Preparation method and application of bio-based closed-loop recyclable bionic gas gel
By constructing a bio-based dynamic reversible imine bond cross-linking network and directional freeze-drying technology, a closed-loop recyclable bionic aerogel with multi-functional properties was prepared, which solved the problems of polymer aerogels in sustainable development and recycling and reprocessing. challenge, achieving efficient chemical recovery and multifunctional performance.
Patent Information
- Application Number
- CN202410929202.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
AI Technical Summary
Existing polymer aerogels have challenges in terms of sustainable development and recycling and reprocessing. Their performance cannot meet the needs of multiple bionic structures and multi-functions, and their recycling and reprocessing performance is immature.
Bio-based raw materials are used to construct a dynamic reversible imine bond cross-linked network, and the structure is controlled by directional freeze-drying technology to prepare a bionic aerogel with ultra-fast degradation and closed-loop chemical recovery capabilities. It combines multi-level roughness structure and pore structure to achieve hydrophobic, Flame retardant and multifunctional properties.
The prepared bio-based closed-loop recyclable aerogel has excellent mechanics, thermal insulation, hydrophobic and lipophilic properties, and can realize full material reuse and reprocessing in the degradation solution. It is suitable for a variety of application scenarios, such as oil-water separation. and phase change energy storage.
Smart Images

Figure CN118725397A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional materials, and in particular relates to a preparation method of a bio-based closed-loop recyclable biomimetic aerogel and an application thereof. Background Art
[0002] Polymer aerogels have attracted widespread attention due to their unique low density, high porosity, and good thermal insulation properties. These properties make them have important application potential in aerospace, energy storage and conversion, biomedicine, sensors, waste adsorption and filtration, artificial intelligence, building insulation and shock absorption, etc. However, as the world's energy, resources and environment face huge challenges, the traditional petroleum-based polymer industry must cope with the urgent demand for large amounts of energy and resources, which is a severe test. There are currently two directions to address this concern: (1) synthesizing polymers from renewable resources; (2) developing recyclable polymers to reduce waste.
[0003] The synthesis of polymer aerogels from renewable resources provides a viable solution to the depletion of fossil fuels and the growing environmental threats. Biomass resources and materials mainly come from plants, animals and marine organisms, including cellulose, hemicellulose, polysaccharides, proteins, peptides and other types of biopolymers. Due to the unique properties of bio-based materials such as high biocompatibility, good biodegradability and easy modification, more and more literature focuses on the preparation routes and applications of various functional nanomaterials based on biomass precursors, including 1D nanofibers, 2D membranes, films and sheets, and 3D structured biomass-based hydrogels and aerogel materials. In addition, by optimizing the synthesis strategy of aerogels, the physical properties of aerogels such as specific surface area, porosity, mechanical strength and conductivity can be adjusted. Alternatively, by coupling with other functional nanoscale building blocks (such as nanoparticles, quantum dots (QDs), CNTs, graphene, etc.), biomass-based hybrid aerogels with improved physical and chemical properties and functions can be obtained. Bio-based aerogel not only inherits the light weight, high strength and excellent thermal insulation properties of polymer aerogel, but also greatly reduces the burden on the environment due to its renewable and biodegradable raw materials, which is in line with the current pursuit of sustainable development and green materials.
[0004] Recycling and reuse are another effective way to reduce fossil resource consumption and environmental pollution and reduce waste. The current recycling process mainly relies on primary recycling and secondary (mechanical) recycling. The former can also be called closed-loop recycling, which refers to the reprocessing of uncontaminated single polymers to produce products with unchanged uses), while the latter is usually called "downgraded recycling", which can provide low-value materials with different uses from the original materials. However, the recovery rate of polymer waste for recycling is usually very low, which shows that there is still a lot of research space and development potential for recyclable polymers. Chemically recyclable polymers can return to the corresponding monomers during the depolymerization process, repolymerize into polymers of original quality, or be converted into higher value or higher value-added materials during the upcycling or reuse process. Therefore, this depolymerization and chemical recycling or upcycling process can reduce the demand for limited raw materials and minimize the negative impact on the environment.
[0005] Dynamic covalent cross-linked networks have been widely used in polymer composites for recycling and self-repair after mechanical damage. The intrinsic mechanism is that they can reintegrate the robustness of covalent bonds and the intrinsic reversibility of non-covalent physical interactions. The strategy of constructing dynamic covalent networks provides a new idea for the recycling of polymer aerogels, and it comes with the unique property of reversible repair. At present, various reversible reactions are used to form dynamic covalent networks, including Diels-Alder (DA) reaction, olefin metathesis, free radical recombination, etc. In addition, dynamic covalent bonds are also widely used to generate covalent networks, such as lipid bond exchange, disulfide bond exchange, Schiff base (amino and aldehyde groups) and imine-type bonds (imine, acylhydrazone, hydrazone, etc.). Among them, Schiff base bonds are well-known dynamic covalent bonds in the formation of reversible cross-linked polymers due to their advantages such as high controllability, mild reaction and reaction flexibility.
[0006] After determining the basic unit, the structure of the aerogel needs to be constructed. One of the current research hotspots is to seek natural design inspiration to construct high-performance multifunctional biomimetic aerogels. For example, the stems of trees and vascular plants present anisotropic porous structures, and their longitudinal channels are conducive to the directional and rapid transmission of water and nutrients. In addition, the well-known lotus effect is inspired by the superhydrophobic properties caused by the multi-level surface protrusions on the surface of the lotus leaf. A thorough analysis of the special structure of natural organisms and a deep understanding of the relationship between structure and function will help the design of multifunctional aerogels. To this end, many processing methods have been proposed, including three-dimensional (3D) printing, hydrogel casting, and electrophoretic deposition, to develop bio-inspired functional materials with different structures. However, most of these methods are complex, time-consuming, and labor-intensive, which is not conducive to the production of actual materials. Using directional freeze-drying technology based on traditional freeze-drying to regulate structural orientation and construct porous 3D anisotropic polymer-based materials has many advantages. On the one hand, the orderly arrangement and assembly of the porous structure brought about by this technology can improve the structural stability of the material. On the other hand, the special anisotropic structure will also give the material anisotropic properties and rapid directional transmission of electricity, heat and magnetism, which is necessary in application scenarios such as oil-water separation, thermal insulation, electromagnetic interference shielding, and energy storage.
[0007] At present, there is little work on using bio-based raw materials to construct polymer aerogels with multiple biomimetic structures, and the performance is difficult to meet the requirements of various use environments. At the same time, there is no mature report on designing the cross-linked network of polymer aerogels on this basis to enable them to have multiple recycling and reprocessing properties. Therefore, it is very promising to develop a new type of bio-based, multifunctional aerogel with multiple biomimetic structures that can be recycled and reprocessed by multiple means. Summary of the invention
[0008] In view of the problems of sustainable development faced by current polymer aerogels, the present invention provides a method for preparing bio-based closed-loop recyclable biomimetic aerogel. The aerogel has excellent flame retardancy, good mechanical properties, chemical recycling and reprocessing, and excellent characteristics such as hydrophobicity and lipophilicity, which specifically solves many problems existing in current polymer aerogels.
