Activating agent for rubber vulcanization reaction as well as preparation method and application of activating agent

By using nanomaterial carriers doped with non-metallic elements to anchor zinc oxide in the rubber vulcanization reaction to form fully exposed sub-nanometer clusters, the problems of high cost of zinc oxide activators and low zinc utilization are solved, and efficient Rubber vulcanization and resource conservation.

CN118725408AActive Publication Date: 2024-10-01UNIV OF SCI & TECH OF CHINA +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410771144.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The zinc oxide activator used in the existing rubber vulcanization reaction is high in cost and has low zinc utilization rate, resulting in water pollution and resource waste.

Method used

Nanomaterials doped with non-metallic elements are used as carriers to anchor zinc oxide to form fully exposed sub-nanometer clusters, which improves catalytic activity and zinc atom utilization and reduces the dosage of zinc oxide.

Benefits of technology

Efficient rubber vulcanization reaction is achieved, vulcanization time is shortened, reaction efficiency is improved, metal resources are saved, and the preparation process has low dependence on temperature, making it easy to be industrialized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725408A_ABST
    Figure CN118725408A_ABST
Patent Text Reader

Abstract

The invention provides an activating agent for rubber vulcanization reaction as well as a preparation method and application thereof, and belongs to the technical field of catalysts. The activating agent for the rubber vulcanization reaction comprises a carrier and zinc oxide. Wherein the carrier is a nano material doped with non-metallic elements. The zinc oxide is anchored on the outer surface of the carrier. Zinc oxide is coordinated with non-metallic elements doped on the outer surface of the carrier, and a monatomic layer is formed in the form of fully exposed sub-nanoclusters. Zinc oxide is coordinated with non-metallic elements doped on the outer surface of the carrier, and zinc atoms are not overlapped and are anchored on the outer surface of the carrier in the form of sub-nanoclusters in a dispersed full exposure mode, so that the zinc atoms can be fully exposed to serve as active centers, and the catalytic activity is improved. The activator can be applied to the vulcanization reaction in the rubber field, the vulcanization reaction efficiency is improved, the zinc consumption can be reduced by 70-80% due to full exposure of zinc atoms, and industrial energy consumption and metal resources are saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, in particular to an activator for rubber vulcanization reaction and a preparation method and application thereof, and more particularly to a fully exposed sub-nano cluster material capable of replacing vulcanization reaction. Background Art

[0002] The amount of rubber used is high, and my country's annual consumption is about 10 million tons. For vulcanized rubber, a large amount of zinc oxide needs to be added as an activator during the production process. Zinc oxide has the functions of activating the vulcanization system, increasing the crosslinking density, and improving the anti-aging properties of vulcanized rubber. At present, zinc oxide is still a relatively effective rubber activator and plays a very important role. However, the cost of zinc oxide is high, and excessive use will cause more serious water pollution. In addition, the zinc oxide activators used are mostly granular nano zinc oxide, which has problems such as low zinc utilization and insufficient activity, making it difficult to reduce the amount of zinc used. Summary of the invention

[0003] In view of this, in order to at least partially solve at least one of the above-mentioned technical problems, the present invention provides an activator for rubber vulcanization reaction and a preparation method and application thereof.

[0004] According to an embodiment of one aspect of the present invention, an activator for rubber vulcanization reaction is provided, comprising: a carrier, which is a nanomaterial doped with non-metallic elements; zinc oxide, anchored on the outer surface of the carrier; wherein the zinc oxide is coordinated with the non-metallic elements doped on the outer surface of the carrier to form a single atomic layer in the form of fully exposed sub-nano clusters.

[0005] According to an embodiment of the present invention, the mass ratio of zinc oxide to the carrier is (0.5-10):100.

[0006] According to an embodiment of the present invention, the nanomaterial includes at least one of carbon black, white carbon black or graphene oxide; the non-metallic element includes at least one of nitrogen, oxygen, phosphorus and boron; the particle size of the carbon black is 10-100 nm, and the specific surface area is 50-150 m 2 / g; the particle size of white carbon black is 20~100nm, and the specific surface area is 100~300m 2 / g; the size of graphene oxide is 1~10μm, the thickness is 3~10nm, and the specific surface area is 100~400m 2 / g.

[0007] According to an embodiment of the present invention, the doping amount of the non-metallic element accounts for 0.5-5% by mass of the nanomaterial.

