storage density of BOPP polymer film dielectrics is only 1-2J / cm 3 , due to its low dielectric constant of 2.1-2.2. Therefore, it cannot meet the needs of capacitors to develop in the direction of high energy storage and miniaturization. Research on new thin and light high dielectric constant dielectric materials has become an important development field in the electronic power materials industry.
[0003] At present, the development of most high dielectric constant polymer composite dielectric materials focuses on inorganic composite polymer dielectric materials based on interface polarization enhancement and percolation theory and all-organic polymer dielectric materials based on dipole orientation polarization enhancement. Existing inorganic composite polymer dielectric materials include high dielectric constant ceramic particle-polymer composite materials and conductive metal particle-polymer percolation composite materials. For example, Liu Xiaolin (J Adv Phys, 2015; 4(4):357) prepared a three-phase composite Ni@p-BaTiO 3 / PVDF material, the highest dielectric constant reaches 20.1, which is comparable to p-BaTiO 3 / PVDF composite materials increased by 78%. Although the apparent dielectric constant of this type of high-dielectric ceramic particle-polymer composite dielectric material has increased by several times to dozens of times, the dielectric loss has also increased significantly compared to pure polymers, and the relatively high amount of inorganic doping has also affected the processing performance of the material. Zhang et al. (ACS Appl Mater Interfaces 2017; 9: 10106) studied the leakage current characteristics of conductive metal particle-polymer nano-percolation composite materials filled with PP nano-aluminum particles (18 and 100nm) under high fields, and found that the bulk conductivity of the composite material increased with the electric field strength. When the electric field was higher than 35MV / m, the Fowler-Nordheim field electron emission effect appeared, and electrons were excited from the metal nanoparticles into the polymer matrix to form the entire nanoparticle composite conductive material. This type of conductive metal particle-polymer nanocomposite material is generally not suitable for high energy density capacitor applications, but is more suitable for electronic switches.
[0004] For existing all-organic polymer dielectric materials based on dipole orientation polarization enhancement, developers have adopted a design strategy of adding polar groups to the polymer main chain or side groups to increase the internal dipole moment and enhance the orientation polarization of the molecular chain to obtain all-organic polymer dielectric materials with high dielectric constant and high energy storage density. For example, Zhang et al. (Mater. Horiz. 2020; 7:592) used sulfone groups to modify high-temperature polymer polyphenylene ether (PPO) to obtain a modified polymer with a dielectric constant of up to 7.0, a breakdown field strength of more than 800 MV / m, and an energy storage density of 20 J / cm at room temperature. 3 . However, although the dipole moment of the side group makes a great contribution to the improvement of the dielectric constant, the potential hygroscopicity of the polar polymer leads to the formation of a non-ionic double layer, which can cause electrochemical degradation of the polymer under high local electric fields. At the same time, these dipole-modified polymers are difficult to process into high-quality capacitor films. The operating electric field frequency of the above two types of polymer-based dielectric materials is generally lower than 10KHz, and there is a more serious dielectric relaxation phenomenon under higher frequency electric fields, which leads to serious heating of the composite materials, a significant increase in dielectric loss and a decrease in energy storage efficiency.
[0005] Polyvinylidene fluoride (PVDF) is a semi-crystalline polymer with excellent dielectric properties, low material processing temperature, low melt viscosity, and easy processing and molding, so it has become the first choice for polymer composite matrix. Among them, because all F atoms in polar β-phase PVDF are arranged on the same side of the molecular chain, PVDF has spontaneous polarization properties, such as adding nucleating agents or oriented stretching to obtain PVDF materials with high β-crystalline content. Chinese patent application (application number: 201210372386.X) and Chinese patent application (application number: 201710378379.3) respectively disclose a polyvinylidene fluoride composite material with high polar content obtained by hexadecyltrimethylammonium bromide (CATB) and 1-butyl-3-methylimidazolium hexafluorophosphate (BMIMPF6) and its preparation method. However, the small molecular organic matter doped in these methods is too hygroscopic and has large ion leakage conduction, which leads to a high loss value of the final material. High loss not only reduces the dielectric energy storage efficiency, but also can be converted into heat to destroy the dielectric and make it ineffective.