[0009] The present invention uses bio-based raw materials to construct a high-performance aerogel network similar to plants in nature in terms of structure and green properties. The network uses biomass monomers to construct its basic cross-linking unit, and each monomer is cross-linked with a dynamically reversible imine bond. This rich reversible cross-linking point gives the aerogel ultra-fast degradation performance, and closed-loop chemical monomer recovery and reprocessing can be performed. Even, using a highly active reversible network, the reuse and reprocessing of all materials can be achieved in the degradation liquid. This green recycling and reprocessing feature is deeply in line with the sustainable development strategy. In addition, through directional auxiliary molding, the aerogel network prepared by the present invention has a bionic pore structure, which can achieve rapid liquid transmission against gravity, and its various properties, including mechanical properties, thermal insulation properties, etc., have distinctive anisotropy. At the same time, it has a multi-level roughness structure at the microscopic level, forming a super-hydrophobic property similar to the lotus leaf effect. In addition, the aerogel prepared by the present invention has excellent performance in various potential applications, such as oil-water separation, flame retardant, and phase change energy storage applications.
[0010] The method for preparing the bio-based closed-loop recyclable biomimetic aerogel of the present invention comprises the following steps: Step 1: Add vanillin and triethylamine to ethyl acetate solvent, add phosphorus oxychloride, react in an ice-water bath for a certain period of time, remove the ice bath, and continue to stir and react for a period of time; after the reaction is completed, pour the product into a sufficient amount of deionized water, continue to stir, and obtain a white solid product after filtration, which is recrystallized with ethanol and dried to obtain bio-based trialdehyde phosphate tris (4-formyl-2-methoxyphenyl) ester TMP.
[0011] In step 1, the molar ratio of vanillin to triethylamine is 1:1, and they are mixed and dissolved in a certain amount of ethyl acetate, and the mass fraction of the two in ethyl acetate is 30%-40%.
[0012] In step 1, the molar ratio of vanillin to phosphorus oxychloride is 3:1.
[0013] In step 1, after the system is reacted in an ice-water bath for 25-30 min, the ice-water bath is removed, and the reaction is continued at 25° C. with stirring for 22-26 h.
[0014] Step 2: Dissolve the TMP obtained in step 1 in dimethyl sulfoxide (DMSO) solution, add the diamine monomer in a certain proportion, stir until fully dissolved, and stir at room temperature for 2 h; then add a certain amount of tris(2-aminoethyl)amine (TAEA) to the system, stir for 30 s, and then ultrasonically vibrate for 1 min.
[0015] Step 3: The system of step 2 is quickly transferred to a mold, and allowed to stand at 50-80°C for 2 hours under closed conditions to allow gelation reaction to occur, followed by further aging at room temperature for 12-72 hours.
[0016] Step 4: Transfer the fully aged wet gel to a directional freezing device, use liquid nitrogen as the freezing source, and perform directional freezing for 30 minutes; then remove the sample from the mold and transfer it to the cold trap of the freeze dryer, set the temperature to -50°C, and perform the aging procedure again for 12 hours; then quickly transfer the sample to a sample tray, with a vacuum degree of less than 1 Pa, and dry for 72-120 hours; finally, transfer the obtained material to a vacuum oven and dry it at 70°C for 12 hours to obtain the target aerogel.
[0017] In step 2, the solid content of the reaction system ranges from 2% to 20%.
[0018] In step 2, the diamine monomer is selected from one or more of 1,4-bis(2-trifluoromethyl-4-aminophenoxy)benzene (p-6FAPB), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), diethylenetriamine, aliphatic linear diamines (1,8-octanediamine, 1,3-propylenediamine and 1,7-diaminoheptane, etc.), p-phenylenediamine, anthracene-2,6-diamine, 3,6-diaminocarbazole, 2,7-diaminofluorene, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfide, etc.
[0019] In step 2, the molar ratio of the diamine monomer to tris(2-aminoethyl)amine (TAEA) is 1:0, 4:1, 3:2, 1:1, 2:3, 1:4, 0:1, wherein the molar ratio of the structural units of the aldehyde group and the amine group is preferably 1:1.
[0020] The invention discloses an application of the bio-based closed-loop recyclable biomimetic gas gel in the preparation of thermal insulation materials.
[0021] The invention discloses an application of the bio-based closed-loop recyclable biomimetic aerogel in the preparation of oil-water separation materials.
[0022] The invention discloses an application of the bio-based closed-loop recyclable biomimetic aerogel in the preparation of a composite phase-change heat storage material. Specifically, the aerogel is used as a supporting material and compounded with a phase-change material such as paraffin to prepare a composite phase-change heat storage material.
[0023] Separating and recycling materials from PPCM has always been challenging. Compared with the currently reported phase change composite materials, the composite phase change material prepared by the present invention is based on dynamic network aerogel, which can gradually recycle raw materials and meet the sustainable development goals.
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) the preparation process is simple, green and highly controllable; (2) the bio-based trialdehyde raw materials are environmentally friendly and easy to obtain; (3) the introduction of phosphorus-containing monomers makes it have a good flame retardant effect in commercial applications to reduce the potential fire threat in life. (4) The abundant reversible cross-linking points in the network give the aerogel ultra-fast degradation performance, and closed-loop chemical monomer recovery and reprocessing can be carried out. And the whole material can be reused and reprocessed in the degradation liquid. (5) The prepared aerogel has a multi-level bionic structure, including a bionic pore structure, which can realize rapid liquid transmission against gravity, and its various properties, including mechanical properties, thermal insulation properties, etc. have unique anisotropy. At the same time, it has a multi-level roughness structure at the microscopic level, forming a super-hydrophobic property similar to the lotus leaf effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the preparation of bio-based closed-loop recyclable biomimetic aerogel.
[0026] Figure 2 a is the compression characteristics of dynamic aerogel (vertical direction); b is the longitudinal compression test of TFA-5 under different strain conditions; c is the compression characteristics of dynamic aerogel (horizontal direction); d is the stress-strain curve of the tensile performance of TFAs; e is the thermal conductivity of dynamic aerogel; f is the thermal conductivity test of TFA-5 in the vertical and horizontal directions; g is the heat transfer test of TFA-5 in different directions; h is a schematic diagram of the heat transfer mechanism of dynamic aerogel; i and j are the thermal insulation properties of dynamic aerogel, commercial polyurethane foam and melamine foam under extremely harsh conditions (high temperature environment and low temperature environment), respectively.