[0008] According to an embodiment of another aspect of the present invention, there is provided a method for preparing an activator as described above, comprising: dispersing a carrier in a first solvent to obtain a dispersed solution; adding a zinc metal salt and an alkaline solution to the dispersed solution to carry out a hydrolysis reaction to obtain an activator; wherein the carrier is a nanomaterial doped with a non-metallic element.

[0009] According to an embodiment of the present invention, the alkaline solution includes any one of a sodium hydroxide aqueous solution, a lithium hydroxide aqueous solution, and a potassium hydroxide aqueous solution.

[0010] According to an embodiment of the present invention, the temperature of the hydrolysis reaction is 15-25°C.

[0011] According to an embodiment of the present invention, before dispersing the carrier in the first solvent, the method further includes: dispersing the nanomaterial in the second solvent, adding a non-metallic compound, mixing and stirring to react, and obtaining the carrier; the non-metallic compound includes any one of a nitrogen-containing compound, a sulfur-containing compound, a boron-containing compound, and a phosphorus-containing compound.

[0012] According to an embodiment of the present invention, the temperature of the mixing and stirring reaction is 80-85°C.

[0013] According to another embodiment of the present invention, there is provided a use of the above-mentioned activator in a rubber vulcanization reaction.

[0014] According to an embodiment of the present invention, by using a nanomaterial doped with non-metallic elements as a carrier, a higher specific surface area and a richer active site can be provided. The doped non-metallic elements can adjust the electronic structure and chemical properties of the carrier. Zinc oxide forms a coordination effect with the non-metallic elements doped on the outer surface of the carrier, for example, a chemical bond can be formed. This coordination effect can form a coordination unsaturated zinc-oxygen bond with the doped non-metallic elements, which helps to improve the catalytic activity of zinc oxide. Fully exposed sub-nano clusters refer to zinc oxide that is completely exposed on the outer surface of the carrier and bonded to the doped non-metallic elements through coordination bonds. Unlike the conventionally formed nano zinc oxide particles, the zinc oxide of the present invention is not embedded in the activator, but is completely anchored on the outer surface of the carrier and forms a single atomic layer. Therefore, the zinc oxide in the activator of the present invention has a zinc atom utilization rate of nearly 100%. When it is subsequently applied to the rubber vulcanization reaction, it can effectively replace the existing nano zinc oxide particles, and because the zinc oxide of the present invention is in a fully exposed state, the amount of metallic zinc can be reduced by 70-80% on the basis of the amount of conventional zinc oxide nanoparticles, which helps to save metal resources. When the activator of the present invention is subsequently applied to a rubber vulcanization reaction, it has high activity, can shorten the positive vulcanization time, and improve the reaction efficiency, so it can be promoted in industry and help achieve green and sustainable development.

[0015] According to the embodiments of the present invention, the preparation process of the activator of the present invention is not highly dependent on temperature and can be prepared at room temperature. Compared with the traditional indirect method for preparing zinc oxide which requires a high temperature of 1000°C, the method of the present invention can save industrial energy consumption and is easy for industrial preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The above and other objects, features and advantages of the present invention will become more apparent through the following description of the embodiments of the present invention with reference to the accompanying drawings, in which:

[0017] Figure 1 The present invention shows a flow chart of preparing an activator for rubber vulcanization reaction according to an embodiment of the present invention;

[0018] Figure 2 The transmission electron microscope image of the activator 1 suitable for rubber vulcanization reaction in Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0019] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.

[0020] Below, embodiments of the present invention will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of embodiments of the present invention. However, it is apparent that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of concepts of the present invention.

[0021] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. The term "comprising" used herein indicates the existence of features, steps, operations, but does not exclude the existence or addition of one or more other features.

[0022] In the case of using expressions such as "at least one of A, B, and C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, and C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.). In the case of using expressions such as "at least one of A, B, or C, etc.", it should generally be interpreted in accordance with the meaning of the expression generally understood by those skilled in the art (for example, "a system having at least one of A, B, or C" should include but is not limited to a system having A alone, B alone, C alone, A and B, A and C, B and C, and / or A, B, C, etc.).

[0023] In the present invention, the term "fully exposed sub-nano clusters" refers to atomically dispersed, fully exposed zinc oxide cluster activators composed of zinc oxide, the size of which is less than 1 nanometer and is dispersed on the outer surface of the carrier in the form of a single atomic layer, thereby ensuring that all zinc oxide can participate in the adsorption and activation of the reactants.

