Rubber composite material for plate spring rubber support

By optimizing the formula using cerium oxide hybrid fillers, organic antioxidants and silane coupling agents in rubber composite materials, the aging problem of natural rubber in harsh environments is solved, the service life is extended and the flexural resistance is improved. Fatigue performance enables high performance bearing materials under high temperature conditions.

CN118725425APending Publication Date: 2024-10-01SINO TRUK JINAN POWER CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411000138.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Natural rubber composite materials are prone to aging in harsh environments, resulting in a shortened service life of leaf spring rubber bearings. Existing organic antioxidants are prone to enrichment and migration, making it difficult to maintain long-term protective effects and improve flex fatigue resistance. .

Method used

A combination of cerium oxide hybrid filler and organic antioxidant is used to optimize the formula through ingredients such as silane coupling agent and carbon black to improve the anti-aging and flex fatigue resistance of the rubber. The cerium oxide hybrid filler is prepared through a specific process to slow down the aging process. Releases cerium oxide and enhances the mechanical properties of rubber.

Benefits of technology

Significantly prolongs the anti-aging time of rubber composite materials, improves its resistance to flexural fatigue, ensures the maintenance of service life under high temperature conditions, and improves the tensile strength and elongation at break of rubber products, meeting the requirements of leaf spring rubber Support requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of polymer rubber materials, in particular to a rubber composite material for a plate spring rubber support, which is prepared from the following raw materials in parts by mass: 100 parts of composite rubber, 2 to 10 parts of cerium oxide hybrid filler, 1 to 5 parts of silane coupling agent, 1 to 4 parts of anti-aging agent, 30 to 60 parts of carbon black, 3 to 8 parts of zinc oxide, 2 to 4 parts of stearic acid, 1 to 3 parts of vulcanizing agent and 1 to 2 parts of accelerant. The rubber raw material contains the cerium oxide hybrid filler, the hybrid filler has the effect of slowly releasing cerium oxide, and meanwhile, the service life of a rubber composite product can be effectively prolonged by utilizing the free radical scavenging capacity of cerium oxide and the crack growth prevention performance of the hybrid filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer rubber materials, and in particular to a rubber composite material for a leaf spring rubber bearing. Background Art

[0002] The vehicle damping shock absorbing element is an indispensable part of the vehicle shock absorption system, which can effectively reduce the vibration and noise generated during the operation of the vehicle and improve the comfort of the driver and passengers. The leaf spring shock absorption structure is a common vehicle shock absorption structure, in which the support connecting the leaf spring and the frame plays a role in supporting and further reducing small vibrations. In the leaf spring support, rubber is an important component.

[0003] Rubber is a viscoelastic material with reversible deformation characteristics at room temperature. It can produce large deformation under small stress conditions, and the deformation can be fully or partially restored. At the same time, during the production process, rubber has strong fluidity at high temperatures, and the shape design is simple and controllable, which can meet the shape requirements of most products. In addition, rubber materials can be designed and studied through formulation. Among them, natural rubber is an ideal matrix for rubber composite materials for shock-absorbing bearings because of its good mechanical properties and high resilience. However, due to the weak aging resistance of natural rubber and the harsh working environment of leaf spring rubber bearings, which need to be exposed to sunlight all year round, and the fact that they are dynamic products, repeated compression deformation further aggravates the aging behavior of rubber, which eventually leads to cracking of the rubber, loss of use value of the bearing, and increased enterprise costs. Therefore, it is of great significance to improve the heat-oxidative aging resistance and flexural fatigue resistance of natural rubber composite materials.

[0004] At present, the main way to improve the thermal oxidation aging and flexural fatigue resistance of natural rubber is to add amines, phenols or other types of chemical antioxidants, which can react with oxygen to slow down the aging of rubber. However, organic antioxidants are very likely to be enriched and migrated out during the use of products, resulting in a decrease in protective ability and pollution to the environment, and it is difficult to maintain the protective effect for a long time. Therefore, non-organic antioxidants have received widespread attention. Nano-cerium oxide has excellent free radical capture ability, effectively removes free radicals generated during the aging process of rubber, and can significantly improve the thermal oxidation aging resistance of rubber materials. In addition, a large number of studies have shown that the addition of inorganic nanoparticles can improve the crack propagation resistance of dynamic rubber products. Summary of the invention

[0005] In view of the technical problems that organic antioxidants are easily enriched and migrated out during the use of products, thereby reducing the protection time, the purpose of the present invention is to provide a rubber composite material for leaf spring rubber bearings, which has the technical effect of extending the anti-aging time of the rubber composite material and improving the flexural fatigue resistance of the rubber composite material.