[0027] Figure 3 (a) is the FT-IR spectrum of TMP and TFA-5 samples; (b) is the XPS spectrum of dynamic aerogel.
[0028] Figure 4 a is the dynamic aerogel hydrophobicity and lipophilicity test image; b is the water contact angle measurement of the dynamic aerogel; c is the adsorption test of the aerogel on various organic solvents; SEM images of the microstructure of TFAs: d is TFA-10, e is TFA-5, and f is TFA-3.
[0029] Figure 5 This is a photo of the TFA-5 solvent resistance test.
[0030] Figure 6 (a) shows the anti-gravity liquid transport capability test of dynamic aerogels; SEM images of the directional channels inside TFA-5 aerogels: (b) top section, (c) bottom section.
[0031] Figure 7a is a schematic diagram of the dissociation and repolymerization of cross-linked molecules in dynamic aerogels; b is the dissociation process of TFA-5 in degradation solutions of different concentrations; c is the degradation kinetics of dynamic aerogels in 1.5 M HCl; d is the recovery of monomer TMP 1 HNMR spectrum; e is a schematic diagram of the material-free, environmentally sustainable recycling and post-processing of dynamic aerogels; compression characteristics of green regenerated dynamic aerogels: f vertical direction, g horizontal direction; h is the tensile stress-strain curve of welded aerogels; i is the SEM image of green regenerated aerogels.
[0032] Figure 8 (a) is the dynamic aerogel welding test and its principle diagram; (b) is the SEM image of the weld.
[0033] Fig. 9 a is the TGA curve of dynamic aerogel; SEM image of TFA-5 carbon slag: b is the interior, c is the surface; d is the SEM image of TTA-5 carbon surface layer; energy spectrum of TFA-5 carbon after combustion: e is carbon, f is nitrogen, g is phosphorus; h is the LOI value of dynamic aerogel and comparative commercial foam; i is the Raman spectrum curve of carbon slag after dynamic aerogel combustion; microcalorimetry test of dynamic aerogel: j is HRR, k is THR; l is a schematic diagram of the combustion process of TFAs.
[0034] Fig.10 Shape stability test for PPCM-3, PPCM-5, PPCM-10 and pure PW.
[0035] Fig.11 DSC curves of PW and PPCM during melting and crystallization: a melting and b crystallization process; c is the total enthalpy of melting and crystallization of the test sample; d is the enthalpy efficiency; e is the XRD spectrum of PW and PPCMs; f is the SEM image inside the PPCM; during the heating test of PPCMs and TFA-5: g is the infrared image, h is the curve of surface temperature change with time; i is the schematic diagram of PPCM heat storage and step-by-step recovery of raw materials.
[0036] Fig.12 a is the XRD spectrum of the recovered PW; b is the XRD spectrum of the recovered TMP monomer 1 H NMR spectrum. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, the purpose of which is to explain the content of the present invention more specifically and clearly rather than to limit the protection scope of the present invention. Embodiment 1:
[0038] The preparation of the bio-based closed-loop recyclable biomimetic aerogel in this embodiment includes the following steps: 1. First, synthesize the bio-based trialdehyde monomer tris(4-formyl-2-methoxyphenyl)phosphate (TMP), which is prepared by the reaction of phosphorus oxychloride and vanillin. First, vanillin (45.6 g, 0.3 mol) and triethylamine (30.3 g, 0.3 mol) were mixed and dissolved in 220 mL of ethyl acetate, and phosphorus oxychloride (15.3 g, 0.1 mol) was added dropwise to the above solution under ice-water bath conditions. After reacting in the ice-water bath for 30 min, the ice-water bath was removed, and the reaction was continued at 25°C for 24 h under stirring. After the reaction was completed, the mixed solution was poured into 1000 mL of deionized water and continued to stir for 0.5 h. The above mixed solution was filtered to obtain a white solid (yield of about 94%). The obtained crude product was recrystallized with ethanol and dried in a vacuum oven at 70°C for 30 h to obtain the final product TMP, which is a white powder with a vanilla flavor.
[0039] 2. Dissolve 1.0 g (2 mmol) of TMP in 12 g of dimethyl sulfoxide (DMSO) solution, then add 0.54 g (1.2 mmol) of 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene (p-6FAPB) to 20 g of DMSO and stir until fully dissolved. Mix the above solutions and stir at room temperature for 2 h. Next, quickly add 0.18 g (1.2 mmol) of tris(2-aminoethyl)amine (TAEA) to the above solution, stir for 30 s, and then ultrasonically vibrate the mixed solution for 1 min. Then, quickly transfer the solution to the mold and let it stand at 60 °C for 2 h under sealed conditions. During this period, the reaction proceeds rapidly and gelation occurs. The gelation process is further aged at room temperature for 48 h. The mold used is a cubic or cylindrical container made of polytetrafluoroethylene with open bottom and top, and the bottom is covered with a 0.01 mm thick PE film.
[0040] 3. Transfer the fully aged wet gel to a directional freezing device with liquid nitrogen as the freezing source for 30 minutes of directional freezing. Then remove the sample from the mold and transfer it to the freeze dryer cold trap with the temperature set to -50°C. Perform the aging procedure again for 12 hours. Next, start the drying procedure and quickly transfer the sample to the sample tray with a vacuum degree of less than 1 Pa for 120 hours. Finally, transfer the obtained material to a vacuum oven for 12 hours with the temperature set at 70°C to obtain the target aerogel TFA-5.
[0041] The cross-linked network formed by TMP and diamine p-6FAPB and TAEA through Schiff base reaction was further designed by directional freeze drying to obtain dynamic aerogel with excellent performance. PI aerogel was characterized by FT-IR and XPS. Figure 3 As shown in a, the FT-IR spectra of TMP and TFA-5 samples are at 1590 cm-1 and 1510 cm -1 The skeleton vibration of the benzene ring was clearly observed at 1690 cm -1 The characteristic peak at 1640 cm is related to the C=O bond of TMP monomer. By comparing the FT-IR spectra of TMP and TFA-5, it can be clearly seen that C=O becomes extremely weak, while the peak at 1640 cm -1 A strong peak corresponding to the C=N bond appeared at , indicating that the Schiff base reaction successfully formed an imine bond, which indicates a high monomer conversion rate of amine and aldehyde. Figure 3 b) Due to the difference in monomers, the peak corresponding to element F of TTA-5 is absent compared to TFA-5, while the intensities of the peaks of other elements are basically the same, which is in line with expectations.