[0024] Rubber vulcanization is an important industrial reaction that increases the crosslinking density of vulcanized rubber and improves its anti-aging properties. Currently, zinc oxide nanoparticles are a relatively effective rubber activator, but there are problems such as low zinc utilization, insufficient activity, and high dosage.

[0025] In the process of realizing the concept of the present invention, it is found that by using nanomaterials doped with non-metallic elements as carriers, zinc oxide can be anchored on the outer surface of the carrier, which can improve the dispersibility of zinc oxide and make zinc oxide coordinate with the non-metallic elements doped on the outer surface of the carrier to form a coordination-unsaturated zinc-oxygen chemical bond, thereby forming a single atomic layer in the form of fully exposed sub-nanoclusters, which helps to improve the catalytic activity of zinc oxide in the sulfurization reaction and the utilization rate of zinc atoms, and can effectively reduce the amount of zinc oxide used.

[0026] Specifically, according to an embodiment of one aspect of the present invention, an activator for rubber vulcanization reaction is provided, comprising: a carrier and zinc oxide. The carrier is a nanomaterial doped with a non-metallic element. The zinc oxide is anchored on the outer surface of the carrier. The zinc oxide is coordinated with the non-metallic element doped on the outer surface of the carrier to form a single atomic layer in the form of fully exposed sub-nano clusters.

[0027] According to an embodiment of the present invention, by using a nanomaterial doped with non-metallic elements as a carrier, a higher specific surface area and a richer active site can be provided. The doped non-metallic elements can adjust the electronic structure and chemical properties of the carrier. Zinc oxide forms a coordination effect with the non-metallic elements doped on the outer surface of the carrier, for example, a chemical bond can be formed. This coordination effect can form a coordination unsaturated zinc-oxygen bond with the doped non-metallic elements, forming an anchoring interaction between zinc oxide and the carrier, which helps to improve the catalytic activity of zinc oxide. Fully exposed sub-nano clusters refer to zinc oxide that is fully exposed on the outer surface of the carrier and bonded to the doped non-metallic elements through coordination bonds. Unlike the conventionally formed nano zinc oxide particles, the zinc oxide of the present invention is not embedded in the activator, but is all anchored on the outer surface of the carrier and forms a single atomic layer. Therefore, the zinc oxide in the activator of the present invention has a zinc atom utilization rate of nearly 100%, and can effectively replace the existing nano zinc oxide particles when it is subsequently applied to the rubber vulcanization reaction. And because the zinc oxide of the present invention is in a fully exposed state, the amount of metallic zinc can be reduced by 70-80% on the basis of the traditional amount of zinc oxide nanoparticles, which helps to save metal resources. When the activator of the present invention is subsequently applied to a rubber vulcanization reaction, it has high activity, can shorten the positive vulcanization time, and improve the reaction efficiency, so it can be promoted in industry and help achieve green and sustainable development.

[0028] According to an embodiment of the present invention, zinc oxide is anchored in the form of sub-nano clusters at the active sites doped with non-metallic elements on the surface of the carrier to form a single atomic layer. The scale of the fully exposed sub-nano clusters formed is less than 1 nm, so it is in the form of sub-nano clusters, which have a large specific surface area and high surface energy, can fully expose zinc oxide and have a coordinately unsaturated zinc-oxygen bond, thereby increasing the atomic utilization and catalytic activity of zinc atoms.

[0029] According to an embodiment of the present invention, the mass ratio of zinc oxide to the carrier is (0.5-10):100, for example, it can be 0.5:100, 1:100, 1.6:100, 2:100, 2.4:100, 3:100, 3.7:100, 4:100, 4.6:100, 5:100, 6:100, 7:100, 8:100, 9:100 or 10:100, but it is not limited thereto. The appropriate mass ratio range can ensure that there is enough transition metal oxide in the catalyst to provide high catalytic activity, and can prevent the agglomeration or migration of fully exposed sub-nano clusters of zinc oxide, while avoiding the use of excessive zinc oxide resulting in high costs.