[0006] Existing technologies for improving the dielectric constant of polymer-based composite film materials still have problems such as complex processes, high costs, difficult processing, and large dielectric loss of materials. Summary of the invention
[0007] The present invention provides a flexible composite dielectric film material, a preparation method and an application thereof, in order to solve the problems that the small molecule organic matter doped in the polyvinylidene fluoride composite material has strong hygroscopicity and large ion leakage conduction, resulting in high loss of the final material, thermal damage caused by low energy storage efficiency, and dielectric failure, and the existing technology for improving the dielectric constant of the polymer-based composite film material still has the problems of complex process, high cost and difficult processing.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0009] A method for preparing a flexible composite dielectric film material comprises the following steps:
[0010] (1) drying the polyvinylidene fluoride particles for use;
[0011] (2) adding polyvinylidene fluoride particles into N,N-dimethylformamide solution and stirring to completely dissolve the particles to obtain a uniform solution;
[0012] (3) adding SAZn particles to the uniform solution obtained in step (2), and then stirring to dissolve to obtain a mixed solution;
[0013] (4) ultrasonically dispersing the mixed solution obtained in step (3) to obtain a uniformly mixed glue solution;
[0014] (5) The glue obtained in step (4) is cast into a mold, and then placed in an oven for drying to obtain a flexible composite dielectric film material.
[0015] Furthermore, the drying temperature of the polyvinylidene fluoride particles in step (1) is 50-100°C.
[0016] Furthermore, the concentration of polyvinylidene fluoride in the uniform solution in step (2) is 1-20 wt %.
[0017] Furthermore, the complete dissolution time of the polyvinylidene fluoride particles and the N,N-dimethylformamide solution in step (2) is 3 hours.
[0018] Furthermore, the weight percentage of the SAZn particles described in step (3) and the polyvinylidene fluoride particles described in step (2) is 0.5-7.5wt%.
[0019] Furthermore, the temperature for stirring and dissolving in step (3) is 30-60°C.
[0020] Furthermore, the stirring time in step (3) is 1-5h.
[0021] Furthermore, the mixed solution in step (4) is subjected to ultrasonic dispersion for 1-4 hours.
[0022] Furthermore, the thickness of the composite film described in step (5) is 5-30 μm.
[0023] The present invention also provides an application of a flexible composite dielectric film material, which is applied to one or more fields including smart grids, hybrid vehicles, electronic equipment, and wind power conversion devices.
[0024] Compared with the prior art, the present invention has the following technical advantages:
[0025] (1) The flexible composite dielectric film material provided by the present invention makes full use of the inductive effect of wide bandgap coordination polymers to increase the polar β-phase crystal content of PVDF, thereby increasing the dielectric constant of the material.
[0026] (2) The coordination polymer SAZn of the present invention is not hygroscopic. Compared with the Chinese patent application (application number: 201210372386.X) and the Chinese patent application (application number: 201710378379.3), the composite membrane will not produce ion leakage, resulting in membrane breakdown under high electric field.
[0027] (3) The flexible composite dielectric film material provided by the present invention only needs to add 5.0% filler by mass. At 1MHz and 180℃, the dielectric constant reaches 21.5, which is 1.9 times that of pure PVDF film under the same conditions. The dielectric loss of the flexible composite dielectric film material is only 0.19. Its discharge energy density and charge and discharge energy efficiency are increased by 188% and 158% respectively compared with pure PVDF film. However, the method using ceramics and nano-metal particles usually requires adding filler by mass ratio of more than 10% to show significant effect.
[0028] (4) The wide bandgap coordination polymer of the present invention can act as a deep trap effect to capture space charges in flexible composite dielectric thin film materials, thereby reducing the conductivity of the thin film material. Compared with the interface polarization mechanism of current ceramic and metal particle fillers, it can be applied to higher electric field conditions.
[0029] (5) The dielectric constant of the flexible composite dielectric film material provided by the present invention is significantly improved, while the dielectric loss is very low, and it has good frequency and temperature stability, and can be used in embedded capacitors, pulse power devices and power energy storage.
[0030] (6) The method for preparing the flexible composite dielectric film material provided by the present invention has a simple process flow, a short preparation cycle, a high product yield, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is the structural diagram of the SAZn complex (all H atoms in the structural formula are omitted for simplicity);
[0032] Figure 2 This is a physical picture of the appearance of the 5.0-SAZn-PVDF film made with SAZn as filler;
[0033] Figure 3 The infrared spectra of SAZn and flexible composite dielectric film materials with different SAZn mass ratios;
[0034] Figure 4 The (a) dielectric constant and (b) dielectric loss of flexible composite dielectric film materials with different SAZn mass ratios at room temperature vary with the logarithm of frequency;
[0035] Figure 5 DE hysteresis loop diagram of pure PVDF and flexible composite dielectric film materials with different SAZn mass ratios under 500MV / m electric field. DETAILED DESCRIPTION
[0036] To further explain the technical means and effects of the present invention, the technical solution of the present invention is further described below in conjunction with the embodiments of the present invention, but the present invention is not limited to the scope of the embodiments.