[0042] Since the directional skeleton structure of aerogel gives it anisotropic mechanical properties, the compression test was carried out in the vertical direction and the sample was compressed to a strain of about 50%, such as Figure 2 a. The compressive strength of TFA-5 is 2.81 MPa. The curve shows three different deformation regions: the initial stage associated with the vertical channel skeleton with a rapid increase in stress at a minimum strain; the subsequent stage with a gradual increase in stress corresponding to the bending deformation of the internal vertical skeleton; and finally, the exponential increase in stress indicates densification. Further compression tests were performed on the TFA-5 specimens at different strains ( Figure 2 b). The results show that the aerogels maintain good elastic recovery when the strain is less than 20%. In summary, the anisotropic mechanical properties, together with the excellent thermal insulation properties, make our dynamic aerogels very suitable for applications that require lightweight, durable and efficient thermal management materials. The dynamic aerogel TFA-5 was also subjected to compression tests in the parallel direction ( Figure 2 c). Initially, when the compression is less than 10%, the stress rises rapidly, indicating that the skeleton provides rigid support. The subsequent plateau on the curve indicates that the pores are gradually collapsing. Compared with the vertical compression, the compressive strength in this direction decreases significantly at 50% strain, highlighting the anisotropic mechanical properties of the aerogel, which is beneficial for applications with specific mechanical requirements. In addition, tensile tests were performed on the aerogel samples in the parallel direction ( Figure 2 d), the results show that the tensile strength of TFA-5 is ~0.11MPa and the elongation is ~2.8%.
[0043] Due to its nanoscale topological structure and tunable directional channel skeleton, dynamic aerogels are expected to exhibit excellent thermal insulation efficiency. Figure 2 As shown in e, the thermal conductivity of TFA-5 is 0.034 W m -1 K -1 .like Figure 2As shown in Figure 5, for the TFA-5 test, when heat flows vertically toward the inner channel of the aerogel, the thermal conductivity decreases by 24% to 0.025 W m -1 K -1 , which is comparable to the thermal conductivity of air (0.023 W m -1 K -1 ). This change is mainly due to the change of the heat conduction path through the solid skeleton, such as Figure 2 h, which explains the heat blocking principle of the dynamic aerogel in the parallel direction. The thermal insulation performance of the dynamic aerogel was further revealed by using an infrared camera. Figure 2 g is an infrared image of aerogel heat transfer. TFA-5 was placed on an 80°C hot plate in different directions. The temperature of the sampling point on the aerogel rose to about 30°C within 120 seconds, and then stabilized, with good thermal insulation effect. For samples placed parallel to the heat flow (right), the temperature at the same height is always lower than that of samples placed vertically (left), with a maximum difference of 1.3°C. The superior thermal insulation performance of the dynamic aerogel was verified by placing the dynamic aerogel TFA-5 and commercial insulation materials of the same size under high and low temperature conditions. The surface temperature of the sample was monitored in real time using an infrared camera. The temperature change curve over time is shown in the figure. Figure 2 i(heat) and Figure 2 j (cold). On a hot plate at 120°C, after 10 minutes of heating, the dynamic aerogel TFA-5 always has the lowest surface temperature. Similarly, on a cold plate (<-30°C), the dynamic aerogel has the highest surface temperature.
[0044] Ensuring the hydrolytic stability of dynamic aerogels is crucial to maintaining their mechanical and thermal insulation properties in high humidity environments, which is essential for their all-weather applications. The hydrophobicity of dynamic aerogel TFA-5 was evaluated using static water contact angle and dynamic water flow tests. Figure 4 As shown in b, the dyed water droplets formed a stable hemisphere on the aerogel surface. When water droplets were placed on the inclined surface of TFA-5 (30°), they did not stay or absorb into the surface, but rolled off quickly. Contact angle measurements showed that the water contact angle of TTA-5 achieved a superhydrophobic contact angle of 154.5°. Scanning electron microscope images of the aerogel surface skeleton showed a nanoscale pearl necklace-like structure with nanopores between the bead clusters. TFA-5 showed an accumulation of beads with significant protrusions, and there were pores between the aggregate clusters ( Figure 4 f).
[0045] The prepared TFA-5 exhibits excellent affinity for organic oils and fats. After contacting with the surface of TFA-5 aerogels, they immediately absorb organic oils and fats (mixed alkanes) ( Figure 4a). For easy observation, we dyed both water and oil and placed TFA-5 at the oil-water interface to perform an oil absorption experiment. As shown in the figure, the aerogel quickly absorbed all the oil in the mixture, leaving only water. The aerogel was immersed in different organic solvents to observe its performance in different oil solvents ( Figure 5 The results showed that the material has excellent tolerance to organic solvents and excellent adsorption capacity for various oils and organic solvents ( Figure 4 c). High porosity enables porous materials to form numerous mass transfer channels and storage spaces, thereby enhancing their adsorption capacity. The excellent hydrophobicity and lipophilicity of dynamic aerogels indicate that they have outstanding potential in selective oil absorption and oil spill cleaning. The vertically arranged channels of aerogels, similar to the structure of plant stems, give them the ability to transport liquids against gravity. In order to simulate the anti-gravity liquid transport behavior of plant stems, aerogels were placed vertically in dyed oil with the pores facing upward. Figure 6 a, Liquid moves rapidly from the bottom to the top of the aerogel in the absence of external forces. The liquid transport time is 8 s for the aerogels placed parallel and 60 s for the aerogels placed vertically, corresponding to transport velocities of 1.25 mm / s and 0.17 mm / s, respectively. This represents a 6.5-fold increase in transport velocity when placed vertically. We believe that the aerogels’ ability to transport liquids under gravity is driven by capillary action, which is largely based on Laplace pressure theory. This mechanism involves the interaction of surface tension and pore structure, where the surface tension of the liquid within the small pores generates capillary forces that push the liquid upward. This gravity-resistant liquid transport capability, combined with the aerogels’ selective oil absorption and resistance to organic solvents, enhances their applicability in environmental cleanup and industrial processes involving liquid separation and transport. Interestingly, the diameters of the vertical channels in our aerogels show a gradient. SEM image of TFA-5 ( Figure 6 b and 6c) show a significant difference in top and bottom pore sizes. This asymmetric gradient structure, with gradually decreasing pore size, enhances capillary action and drives water to the smaller pores at the top. Overall, the dynamic aerogels we developed have a variety of biomimetic structures. Their superhydrophobicity, oleophilicity, and gravity-defying liquid transport properties make them very suitable for a variety of applications. They show great potential in solar water evaporation, seawater desalination, and can be extended to thermal insulation, electromagnetic shielding, energy storage and conversion, etc.