[0030] According to an embodiment of the present invention, the nanomaterial includes at least one of carbon black, white carbon black or graphene oxide. The non-metallic element includes at least one of nitrogen, oxygen, phosphorus and boron. For example, taking sulfur-doped graphene oxide as an example, the zinc atom is connected to the carrier through a zinc-oxygen-sulfur chemical bond, which can effectively improve the surface activity and dispersibility of the zinc oxide activator, thereby improving its catalytic performance. The sulfur element is doped into graphene oxide, new active sites are introduced and the electronic properties of graphene oxide are improved, so that zinc oxide can be connected to graphene oxide through sulfur atoms. Based on this, zinc oxide sub-nano clusters can be stably arranged on the surface of the doped carrier, ensuring that zinc atoms are fully exposed on the catalyst surface, and improving the utilization rate of zinc atoms. In addition, zinc oxide sub-nano clusters have a coordinated unsaturated zinc-oxygen bond, which is conducive to improving the activity of the activator.

[0031] According to an embodiment of the present invention, the particle size of carbon black is 10-100 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm, but not limited thereto. The specific surface area is 50-150 m 2 / g, for example, it can be 50m 2 / g, 60m 2 / g, 70m 2 / g, 80m 2 / g, 90m 2 / g、100m 2 / g, 110m 2 / g, 120m 2 / g, 130m 2 / g, 140m 2 / g or 150m 2 / g. The particle size of white carbon black is 20-100nm, for example, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, but not limited thereto. The specific surface area is 100-300m 2 / g, for example, it can be 100m 2 / g, 150m 2 / g, 200m 2 / g, 250m 2 / g or 300m 2 / g. The size of graphene oxide is 1-10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, but not limited thereto. The thickness is 3-10 nm, for example, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm, but not limited thereto. The specific surface area is 100-400 m 2 / g, for example, it can be 100m 2 / g, 150m 2 / g, 200m 2 / g, 250m 2 / g、300m 2 / g, 350m 2 / g or 400m 2 The size range of the above nanomaterials can provide a large specific surface area, which is helpful for the dispersion and anchoring of zinc oxide, thereby improving the catalytic activity and selectivity of the activator, increasing the utilization rate of zinc atoms, and thus improving the catalytic efficiency and saving costs.

[0032] According to an embodiment of the present invention, the doping amount of the non-metallic element accounts for 0.5-5% of the mass percentage of the nanomaterial, for example, it can be 0.6%, 1.5%, 2.5%, 3.4%, 4.1%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. The doping amount in this range can effectively improve the surface properties of magnesium oxide and introduce new active sites into the nanomaterial to enhance the performance of the carrier, while avoiding the degradation of the carrier performance caused by excessive doping.

[0033] Figure 1 The flowchart of the preparation of the activator for rubber vulcanization reaction according to the embodiment of the present invention is shown.

[0034] According to another embodiment of the present invention, a method for preparing the above-mentioned activator is provided. Figure 1 As shown, it includes steps S101~S102.

[0035] In step S101 , a carrier is dispersed in a first solvent to obtain a dispersed solution.

[0036] In step S102, zinc metal salt and alkaline solution are added to the dispersion solution to perform a hydrolysis reaction to obtain an activator.

[0037] According to an embodiment of the present invention, the carrier is a nano material doped with non-metallic elements. The first solvent includes any one of water and ethanol. The role of dispersing the carrier in the first solvent is to promote the uniform dispersion of the carrier, form a stable dispersed solution, and provide cross-rich contact area and reactive sites for subsequent reactions. The zinc metal salt, which is the prerequisite solution of zinc oxide, and the alkali react with the carrier to undergo a hydrolysis reaction to convert the zinc metal salt into zinc oxide, and form a coordination bond with the non-metallic element on the carrier, anchoring the zinc oxide on the outer surface of the carrier, which helps to form fully exposed sub-nano clusters, thereby being used as an activator in the rubber vulcanization process. The activator can promote the cross-linking reaction between rubber molecular chains to improve the physical properties of the rubber.

[0038] According to an embodiment of the present invention, the carrier includes carbon black doped with non-metallic elements, white carbon black doped with non-metallic elements, and graphene oxide doped with non-metallic elements, and the doped non-metallic elements are selected from any one of nitrogen, sulfur, phosphorus, and boron. The zinc metal salt includes at least one of zinc nitrate, zinc chloride, zinc sulfate, and zinc acetate.

[0039] According to an embodiment of the present invention, the temperature of the hydrolysis reaction is 15-25°C, for example, 15°C, 20°C or 25°C, but not limited thereto. The preparation process of the activator of the present invention is not highly dependent on temperature and can be prepared at room temperature. Compared with the traditional indirect method for preparing zinc oxide requiring a high temperature of 1000°C, the method of the present invention can save industrial energy consumption and is easy to prepare industrially.