[0006] The invention provides a rubber composite material for a leaf spring rubber bearing, comprising the following raw materials in parts by mass: 100 parts of composite rubber, 2-10 parts of cerium oxide hybrid filler, 1-5 parts of silane coupling agent, 1-4 parts of antioxidant, 30-60 parts of carbon black, 3-8 parts of zinc oxide, 2-4 parts of stearic acid, 1-3 parts of vulcanizing agent and 1-2 parts of accelerator.

[0007] Furthermore, the composite rubber includes natural rubber and styrene-butadiene rubber, and the percentage ratio of natural rubber to styrene-butadiene rubber is 50%~80%:20%~50%.

[0008] Furthermore, the preparation method of the cerium oxide hybrid filler comprises: S1. dissolving silicotungstic acid in hydrochloric acid to obtain a silicotungstic acid solution; S2, dispersing nano-cerium oxide in water, and ultrasonically treating the water to obtain a nano-cerium oxide dispersion; S3, mixing the silicotungstic acid solution and the nano-cerium oxide dispersion, and placing them in a reactor for hydrothermal reaction; S4, taking out the hydrothermal reaction product in step S3, performing heat treatment, washing the product after the heat treatment, and obtaining a cerium oxide hybrid filler.

[0009] Furthermore, the mass ratio of silicotungstic acid to nano-cerium oxide is 5:1.

[0010] Furthermore, in step S3, the process conditions of the hydrothermal reaction are: reaction temperature is 150° C., and reaction time is 1 h.

[0011] Furthermore, in step S4, the process conditions of the heat treatment are that the hydrothermal reaction product is heat treated at temperatures of 60° C. and 120° C. for 24 hours respectively.

[0012] Furthermore, the silane coupling agent is bis-(γ-triethoxysilylpropyl) tetrasulfide or bis-[3-(triethoxysilyl)propyl]-disulfide. The effect is that both silane coupling agents are suitable for the composite material containing natural rubber of the present invention, and can effectively improve the bonding ability between fillers and rubber molecules, and improve the mechanical properties and flexural fatigue resistance of rubber.

[0013] Furthermore, the antioxidant includes N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine and 2,6-di-tert-butyl-4-methylphenol in a mass ratio of 2:1:1. The antioxidant is an organic antioxidant, which forms a balanced ratio system with the cerium oxide hybrid filler in the components of the present invention, comprehensively improves the anti-aging ability of the rubber, and prolongs the service life of the product.

[0014] Furthermore, the vulcanizing agent includes sulfur and diisopropylbenzene peroxide in a mass ratio of 1:1.5; the accelerator includes N-tert-butyl-2-benzothiazolesulfonamide and dimethyl disulfide dithiocarbonylamine in a mass ratio of 10:1. The role of the accelerator is to increase the strength of the rubber cross-linking network and improve the rubber's resistance to deformation.

[0015] Furthermore, the carbon black includes carbon black N330 and carbon black N550 in a mass ratio of 1:2.5. The compounding of the two carbon blacks can effectively balance the reinforcement effect and the elasticity of the rubber. The elasticity affects the rubber's resistance to compression deformation, resistance to flexural fatigue, etc.

[0016] The beneficial effects of the present invention are as follows: the rubber raw material of the present invention contains a cerium oxide hybrid filler, and the hybrid filler has the effect of slow-release cerium oxide. The free radical scavenging ability of cerium oxide and the performance of the hybrid filler in preventing crack growth can effectively improve the service life of rubber products. The rubber composite material product prepared by the present invention has a tensile strength of >21.0MPa and an elongation at break of >380%. The retention rates of the tensile strength and elongation at break after hot air aging for 70 hours at 100°C are both above 87%. After 40,000 times of flexion fatigue test, no secondary cracks appear, which meets the requirements of rubber composite materials for leaf spring rubber bearings. DETAILED DESCRIPTION

[0017] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0018] The preparation method of the cerium oxide hybrid filler in the following embodiment is as follows: first, 5.0g of silicotungstic acid is dissolved in 20mL of hydrochloric acid with a concentration of 2mol / L to obtain a silicotungstic acid solution. Then, 1.0g of nano-cerium oxide powder is dispersed in 20mL of deionized water and ultrasonically dispersed at a power of 500W for 1 hour to obtain a nano-cerium oxide dispersion. Then, the silicotungstic acid solution is added to the nano-cerium oxide dispersion to obtain a mixed solution, and the obtained mixed solution is stirred for 1 hour, and then hydrothermally reacted in a reactor at 150°C for 24 hours. After the hydrothermal reaction is completed, the reactor liner is taken out and continued to be treated at 60°C and 120°C for 24 hours respectively. After that, the reaction product is washed 3 times with 1.0M sulfuric acid and deionized water respectively, dried, and the white powder collected is a cerium oxide hybrid filler.