[0037] In an embodiment of the present invention, a method for preparing a flexible composite dielectric film material comprises the following steps:
[0038] (1) drying the polyvinylidene fluoride particles for use;
[0039] (2) adding polyvinylidene fluoride particles into N,N-dimethylformamide solution and stirring to completely dissolve the particles to obtain a uniform solution;
[0040] (3) adding SAZn particles to the uniform solution obtained in step (2), and then stirring to dissolve to obtain a mixed solution;
[0041] (4) ultrasonically dispersing the mixed solution obtained in step (3) to obtain a uniformly mixed glue solution;
[0042] (5) The glue obtained in step (4) is cast into a mold, and then placed in an oven for drying to obtain a flexible composite dielectric film material.
[0043] Preparation of SAZn filler: The complex SAZn is prepared using 3,5-di-tert-butylhydroxybenzoic acid as a ligand and a zinc compound as a zinc-adding agent for the coordination metal. The complex is obtained by using Example 1 of the Chinese patent application "A nanomaterial of a zinc complex containing a substituent, a preparation method and its application (application number: 202310199576.4)". The crystal structure of the complex is as follows Figure 1 .
[0044] In order to make the disclosure of the present invention more complete, it is described below through more specific embodiments.
[0045] Example 1
[0046] (1) drying the polyvinylidene fluoride particles at 50-100° C. for use;
[0047] (2) Weigh 3 g of polyvinylidene fluoride particles and add them to 40 mL of N,N-dimethylformamide solution, stirring for 3 h to completely dissolve them to obtain a uniform solution;
[0048] (3) Weighing 0.15 g of SAZn particles, adding them to the uniform solution obtained in step (2), and continuing to stir on a magnetic stirrer for 2 h to obtain a mixed solution;
[0049] (4) The mixed solution obtained in step (3) is further subjected to ultrasonic dispersion for 2 hours to obtain a uniformly mixed transparent adhesive solution.
[0050] (5) 0.5 mL of the glue obtained in step (4) was cast into a polytetrafluoroethylene mold and placed in a 60° C. oven for drying for 24 h to ensure that the solvent was completely removed. Finally, a 10 μm thick transparent flexible composite dielectric film material 5.0-SAZn-PVDF was obtained. The appearance of the material is as follows: Figure 2 As shown in the figure, at room temperature and 1KHz, the dielectric constant is 19.7, the dielectric loss is 0.043; at 500MV / m, the energy storage density is 4.43J / cm 3 , the energy storage efficiency reaches 56.54%.
[0051] Example 2
[0052] The operation steps are basically the same as those in Example 1, except that 0.015 g of SAZn particles are used. The resulting flexible composite dielectric film material is 0.5-SAZn-PVDF. The dielectric constant is 13.70 and the dielectric loss is 0.030 at room temperature and 1 KHz. The energy storage density is 2.64 J / cm 3 , the energy storage efficiency reaches 46.01%.
[0053] Example 3
[0054] The operation steps are basically the same as those in Example 1, except that 0.075 g of SAZn particles are used. The resulting flexible composite dielectric film material is 2.5-SAZn-PVDF. The dielectric constant is 15.8 and the dielectric loss is 0.038 at room temperature and 1 KHz. The energy storage density is 3.92 J / cm 3 , the energy storage efficiency reaches 52.89%.
[0055] Example 4
[0056] The operation steps are basically the same as those in Example 1, except that 0.225 g of SAZn particles are used. The resulting flexible composite dielectric film material is 7.5-SAZn-PVDF. The dielectric constant is 12.40 and the dielectric loss is 0.049 at room temperature and 1 KHz. The energy storage density is 2.13 J / cm 3 , the energy storage efficiency reaches 57%.
[0057] Example 5
[0058] The operation steps are basically the same as those in Example 1, except that step (3) is not performed. The obtained membrane material is a pure PVDF membrane, and the dielectric constant at 1KHz at room temperature is 11.0, and the dielectric loss is 0.028; under the condition of 500MV / m, the energy storage density is 1.77J / cm 3 , the energy storage efficiency reaches 45.10%.