[0040] According to an embodiment of the present invention, the alkaline solution includes any one of a sodium hydroxide aqueous solution, a lithium hydroxide aqueous solution, and a potassium hydroxide aqueous solution. For example, the alkaline solution can be selected according to actual reaction conditions and a required pH range to promote the anchoring of zinc oxide on the carrier surface in the form of fully exposed sub-nano clusters.

[0041] According to an embodiment of the present invention, the concentration of the carrier is 5-10 g / L, for example, it can be 5.5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L or 9.5 g / L, but it is not limited thereto. The amount of zinc metal salt added is 2.5-40% of the mass fraction of the carrier, for example, it can be 3%, 5%, 10%, 15%, 20%, 25%, 30% or 35%, but it is not limited thereto. The pH range of the hydrolysis reaction is 9-11, for example, it can be 9, 10 or 11, but it is not limited thereto.

[0042] According to an embodiment of the present invention, before dispersing the carrier in the first solvent, the method further includes: dispersing the nanomaterial in the second solvent, adding a non-metallic compound, mixing and stirring the reaction, and obtaining the carrier. The non-metallic compound includes any one of a nitrogen-containing compound, a sulfur-containing compound, a boron-containing compound, and a phosphorus-containing compound. The nitrogen-containing compound can be selected from any one of ammonia water, dimethylformamide, and 2-methylimidazole. The sulfur-containing compound can be selected from any one of thiourea, potassium persulfate, sodium thiosulfate, and n-dodecyl mercaptan. The phosphorus-containing compound can be selected from any one of triphenylphosphine, potassium dihydrogen phosphate, and phosphonic acid. The boron-containing compound can be selected from any one of boric acid, boric anhydride, and boric amide.

[0043] According to an embodiment of the present invention, the second solvent may be, for example, water, ethanol or N,N-dimethylformamide.

[0044] According to an embodiment of the present invention, the temperature of the mixed stirring reaction is 80-85°C, for example, 81°C, 82°C, 83°C, 84°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. This temperature range is conducive to promoting the reaction of nitrogen-containing compounds, sulfur-containing compounds, phosphorus-containing compounds or boron-containing compounds with nanomaterials, thereby achieving effective doping. By accurately controlling these parameters, the preparation process of the carrier can be optimized, thereby improving the performance and efficiency of the carrier.

[0045] According to an embodiment of the present invention, when the carrier is sulfur-doped graphene oxide, the process of preparing the carrier is as follows:

[0046] Graphene oxide powder and thiourea are added to water and mixed evenly, stirred, filtered and dried to obtain sulfur-doped graphene oxide. The hydrogen sulfide (H2S) gas generated by the decomposition of thiourea reacts with oxygen-containing groups (such as carboxyl, hydroxyl, etc.) on the surface of graphene oxide (GO), and sulfur atoms replace oxygen atoms on the surface of graphene oxide or react with oxygen-containing groups to form functional groups such as thioether (-S-) or thiophenol (-SH), and volatile components and chemically bound water are removed by thermal decomposition reaction to form sulfur-doped graphene oxide carrier (S-GO).

[0047] More specifically, the process of preparing sulfur-doped graphene oxide is as follows: at room temperature, add 2g of graphene oxide powder to 500mL of water, stir evenly, then add 0.25g of thiourea and continue stirring, heat the mixed solution to 80-85°C and continue stirring for 12 hours, with the stirring speed controlled at 800-1000rpm. Filter the mixed solution to obtain a solid, then dry and grind it to obtain a sulfur-doped graphene oxide carrier (S-GO).

[0048] According to an embodiment of the present invention, when the zinc metal salt is zinc chloride (ZnCl2), the reaction formula for the preparation process of the activator suitable for the rubber vulcanization reaction is as follows:

[0049] ZnCl2+S-GO+2NaOH→ZnO-S-GO+2NaCl+H2O.

[0050] According to another embodiment of the present invention, there is provided a use of the above-mentioned activator in a rubber vulcanization reaction.