[0019] Example 1 A rubber composite material for a leaf spring rubber bearing is prepared from the following raw materials in parts by mass: 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 5 parts of cerium oxide hybrid filler, 1.5 parts of bis-(γ-triethoxysilylpropyl) tetrasulfide (silane coupling agent), 2 parts of antioxidant, 45 parts of carbon black, 5 parts of zinc oxide, 3 parts of stearic acid, 2 parts of vulcanizing agent, and 1 part of accelerator.

[0020] Among them: the antioxidant includes N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine and 2,6-di-tert-butyl-4-methylphenol in a mass ratio of 2:1:1; the carbon black includes carbon black N330 and carbon black N550 in a mass ratio of 1:2.5; the vulcanizing agent includes sulfur and diisopropylbenzene peroxide in a mass ratio of 1:1.5; the accelerator includes N-tert-butyl-2-benzothiazole sulfonamide and dimethyl disulfide dithiocarbonylamine in a mass ratio of 10:1.

[0021] The preparation method of the rubber composite material in Example 1 includes: putting natural rubber on an open mill, thinning it 8 times, then adding styrene-butadiene rubber and mixing it evenly. Adding zinc oxide and stearic acid and mixing it evenly, adding an antioxidant, a cerium oxide hybrid filler, a silane coupling agent and carbon black in sequence, and adding a vulcanizing agent and an accelerator after mixing evenly. After mixing, the obtained mixed rubber is left for more than 16 hours, and its vulcanization curve is tested at 150°C, and then vulcanized on a flat vulcanizer according to the positive vulcanization time to obtain a rubber composite material.

[0022] Example 2 A rubber composite material for a leaf spring rubber bearing is prepared from the following raw materials in parts by mass: 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 2 parts of cerium oxide hybrid filler, 1 part of bis-(γ-triethoxysilylpropyl) tetrasulfide (silane coupling agent), 1 part of antioxidant, 30 parts of carbon black, 3 parts of zinc oxide, 2 parts of stearic acid, 2 parts of vulcanizing agent, and 1 part of accelerator.

[0023] Example 2 The preparation method of the rubber composite material is the same as that of Example 1.

[0024] Example 3 A rubber composite material for a leaf spring rubber bearing is prepared from the following raw materials in parts by mass: 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 10 parts of cerium oxide hybrid filler, 5 parts of bis-(γ-triethoxysilylpropyl) tetrasulfide (silane coupling agent), 4 parts of antioxidant, 60 parts of carbon black, 8 parts of zinc oxide, 4 parts of stearic acid, 1 part of vulcanizing agent, and 2 parts of accelerator.

[0025] The preparation method of the rubber composite material in Example 3 is the same as that in Example 1.

[0026] Example 4 A rubber composite material for a leaf spring rubber bearing is prepared from the following raw materials in parts by mass: 50 parts of natural rubber, 50 parts of styrene-butadiene rubber, 5 parts of cerium oxide hybrid filler, 1.5 parts of bis-[3-(triethoxysilyl)propyl]-disulfide (silane coupling agent), 2 parts of antioxidant, 45 parts of carbon black, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of vulcanizing agent, and 1.5 parts of accelerator.

[0027] Example 4 The preparation method of the rubber composite material is the same as that of Example 1.

[0028] Example 5 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 2 parts of cerium oxide hybrid filler, 1.5 parts of bis-[3-(triethoxysilyl)propyl]-disulfide (silane coupling agent), 2 parts of antioxidant, 45 parts of carbon black, 5 parts of zinc oxide, 2 parts of stearic acid, 3 parts of vulcanizing agent, and 2 parts of accelerator.

[0029] Example 5 The preparation method of the rubber composite material is the same as that of Example 1.

[0030] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the cerium oxide hybrid filler is replaced by nano cerium oxide.

[0031] Comparative Example 2 Comparative Example 2 is different from Example 1 in that it does not contain cerium oxide hybrid filler.