[0046] The connection points of the dynamic aerogel network are composed of Schiff base structures, allowing efficient depolymerization and closed-loop recycling of the dynamic aerogel. Figure 7a shows the dissociation and repolymerization of the dynamic cross-linked molecular structure. Acidic solutions can act as proton donors or hydrolysis promoters to break the imine bonds, resulting in the separation of TMP, p-6FAPB, and TAEA from the molecular structure. Subsequently, the free monomers can repolymerize at high temperatures to form a fully cross-linked network. The dissociation behavior of the dynamic aerogel samples was studied using different concentrations of aqueous hydrochloric acid mixed with acetone (1:4). Figure 7 b is the degradation process of TFA-5 in degradation solutions with HCl concentrations of 0.5 M, 1 M, 1.5 M, and 2.0 M at 25 °C. As the proton concentration increases, the time from the initial placement of TFA-5 in the degradation solution to the clarification of the solution gradually decreases. In the 1.5 M hydrochloric acid / acetone solution, the dynamic aerogels were completely dissolved in about 4 min. In addition, when the samples were placed in the degradation solution under ultrasonic stirring, they dissociated at an imperceptibly fast rate. The rapid degradability of the dynamic aerogels can be attributed to two main factors. First, the imine bonds connecting the monomers in the dynamic aerogel network provide abundant reversible cross-linking points. More importantly, the dynamic aerogels have an excellent porous structure with a large number of micro-nanoscale pores, which provide a large specific surface area and provide sufficient reaction sites. In addition, when it is pressed into the degradation solution using a vacuum device, the superhydrophobic TFA-5 maintains its block shape, while TTA-5 gradually dissociates into powder within 50 min ( Figure 7 c) After dissociation, the dynamic aerogel network decomposes into small monomer units, allowing the recovery of the original TMP monomer from a solution containing various monomers and oligomers. The recovery rate of TMP reached 75.1%, indicating that the protons in the degradation solution effectively promoted the reverse Schiff base reaction. Figure 7 As shown in Figure d, the 1H NMR spectrum of TMP recovered from TFA-5 is almost the same as that of the original TMP, indicating the stability of TMP during the recovery process.
[0047] Adding the trialdehyde monomer TMP to the mixture in the correct proportions can fully cross-link the mixture again. The regenerated dynamic aerogel is then obtained through a freeze-drying step. Figure 7 e is the green recycling scheme of dynamic aerogel TFA-5. During the entire recycling process, all materials from the original aerogel are reused without waste. From the retained compressive strength in different directions, it can be seen that the structure and performance of the recycled aerogel are almost the same as those of the original aerogel ( Figure 7 f and Figure 7 g). Internal SEM image of the regenerated aerogel shows that its nanostructure ( Figure 7 i) is almost indistinguishable from the original aerogel. In addition, the degradation solution can act as an adhesive to weld the broken aerogel sheets together ( Figure 8 a). Compared with the original specimen, the tensile strength of the welded specimen retained 81% of the original specimen, indicating good recovery efficiency ( Figure 7 h). SEM image ( Figure 8 b) shows that the welding area has been completely fused and the morphology is the same as the original structure.
[0048] The flammability of polymer aerogels has long been a challenge for industry. Due to their porosity, it is more difficult to achieve flame retardancy compared to other solid polymer materials. Thermogravimetric analysis (TGA) of dynamic aerogels allows us to study their thermal degradation behavior, such as Fig. 9 As shown in a, at 800 °C, the carbon yield of TFA-5 is ~15%. The flame retardancy of the dynamic aerogel was further evaluated by measuring the limiting oxygen index (LOI) of the dynamic aerogel. Fig. 9 h). The LOI value of TFA-5 is 36%. The dynamic aerogel has a higher LOI value compared to commercial PU sponge (19%) and melamine foam (30%). This excellent flame retardancy of the dynamic aerogel may be due to the high content of flame retardant elements and the synergistic effect between them. Upon flame attack, the O=PO bonds in the molecules break to form a phosphorus-rich carbon layer. This dense carbon layer acts as a physical barrier to prevent heat from entering the aerogel and inhibit the spread of flames. The nitrogen element acts synergistically during the combustion process and acts as a foaming agent and a char enhancer. In addition, the fluorine element in TFA-5 further enhances the synergistic effect of the flame retardant elements and promotes the flame retardancy of the gas phase and the condensed phase. The SEM and EDS spectra verified this analysis. Fig. 9 b and Fig. 9 c are the internal and surface SEM images of the carbon residue formed after combustion of TFA-5, respectively. The surface carbon layer was observed to be continuous, dense, and uniform. In addition, a large amount of gas was produced during the combustion process, resulting in a large number of pores in the carbon layer. However, the surface carbon layer formed after combustion of TTA-5 showed many defects ( Fig. 9 d). Phosphorus is rich and evenly distributed on the surface of carbon slag ( Fig. 9 g). In addition, the negligible residual nitrogen in the coke indicates that it participates in the generation of gases during combustion ( Fig. 9 f). In addition, the little retention of fluorine in the char indicates that it plays a major role in gas phase flame retardancy. Raman spectra of carbon residues of dynamic aerogel samples ( Fig. 9 i) It can be seen that the sample has a peak at 1340 cm -1 and 1585 cm -1 There are two significant peaks at each location, corresponding to the d band and the g band respectively. The ID / IG ratio, which characterizes the degree of graphitization of carbon slag, is a key indicator for evaluating the flame retardancy of carbon slag. The higher the ratio, the better the flame retardancy. The ID / IG value of TFA-5 is 3.1. The heat release rate (HRR) ( Fig. 9 j) and total heat release rate (THR) ( Fig. 9k) The prepared dynamic aerogels were subjected to microcalorimetry to evaluate their combustion behavior, and the results showed that the HRR values of all samples were lower than 60 W / g. Figure 91 shows a schematic diagram of the combustion process of TFAs. Embodiment 2:
[0049] The preparation of the bio-based closed-loop recyclable biomimetic aerogel in this embodiment includes the following steps: 1. First, synthesize the bio-based trialdehyde monomer tris(4-formyl-2-methoxyphenyl) phosphate (TMP), according to the method of Example 1.
[0050] 2. Dissolve 1.0 g (2 mmol) of TMP in 17 g of dimethyl sulfoxide (DMSO) solution, then add 0.54 g (1.2 mmol) of 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene (p-6FAPB) to 40 g of DMSO and stir until fully dissolved. Mix the above solutions and stir at room temperature for 2 h. Next, quickly add 0.18 g (1.2 mmol) of tris(2-aminoethyl)amine (TAEA) to the above solution, stir for 30 s, and then ultrasonically vibrate the mixed solution for 1 min. After that, quickly transfer the solution to the mold and let it stand at 60 ° C for 2 h under closed conditions. During this period, the reaction proceeds rapidly and gelation occurs. The gelation process is further aged at room temperature for 48 h.
[0051] 3. Transfer the fully aged wet gel to a directional freezing device with liquid nitrogen as the freezing source for 30 min of directional freezing. Then remove the sample from the mold and transfer it to the cold trap of the freeze dryer with the temperature set to -50 °C. Perform the aging procedure again for 12 h. Next, start the drying procedure and quickly transfer the sample to the sample tray with a vacuum degree of less than 1 Pa for 120 h. Finally, transfer the obtained material to a vacuum oven for 12 h with the temperature set at 70 °C to obtain the target aerogel TFA-3.