[0059] Example 6
[0060] The operation steps are basically the same as those in Example 1, except that the thickness of the composite film is 5 μm. The dielectric constant of the obtained flexible composite dielectric film material at room temperature and 1 KHz is 20.80, and the dielectric loss is 0.038; under 600 MV / m, the energy storage density is 6.97 J / cm 3 , the energy storage efficiency reaches 69%.
[0061] Example 7
[0062] The operation steps are basically the same as those in Example 1, except that the thickness of the composite film is 20 μm. The dielectric constant of the obtained flexible composite dielectric film material at room temperature and 1 KHz is 20.00, and the dielectric loss is 0.042; under the condition of 400 MV / m, the energy storage density is 4.04 J / cm 3 , the energy storage efficiency reaches 45.0%.
[0063] Example 8
[0064] The operation steps are basically the same as those in Example 1, except that the thickness of the composite film is 30 μm. The dielectric constant of the obtained flexible composite dielectric film material at room temperature and 1 KHz is 20.10, the dielectric loss is 0.040; under 300 MV / m, the energy storage density is 3.10 J / cm 3 , the energy storage efficiency reaches 40%.
[0065] The performance of the flexible composite dielectric film material obtained in the above experiment was tested. The dielectric constant and dielectric loss were measured using a Tonghui TH2839 impedance analyzer, and the energy storage density and energy storage efficiency were measured using a PK-FERRO20B ferroelectric analyzer. The performance of the film material obtained in Examples 1-5 was tested. The experimental results are shown in Table 1. Figure 3-5 As shown:
[0066] Table 1 Test results of membrane material properties of Examples 1-5
[0067]
[0068]
[0069] Depend on Figure 3As shown in the figure, with the increase of the amount of SAZn added, the infrared peak intensity corresponding to the polarity β of the flexible composite dielectric film material becomes stronger and stronger, and reaches the maximum when the mass ratio of SAZn is 5.0%. After that, the peak intensity corresponding to the polarity β of the flexible composite dielectric film material with a mass ratio of 7.5% obtained by continuing to add SAZn is less than that of the flexible composite dielectric film material with a mass ratio of 5.0%. The dielectric constant of the material also decreases.
[0070] From Table 1 and Figure 4 , 5 As shown, with the increase of SAZn content in the flexible composite dielectric film material, the energy storage density of the flexible composite dielectric film material gradually increases. When the mass ratio of SAZn in the flexible composite dielectric film material is 5.0%, the energy storage density of the flexible composite dielectric film material is at an optimal value.
[0071] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a flexible composite dielectric film material, characterized in that: The following steps are involved: (1) drying the polyvinylidene fluoride particles for use; (2) adding polyvinylidene fluoride particles into N,N-dimethylformamide solution and stirring to completely dissolve the particles to obtain a uniform solution; (3) adding SAZn particles to the uniform solution obtained in step (2), and then stirring to dissolve to obtain a mixed solution; (4) ultrasonically dispersing the mixed solution obtained in step (3) to obtain a uniformly mixed glue solution; (5) The glue obtained in step (4) is cast into a mold, and then placed in an oven for drying to obtain a flexible composite dielectric film material.
2. The method for preparing a flexible composite dielectric film material according to claim 1, characterized in that: The concentration of polyvinylidene fluoride in the uniform solution in step (2) is 1-20 wt %.
3. The method for preparing the flexible composite dielectric film material according to claim 1, characterized in that: The complete dissolution time of the polyvinylidene fluoride particles and N,N-dimethylformamide solution described in step (2) is 3 hours.
4. The method for preparing a flexible composite dielectric film material according to claim 1, characterized in that: The weight percentage of the SAZn particles described in step (3) and the polyvinylidene fluoride particles described in step (2) is 0.5-7.5wt%.
5. The method for preparing a flexible composite dielectric film material according to claim 1, characterized in that: The temperature for stirring and dissolving in step (3) is 30-60°C.
6. The method for preparing a flexible composite dielectric film material according to claim 1, characterized in that: The stirring time in step (3) is 1-5h.
7. The method for preparing a flexible composite dielectric film material according to claim 1, characterized in that: The mixed solution in step (4) is subjected to ultrasonic dispersion for 1-4 hours.
8. The method for preparing the flexible composite dielectric film material according to claim 1, characterized in that: The thickness of the film prepared in step (5) is 5-30 μm.
9. A flexible composite dielectric thin film material prepared according to the method according to any one of claims 1 to 8.
10. An application of the flexible composite dielectric film material according to claim 9, characterized in that: It is applied in one or more fields including smart grid, hybrid electric vehicle, electronic equipment and wind power conversion device.