[0051] According to an embodiment of the present invention, since zinc oxide exists in the form of fully exposed sub-nano clusters, it means that each zinc oxide atom can directly participate in the reaction, providing more active sites, thereby improving the efficiency of the rubber vulcanization reaction. Since zinc oxide forms a coordination bond with the non-metallic elements doped on the surface of the carrier, this interaction can further enhance the catalytic performance of zinc oxide, making the vulcanization reaction more rapid and thorough. Since the zinc oxide of the single atomic layer is evenly distributed on the outer surface of the carrier, it helps to achieve the uniformity of cross-linking between the rubber molecular chains, thereby improving the consistency and quality of the rubber material. Since the activator has a high efficiency, the vulcanization process can be completed in a shorter time, which helps to save energy and reduce production costs. In addition, since nanomaterials doped with non-metallic elements are used as carriers, the amount of zinc oxide used can be reduced, and the preparation and application system of the entire activator is more friendly to the environment, reducing the potential impact on the environment.

[0052] According to the embodiments of the present invention, when the activator of the present invention is used to carry out a rubber vulcanization reaction, the vulcanized rubber can have relatively excellent mechanical properties.

[0053] According to an embodiment of the present invention, auxiliary agents may be added during the vulcanization reaction, such as stearic acid, antioxidant, accelerator, sulfur, etc.

[0054] According to an embodiment of the present invention, the rubber includes at least one of natural rubber, styrene-butadiene rubber, nitrile rubber, chloroprene rubber, EPDM rubber, and butadiene rubber.

[0055] The present invention is further described below by way of examples. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive explanation of embodiments of the present invention. However, it is apparent that one or more embodiments may be implemented without these specific details. Moreover, in the absence of conflict, the details in the following embodiments may be combined arbitrarily into other feasible embodiments.

[0056] The test materials and reagents used in the following examples, unless otherwise specified, can be obtained from commercial sources. Among them, zinc nitrate, zinc chloride, zinc sulfate, sodium hydroxide and thiourea, etc., are used to prepare catalyst materials, with a specification of 500g, and the manufacturer is a certain group chemical reagent Co., Ltd. (Shanghai trial); the manufacturer of graphene oxide is a certain company in Suzhou; the manufacturer of carbon black N330, white carbon black, commercial zinc oxide (purity 99.7%), natural rubber and rubber additives is a certain rubber raw material company in Guangzhou. Those that do not specify specific techniques or conditions in the examples are all conventional methods, which can be carried out according to the techniques or conditions described in the literature in this field or according to the product instructions.

[0057] Embodiment 1:

[0058] Preparation process of sulfur-doped graphene oxide support:

[0059] Add 2 g of graphene oxide powder to 500 mL of water at room temperature and stir until uniformly dispersed. Then add 0.25 g of thiourea, raise the solution temperature to about 82°C, and continue stirring for 12 hours at a stirring speed of 850 rpm. Filter and dry, and grind to obtain a sulfur-doped graphene oxide carrier.

[0060] Preparation process of activator 1:

[0061] Weigh 1g of sulfur-doped graphene oxide carrier, add it to 200mL of water and stir evenly, then add 0.2g of zinc nitrate and 10mL of 0.1M sodium hydroxide solution, continue stirring for 12 hours, and keep the stirring speed at 900rpm. The obtained suspension was filtered and dried in an oven at 100°C for 12 hours to finally obtain an activator 1 suitable for rubber vulcanization reaction. Among them, the surface of the sulfur-doped graphene oxide carrier is loaded with zinc oxide sub-nanoclusters 1 (denoted as ZnO-S-GO).

[0062] Figure 2 The transmission electron microscope image of the activator 1 suitable for rubber vulcanization reaction in Example 1 of the present invention is shown. Figure 2 It can be seen that the bright spot encircled by the dotted line is the zinc oxide sub-nano cluster 1, and the surrounding area is the sulfur-doped graphene oxide carrier. It can be seen that the zinc oxide sub-nano cluster 1 is effectively anchored on the outer surface of the sulfur-doped graphene oxide carrier, and the zinc atoms are in a completely dispersed state without overlapping, so it can be verified that the obtained zinc oxide is in a fully exposed state, which can fully expose the catalytic active sites. The diameter of the cluster can be measured according to the magnification of the electron microscope, and its diameter is less than 1nm, so it is a sub-nanometer scale.

[0063] Embodiment 2:

[0064] The catalyst suitable for rubber vulcanization reaction was prepared by the same method as in Example 1, except that 0.25 g of thiourea added in Example 1 was replaced with 1 mL of ammonia water. The zinc oxide sub-nano cluster 2 was supported on the nitrogen-doped graphene oxide carrier, and the zinc oxide sub-nano cluster 2 was recorded as ZnO-N-GO.