[0052] Since the directional skeleton structure of aerogel gives it anisotropic mechanical properties, the compression test was carried out in the vertical direction and the sample was compressed to a strain of about 50%, such as Figure 2 a. The compressive strength of TFA-3 is 1.42 MPa. The curve shows three different deformation regions: the initial stage associated with the vertical channel skeleton with a rapid increase in stress with minimum strain; the subsequent stage with a gradual increase in stress corresponding to the bending deformation of the internal vertical skeleton; and finally, the exponential increase in stress indicates densification. The dynamic aerogel was also subjected to compression tests in the parallel direction ( Figure 2c). Initially, when the compression is less than 10%, the stress rises rapidly, indicating that the skeleton provides rigid support. The subsequent plateau on the curve indicates that the channel is gradually collapsing. Compared with the vertical compression, the compressive strength in this direction decreases significantly at 50% strain, highlighting the anisotropic mechanical properties of the aerogel, which is beneficial for applications with specific mechanical requirements. In addition, tensile tests were performed on the aerogel samples in the parallel direction ( Figure 2 d), the results show that the tensile strength of TFA-3 is ~0.08 MPa and the elongation is ~3.8%.
[0053] Due to its nanoscale topological structure and tunable directional channel skeleton, dynamic aerogels are expected to exhibit excellent thermal insulation efficiency. Figure 2 As shown in e, the thermal conductivity of TFA-3 is 0.033 W m -1 K -1 .
[0054] The hydrophobicity of the dynamic aerogel TFA-3 was evaluated using static water contact angle. Contact angle measurements showed that the water contact angle of TFA-3 achieved a water contact angle of 130.7°. Scanning electron microscope images of the aerogel surface skeleton showed a nanoscale pearl necklace-like structure with nanopores between the bead clusters. The microbeads in TFA-3 could not aggregate, inhibiting the formation of a layered protrusion structure ( Figure 3 g).
[0055] The material has excellent resistance to organic solvents and excellent adsorption capacity for various oils and organic solvents ( Figure 4 c) TFA-3's anti-gravity liquid transport capacity is the same as TFA-5. The rapid degradation test, monomer recovery and green recovery performance of dynamic aerogel TFA-3 are the same as TFA-5.
[0056] The flammability of polymer aerogels has long been a challenge for industry. Due to their porosity, it is more difficult to achieve flame retardancy compared to other solid polymer materials. Thermogravimetric analysis (TGA) of dynamic aerogels allows us to study their thermal degradation behavior, such as Fig. 9 As shown in a, at 800 °C, the char yield of TFA-3 is ~12%. Embodiment 3:
[0057] The preparation of the bio-based closed-loop recyclable biomimetic aerogel in this embodiment includes the following steps: 1. First, synthesize the bio-based trialdehyde monomer tris(4-formyl-2-methoxyphenyl) phosphate (TMP), according to the method of Example 1.
[0058] 2. Dissolve 1.0 g (2 mmol) of TMP in 5 g of dimethyl sulfoxide (DMSO) solution, then add 0.54 g (1.2 mmol) of 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene (p-6FAPB) to 10 g of DMSO and stir until fully dissolved. Mix the above solutions and stir at room temperature for 2 h. Next, quickly add 0.18 g (1.2 mmol) of tris(2-aminoethyl)amine (TAEA) to the above solution, stir for 30 s, and then ultrasonically vibrate the mixed solution for 1 min. After that, quickly transfer the solution to a special mold and let it stand at 60 ° C for 2 h under closed conditions. During this period, the reaction proceeds rapidly and gelation occurs. The gelation process is further aged at room temperature for 48 h.
[0059] 3. Transfer the fully aged wet gel to a directional freezing device with liquid nitrogen as the freezing source for 30 min of directional freezing. Then remove the sample from the mold and transfer it to the freeze dryer cold trap with the temperature set to -50 °C. Perform the aging procedure again for 12 h. Next, start the drying procedure and quickly transfer the sample to the sample tray with a vacuum degree of less than 1 Pa for 120 h. Finally, transfer the obtained material to a vacuum oven for 12 h with the temperature set at 70 °C to obtain the target aerogel TFA-10.
[0060] Since the directional skeleton structure of aerogel gives it anisotropic mechanical properties, the compression test was carried out in the vertical direction and the sample was compressed to a strain of about 50%, such as Figure 2 a. The compressive strength of TFA-10 is 2.83 MPa. The curve shows three different deformation regions: the initial stage associated with the vertical channel skeleton with a rapid increase in stress with minimum strain; the subsequent stage with a gradual increase in stress corresponding to the bending deformation of the internal vertical skeleton; and finally, the exponential increase in stress indicates densification. The dynamic aerogel was also subjected to compression tests in the parallel direction ( Figure 2 c). Initially, when the compression is less than 10%, the stress rises rapidly, indicating that the skeleton provides rigid support. The subsequent plateau on the curve indicates that the pores are gradually collapsing. Compared with the vertical compression, the compressive strength in this direction decreases significantly at 50% strain, highlighting the anisotropic mechanical properties of the aerogel, which is beneficial for applications with specific mechanical requirements. In addition, tensile tests were performed on the aerogel samples in the parallel direction ( Figure 2 d), the results show that the tensile strength of TFA-10 is ~0.21MPa and the elongation is ~1.4%.
[0061] Due to its nanoscale topological structure and tunable directional channel skeleton, dynamic aerogels are expected to exhibit excellent thermal insulation efficiency. Figure 2 As shown in e, the thermal conductivity of TFA-10 is 0.041 W m-1 K -1 .
[0062] The hydrophobicity of the dynamic aerogel TFA-10 was evaluated using static water contact angle. Contact angle measurements showed that TFA-10 achieved a water contact angle of 142.6°. Scanning electron microscopy images of the aerogel surface skeleton showed a nanoscale pearl necklace-like structure with nanopores between the bead clusters. The tightly packed beads and shrunken porosity observed in TFA-10 ( Figure 4 d).
[0063] The material has excellent resistance to organic solvents and excellent adsorption capacity for various oils and organic solvents ( Figure 4 c) TFA-10 has the same anti-gravity liquid transport capacity as TFA-5. The rapid degradation test, monomer recovery and green recovery performance of dynamic aerogel TFA-10 are the same as TFA-5.