[0032] The properties of the rubber composite products prepared in each embodiment and comparative example were tested. The testing methods included: tensile performance test (GB / T 528-2009), hot air aging test (100°C×70h, GB / T3512-2014) and flexural fatigue test (GB / T 13934-2006) in accordance with the corresponding national standards.

[0033] Table 1 Performance test data of rubber products obtained in various embodiments and comparative examples

[0034] It can be seen from Table 1 that the rubber product prepared in the present invention has a tensile strength of >21.0 MPa and an elongation at break of >380%. The retention rates of the tensile strength and elongation at break after hot air aging for 70 hours at 100°C are both above 87%. No secondary cracks appear in the flexure fatigue test after 40,000 times, thus meeting the requirements of rubber composite materials for leaf spring rubber bearings.

[0035] At the same time, it can be seen from the comparative data of the embodiments and comparative examples that the cerium oxide hybrid filler prepared by the present invention can improve the performance of rubber products, has a more excellent anti-aging effect in the same time, and prolongs the anti-aging time of the rubber composite material, indicating that the hybrid filler prepared by the present invention has the effect of slow-release cerium oxide. At the same time, the flexural fatigue test of the rubber product prepared by the present invention increases the occurrence of secondary cracks from 30,000 times to 40,000 times, thereby improving the flexural fatigue resistance of the rubber composite material.

[0036] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.

Claims

1. A rubber composite material for a leaf spring rubber bearing, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of composite rubber, 2-10 parts of cerium oxide hybrid filler, 1-5 parts of silane coupling agent, 1-4 parts of antioxidant, 30-60 parts of carbon black, 3-8 parts of zinc oxide, 2-4 parts of stearic acid, 1-3 parts of vulcanizing agent and 1-2 parts of accelerator.

2. The rubber composite material for a leaf spring rubber bearing according to claim 1, characterized in that: The composite rubber includes natural rubber and styrene-butadiene rubber, and the percentage of natural rubber to styrene-butadiene rubber is 50%~80%:20%~50%.

3. The rubber composite material for a leaf spring rubber bearing according to claim 1, characterized in that: The preparation method of the cerium oxide hybrid filler comprises: S1. dissolving silicotungstic acid in hydrochloric acid to obtain a silicotungstic acid solution; S2, dispersing nano-cerium oxide in water, and ultrasonically treating the water to obtain a nano-cerium oxide dispersion; S3, mixing the silicotungstic acid solution and the nano-cerium oxide dispersion, and placing them in a reactor for hydrothermal reaction; S4, taking out the hydrothermal reaction product in step S3, performing heat treatment, washing the product after the heat treatment, and obtaining a cerium oxide hybrid filler.

4. The rubber composite material for a leaf spring rubber bearing according to claim 3, characterized in that: The mass ratio of silicotungstic acid to nano-cerium oxide is 5:

1.

5. The rubber composite material for a leaf spring rubber bearing according to claim 3, characterized in that: In step S3, the process conditions of the hydrothermal reaction are: reaction temperature is 150° C., and reaction time is 1 h.

6. The rubber composite material for a leaf spring rubber bearing according to claim 3, characterized in that: In step S4, the process conditions of heat treatment are that the hydrothermal reaction product is heat treated at temperatures of 60° C. and 120° C. for 24 hours respectively.

7. The rubber composite material for a leaf spring rubber bearing according to claim 1, characterized in that: The silane coupling agent is bis-(γ-triethoxysilylpropyl)tetrasulfide or bis-[3-(triethoxysilyl)propyl]-disulfide.

8. The rubber composite material for a leaf spring rubber bearing according to claim 1, characterized in that: The antioxidant comprises N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine and 2,6-di-tert-butyl-4-methylphenol in a mass ratio of 2:1:

1.

9. The rubber composite material for a leaf spring rubber bearing according to claim 1, characterized in that: The vulcanizing agent includes sulfur and dicumyl peroxide in a mass ratio of 1:1.5; the accelerator includes N-tert-butyl-2-benzothiazole sulfenamide and dimethyl disulfide bisthiocarbonylamine in a mass ratio of 10:

1.

10. The rubber composite material for a leaf spring rubber bearing according to claim 1, characterized in that: The carbon black includes carbon black N330 and carbon black N550 in a mass ratio of 1:2.5.

Citation Information

Cited By

  • High-wear-resistance carbon fiber reinforced nano cerium dioxide / butadiene styrene rubber composite material and preparation method thereof

    CN120737455A