[0065] Example 3

[0066] Preparation process of sulfur-doped carbon black carrier:

[0067] Add 2 g of carbon black powder to 500 mL of water at room temperature and stir until uniformly dispersed. Add 0.25 g of thiourea, raise the solution temperature to about 82°C, and continue stirring for 12 hours at a stirring speed of 850 rpm. Filter and dry, and grind to obtain a sulfur-doped carbon black carrier.

[0068] Weigh 1g of sulfur-doped carbon black carrier, add it to 200mL of water and stir evenly, then add 0.2g of zinc nitrate and 10mL of 0.1M sodium hydroxide solution, continue stirring for 12 hours, and keep the stirring speed at 900rpm. The obtained suspension was filtered and dried in an oven at 100°C for 12 hours to finally obtain an activator 3 suitable for rubber vulcanization reaction. Among them, the surface of the sulfur-doped carbon black carrier is loaded with zinc oxide sub-nano clusters 3 (denoted as ZnO-S-CB).

[0069] Example 4

[0070] Preparation process of sulfur-doped silica carrier:

[0071] Add 2g of white carbon black powder to 500mL of water at room temperature and stir until uniformly dispersed. Then add 0.25g of thiourea, raise the solution temperature to about 82°C, and continue stirring for 12 hours at a stirring speed of 850rpm. Filter and dry, and grind to obtain a sulfur-doped white carbon black carrier.

[0072] Weigh 1g of sulfur-doped silica carrier, add it to 200mL of water and stir evenly, then add 0.2g of zinc nitrate and 10mL of 0.1M sodium hydroxide solution, continue stirring for 12 hours, and keep the stirring speed at 900rpm. The obtained suspension was filtered and dried in an oven at 100°C for 12 hours to finally obtain an activator 4 suitable for rubber vulcanization reaction. Among them, the surface of the sulfur-doped silica carrier is loaded with zinc oxide sub-nano clusters 4 (denoted as ZnO-S-Silica).

[0073] Test example:

[0074] The activators suitable for rubber vulcanization reaction prepared in Examples 1 to 4 were used for performance testing experiments, and commercial ZnO nanoparticles (99.7%) were used as controls:

[0075] Analysis of the chemical properties of ZnO sub-nanoclusters 1~ZnO sub-nanoclusters 4 and commercial ZnO nanoparticles.

[0076] Table 1 shows the chemical property analysis parameters of Examples 1-4 and commercial ZnO (99.7%)

[0077]

[0078] As shown in Examples 1 to 4 in Table 1, the zinc content in the examples is lower than that in commercial zinc oxide, and the specific surface area is larger than that in commercial zinc oxide nanoparticles.

[0079] Vulcanized rubber was prepared using zinc oxide sub-nanoclusters 1 to 4, wherein the formula of the vulcanized rubber was as shown in Table 2.

[0080] Table 2 Vulcanized rubber formulations of Examples 1 to 4 and commercial ZnO (99.7%) (unit: phr)

[0081]

[0082] The zinc dosages of Examples 1 to 4 and commercial ZnO (99.7%) in Table 2 were calculated to be 0.784, 0.72, 0.96, 0.93 and 3.2 phr, respectively, based on the zinc content in Table 1. phr represents the dosage of zinc oxide to be added per 100 parts of natural rubber. Therefore, relative to commercial ZnO (99.7%), the zinc dosages in Examples 1 to 4 were reduced by 75.5%, 77.5%, 70.0% and 70.9%, respectively, thereby verifying that the zinc dosage can be reduced by 70-80%.

[0083] According to the rubber formula in Table 2 above, the rubber material was first mixed on a two-roll open mill, and then various additives (stearic acid, antioxidant 4010NA, accelerator NS, sulfur, etc.) were added to obtain a mixed rubber. Then, vulcanization was performed at 150°C according to the positive vulcanization time to obtain a vulcanized rubber. The tensile strength and elongation at break of the vulcanized rubber were tested according to the national standard GB / T528-2009, and the vulcanization performance of activator 1 to activator 4 was tested at 150°C using a vulcanizer. The performance comparison is shown in Table 3 below.