[0064] The flammability of polymer aerogels has long been a challenge for industry. Due to their porosity, it is more difficult to achieve flame retardancy compared to other solid polymer materials. Thermogravimetric analysis (TGA) of dynamic aerogels allows us to study their thermal degradation behavior, such as Fig. 9 As shown in a, at 800 °C, the char yield of TFA-10 is ~15%. Embodiment 4:
[0065] The preparation of the bio-based closed-loop recyclable biomimetic aerogel in this embodiment includes the following steps: 1. First, synthesize the bio-based trialdehyde monomer tris(4-formyl-2-methoxyphenyl) phosphate (TMP), according to the method of Example 1.
[0066] 2. Dissolve 1.0 g (2 mmol) of TMP in 12 g of dimethyl sulfoxide (DMSO) solution, then add 0.54 g (1.2 mmol) of 1,4-bis(4-aminophenoxy)benzene (TPE-Q) to 32 g of DMSO and stir until fully dissolved. Mix the above solutions and stir at room temperature for 2 h. Next, quickly add 0.18 g (1.2 mmol) of tris(2-aminoethyl)amine (TAEA) to the above solution, stir for 30 seconds, and then ultrasonically vibrate the mixed solution for 1 min. After that, quickly transfer the solution to a special mold and let it stand at 60 ° C for 2 h under closed conditions. During this period, the reaction proceeds rapidly and gelation occurs. The gelation process is further aged at room temperature for 48 h.
[0067] 3. Transfer the fully aged wet gel to a directional freezing device with liquid nitrogen as the freezing source for 30 min of directional freezing. Then remove the sample from the mold and transfer it to the freeze dryer cold trap with the temperature set to -50 °C. Perform the aging procedure again for 12 h. Next, start the drying procedure and quickly transfer the sample to the sample tray with a vacuum degree of less than 1 Pa for 120 h. Finally, transfer the obtained material to a vacuum oven for 12 h with the temperature set at 70 °C to obtain the target aerogel TTA-5.
[0068] Since the directional skeleton structure of aerogel gives it anisotropic mechanical properties, the compression test was carried out in the vertical direction and the sample was compressed to a strain of about 50%, such as Figure 2 a. The compressive strength of TTA-5 is 2.15 MPa. The curve shows three different deformation regions: the initial stage associated with the vertical channel skeleton with a rapid increase in stress with minimum strain; the subsequent stage with a gradual increase in stress corresponding to the bending deformation of the internal vertical skeleton; and finally, the exponential increase in stress indicates densification. The dynamic aerogel was also subjected to compression tests in the parallel direction ( Figure 2 c). Initially, when the compression is less than 10%, the stress rises rapidly, indicating that the skeleton provides rigid support. The subsequent plateau on the curve indicates that the channel is gradually collapsing. Compared with the vertical compression, the compressive strength in this direction drops significantly at 50% strain, highlighting the anisotropic mechanical properties of the aerogel, which is beneficial for applications with specific mechanical requirements.
[0069] Due to its nanoscale topological structure and tunable directional channel skeleton, dynamic aerogels are expected to exhibit excellent thermal insulation efficiency. Figure 2 As shown in e, the thermal conductivity of TTA-5 is 0.034 W m -1 K -1 .
[0070] The hydrophobicity of the dynamic aerogel TTA-5 was evaluated by static water contact angle. The contact angle measurement showed that the water contact angle of TTA-5 achieved a water contact angle of 132.1°. The rapid degradation test of the dynamic aerogel TTA-5, the monomer recovery and green recovery performance are the same as TFA-5.
[0071] The flammability of polymer aerogels has long been a challenge for industry. Due to their porosity, it is more difficult to achieve flame retardancy compared to other solid polymer materials. Thermogravimetric analysis (TGA) of dynamic aerogels allows us to study their thermal degradation behavior, such as Fig. 9 As shown in a, at 800 °C, the carbon yield of TFA-10 is ~7.0%. The SEM image shows that the surface carbon layer formed after the combustion of TTA-5 shows many defects ( Fig. 9 d). Embodiment 5:
[0072] In this embodiment, the preparation of the phase change composite material based on the bio-based closed-loop recyclable biomimetic aerogel comprises the following steps: The aerogel TFAs in Example 1, Example 2 and Example 3 were used as supporting materials, and paraffin was used as the phase change material unit to prepare phase change composite materials PPCMs. The specific preparation method is as follows: TFA-3, TFA-5 and TFA-10 were immersed in molten paraffin liquid, placed in a vacuum oven, the temperature was set to 80°C, and maintained for 12 h. Then the TFAs were taken out of the paraffin and placed in an oven at 80°C for 10 h. The samples were taken out to obtain phase change composite materials PPCM-3, PPCM-5 and PPCM-10.
[0073] Compared with the currently reported phase-change composites, the prepared PPCMs are based on dynamic network aerogels, which can gradually recycle raw materials and meet the sustainable development goals. Fig.10 The shape stability tests of PPCM-3, PPCM-5, PPCM-10 and pure paraffin (PW) were performed. After heating at 80 °C for 10 min, PW completely melted, while the PPCMs samples retained their original shape after heating for 2 h, and no leakage was observed. The absorption rates of PPCM-3, PPCM-5 and PPCM-10 were still high, at 96.2%, 98.2% and 95.9%, respectively. The thermal storage performance of PPCMs was characterized by DSC. Fig.11 a and 11b describe the endothermic and exothermic processes, respectively. Both pure PW and PPCMs exhibit two characteristic peaks. In the endothermic stage, a peak appears at around 30 °C, corresponding to the solid-solid phase transition of PW, followed by a broad peak at around 50 °C, which is the main peak of the solid-liquid phase transition. Compared with pure PW, the phase transition temperature of the sample has hardly changed, except that the latent heat value has slightly decreased due to the inclusion of a dynamic aerogel skeleton. The total enthalpy of PPCMs includes two parts: solid-solid phase change enthalpy and solid-liquid phase change enthalpy. Fig.11 c gives the enthalpy calculation results of different samples. The total melting enthalpy of PPCM-5 is as high as 160.5 J / g, and the solid-liquid phase change enthalpy is 126.8 J / g, which is comparable to the heat storage enthalpy of pure PW. The heat storage performance of the PPCM sample was further characterized by the enthalpy efficiency (λ) and relative enthalpy efficiency (η). The results are shown in Fig.11 d. The results show that the enthalpy efficiencies of all PPCMs are very close to the respective loadings of their PW components. For example, PPCM-5 has a λ as high as 97.4%, and the melting enthalpy and crystallization enthalpy are 160.1 and 162.8 J / g, respectively. In addition, the relative enthalpy efficiency is always less than 1, which is mainly due to the fact that the dynamic aerogel foam scaffold affects the crystallization properties of PW. The prepared PPCMs have high thermal enthalpy, which lays a solid foundation for their application. Fig.11e is the XRD spectrum of PW and PPCMs. On the pure PW curve, two sharp diffraction peaks were observed at 21.1° and 22.8°, corresponding to the (110) and (200) crystal planes, respectively. TFA-5 showed only a weak signal peak, indicating that the crystallinity was not obvious. PPCM mainly showed the characteristic peaks of PW without change, indicating that PW was completely preserved in the dynamic framework of the aerogel. The SEM image of PPCM showed that its internal pores were completely filled with PW ( Fig.11 f), the boundary between the PW and the inner wall is almost indistinguishable.
[0074] PPCMs and aerogels handle heat flow differently. As mentioned earlier, aerogels mainly use static air in their micro-nanostructures to limit heat transfer, thereby providing excellent insulation. In contrast, PPCMs made of dynamic aerogels absorb external heat as a porous skeleton, transforming from an ordered state to a disordered state. When the ambient temperature drops, the stored heat is released when the PCM transforms back. Therefore, unlike aerogels, PPCMs can manage heat intelligently. We studied the heat storage and release behaviors of the prepared PPCMs. Block PCCM and its skeleton material TFA-5 were placed on a hot plate at 80°C. After heating for a period of time, they were taken out and cooled naturally. The surface temperature distribution of the samples was observed and recorded using a thermal infrared imager ( Fig.11 g). Fig.11 h is the surface temperature variation of PCCM-5 and TFA-5 over time. Due to the heat preservation effect of the aerogel, after about 4 min of heating, the surface temperature of TFA-5 stabilized at around 35 °C, while the temperature of PCCM-5 continued to rise. After removing the heat source, TFA-5 cooled rapidly to ambient temperature, while PCCM-5 cooled more slowly and showed a temperature plateau, corresponding to the phase change of PCM. The temperature sensor recorded the bottom temperature of the sample. During the heating process, the temperature of PCCM-5 rose rapidly to the phase change range of PW. As PW melted and absorbed heat, the rate of temperature increase slowed down. Once PW completed the phase change, the internal temperature continued to rise rapidly. After removing the hot plate, the temperature dropped to the point where PW began to transform, resulting in a plateau period due to the release of stored heat. In contrast, TFA-5 showed rapid temperature changes without delay during both heating and cooling. This indicates a very high affinity between PW and TFA framework. These results confirm that our PCCMs can effectively manage heat flow and control the temperature of various systems through effective heat storage and release, such as Fig.11i. Separation and recovery of materials from PPCM has always been challenging. However, our PPCM exhibited excellent recovery performance. The recovery process involved placing the PCCM sample in a 1.5M HCl aqueous solution followed by ultrasonic stirring for 30 min and then allowing it to settle. The oily paraffin separated from the aqueous phase to form layers. After separation of the layers, the paraffin fragments were collected, washed and dried. The bottom layer was filtered and washed with ethanol to obtain TMP powder. The 1H NMR spectrum of the recovered TMP monomer and the XRD spectrum of the recovered PW are shown in Fig.12 The monomer recovery process of PPCM is shown in Fig.11 i. The recovered TMP monomer can be used to synthesize dynamic aerogels.
Claims
1. A method for preparing a bio-based closed-loop recyclable biomimetic gel, characterized in that The steps include: Step 1: Add vanillin and triethylamine to ethyl acetate, then add phosphorus oxychloride, react in an ice-water bath for a certain period of time, remove the ice bath, and continue to stir and react for a period of time; after the reaction, pour the product into a sufficient amount of deionized water, continue to stir, and obtain a white solid product after suction filtration, which is recrystallized with ethanol and dried to obtain bio-based trialdehyde phosphate tris (4-formyl-2-methoxyphenyl) ester TMP; Step 2: Dissolve the TMP obtained in step 1 in dimethyl sulfoxide, add the diamine monomer in a certain proportion, stir until fully dissolved, and stir at room temperature for 2 h; then add a certain amount of tris(2-aminoethyl)amine to the system, stir for 30 s, and then ultrasonically vibrate for 1 min; Step 3: The system of step 2 is quickly transferred to a mold, and allowed to stand at 50-80°C for 2 hours under closed conditions to allow gelation reaction to occur, and then further aged at room temperature for 12-72 hours; Step 4: Transfer the fully aged wet gel to a directional freezing device, use liquid nitrogen as the freezing source, and perform directional freezing for 30 minutes; then remove the sample from the mold and transfer it to the cold trap of the freeze dryer, set the temperature to -50°C, and perform the aging procedure again for 12 hours; then quickly transfer the sample to a sample tray, with a vacuum degree of less than 1 Pa, and dry for 72-120 hours; finally, transfer the obtained material to a vacuum oven and dry it at 70°C for 12 hours to obtain the target aerogel.
2. The preparation method according to claim 1, characterized in that: In step 1, the molar ratio of vanillin to triethylamine is 1:1, and the molar ratio of vanillin to phosphorus oxychloride is 3:
1.
3. The preparation method according to claim 1, characterized in that: In step 1, after the system is reacted in an ice-water bath for 25-30 min, the ice-water bath is removed, and the reaction is continued at 25° C. with stirring for 22-26 h.
4. The preparation method according to claim 1, characterized in that: In step 2, the diamine monomer is selected from one or more of 1,4-bis(2-trifluoromethyl-4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, diethylenetriamine, aliphatic linear diamines, p-phenylenediamine, anthracene-2,6-diamine, 3,6-diaminocarbazole, 2,7-diaminofluorene, 4,4'-diaminodiphenylmethane, and 4,4'-diaminodiphenyl sulfide.
5. The preparation method according to claim 1, characterized in that: In step 2, the ratio of the molar amount of aldehyde groups contained in TMP to the total molar amount of amine groups contained in the diamine monomer and tris(2-aminoethyl)amine is 1:
1.
6. The preparation method according to claim 5, characterized in that: The molar ratio of the diamine monomer to tris(2-aminoethyl)amine is 0-4:4-0, and the molar ratio of the two is not 0 at the same time.
7. The preparation method according to claim 6, characterized in that: The molar ratio of the diamine monomer to tris(2-aminoethyl)amine is 1:0, 4:1, 3:2, 1:1, 2:3, 1:4 or 0:
1.
8. Use of the bio-based closed-loop recyclable bionic aerogel prepared according to any one of the preparation methods of claims 1 to 7 in the preparation of thermal insulation materials.
9. Use of the bio-based closed-loop recyclable biomimetic aerogel prepared according to any one of the preparation methods of claims 1 to 7 in the preparation of oil-water separation materials.
10. Use of the bio-based closed-loop recyclable bionic aerogel prepared according to any one of the preparation methods of claims 1 to 7 in the preparation of composite phase change heat storage materials; specifically, using aerogel as a supporting material and compounding it with a phase change material to prepare a composite phase change heat storage material.
Citation Information
Cited By
Flexible shaped polymer composite inorganic phase change material as well as preparation method and application thereof
CN120349776A
Bio-based oil-water separation material
CN120420960A