[0084] Table 3 Test parameters of sulfurization performance of Examples 1 to 4 and commercial ZnO (99.7%)

[0085]

[0086] M H and M L They are the maximum torque and the minimum torque respectively, and the larger the difference, the better the vulcanization effect. Ts2 represents the scorch time, and its effect on the vulcanization performance can be evaluated in conjunction with T90. T90 is the positive vulcanization time, and the shorter the time, the higher the activity of the activator. Ts2 represents the scorch time, and its effect on the vulcanization performance can be evaluated in conjunction with T90, and its vulcanization effect is mainly affected by the value of T90. As shown in Table 3, the maximum and minimum torque difference of Examples 1 to 4 is greater than the maximum and minimum torque difference of commercial zinc oxide particles, proving that the vulcanization effect of the activator prepared in the examples is higher than that of commercial zinc oxide particles. According to the comparison of T90, the positive vulcanization time of Examples 1 to 4 is shorter than the positive vulcanization time of commercial zinc oxide particles, indicating that the activity of the activator prepared in Examples 1 to 4 is higher than that of commercial products.

[0087] Mechanical and aging performance tests were performed on Examples 1 to 4 and commercial zinc oxide nanoparticles, and the aging test process conditions were: 100° C.×72 h.

[0088] Table 4 shows the mechanical and aging performance parameters of Examples 1 to 4 and commercial ZnO (99.7%)

[0089]

[0090] It can be seen from the data in Table 4 that the tensile strength and tensile elongation of the rubber product after vulcanization and aging of the activator 1 prepared in Example 1 are both the highest. In addition, the tensile strength and tensile elongation in Examples 1 to 4 are higher than those of commercial zinc oxide nanoparticles, indicating that the activators 1 to 4 provided by the present invention for rubber vulcanization reactions not only have excellent activity (shorter positive vulcanization time), but also can make the vulcanized rubber have excellent mechanical properties, and can reduce the consumption of zinc oxide by 70%-80%, thereby significantly saving metal resources and promoting sustainable development. In addition, the industrial application prospects of this material are broad and have important practical value.

[0091] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An activator for rubber vulcanization reaction, comprising: A carrier, wherein the carrier is a nanomaterial doped with a non-metallic element; Zinc oxide, anchored on the outer surface of the carrier; The zinc oxide is coordinated with the non-metallic elements doped on the outer surface of the carrier to form a single atomic layer in the form of fully exposed sub-nanometer clusters.

2. The activator according to claim 1, wherein The mass ratio of zinc oxide to the carrier is (0.5-10):

100.

3. The activator according to claim 1, wherein The nanomaterial includes at least one of carbon black, white carbon black or graphene oxide; The non-metallic element includes at least one of nitrogen, oxygen, phosphorus and boron; The particle size of the carbon black is 10-100 nm, and the specific surface area is 50-150 m 2 / g; the particle size of the white carbon black is 20~100nm, and the specific surface area is 100~300m 2 / g; the graphene oxide has a size of 1~10μm, a thickness of 3~10nm, and a specific surface area of ​​100~400m 2 / g.

4. The activator according to claim 3, wherein The doping amount of the non-metallic element accounts for 0.5-5% of the mass percentage of the nano material.

5. A method for preparing an activator as claimed in any one of claims 1 to 4, comprising: dispersing the carrier in the first solvent to obtain a dispersed solution; Adding zinc metal salt and alkaline solution to the dispersed solution to carry out a hydrolysis reaction to obtain the activator; Wherein, the carrier is a nano material doped with non-metallic elements.

6. The preparation method according to claim 5, wherein: The alkaline solution includes any one of a sodium hydroxide aqueous solution, a lithium hydroxide aqueous solution, and a potassium hydroxide aqueous solution.

7. The preparation method according to claim 5, wherein: The temperature of the hydrolysis reaction is 15-25°C.

8. The preparation method according to claim 5, wherein Before dispersing the carrier in the first solvent, the method further comprises: Dispersing the nanomaterial in a second solvent, adding a non-metallic compound, mixing and stirring to react, to obtain the carrier; The non-metallic compound includes any one of a nitrogen-containing compound, a sulfur-containing compound, a boron-containing compound, and a phosphorus-containing compound.

9. The preparation method according to claim 8, wherein: The temperature of the mixing and stirring reaction is 80-85°C.

10. Use of the activator as claimed in any one of claims 1 to 4 in a rubber vulcanization reaction.

Citation Information

Patent Citations

  • Zinc oxide vulcanizing agent for carboxyl rubber and preparation method thereof

    CN112280132A

  • Vulcanization activator and preparation method thereof

    CN116355455A

  • Active zinc oxide for rubber vulcanization

    FR600405A

  • vulcanization

    GB1447115A