High-bending-resistance ceramic material for 5G communication base station and preparation method of high-bending-resistance ceramic material

The anti-bending sintering additive and HA-coated sintering powder were prepared by blending and calcining, and combined with SrTa2O6 and BaTi4O9 blending sintering, the problem of excessive grains and poor dielectric properties of ceramic materials during high-temperature sintering is solved, and high resistance is achieved The preparation of ceramic materials with bent and low dielectric constants improves the flexural strength and dielectric properties of ceramics.

CN118930228AActive Publication Date: 2024-11-12XINHUA COUNTY SHUNDA ELECTRONIC CERAMICS CO LTD

Patent Information

Application Number
CN202411436217.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-12
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

During the high-temperature sintering process, existing ceramic materials are prone to excessive grain size and decrease in strength, and the dielectric performance of low-temperature co-soluble sintering additives is poor, affecting the strength and dielectric properties of the ceramic.

Method used

The anti-bending sintering additives were prepared by blending and calcining of Li2CO3, SiO2, Bi2O3 and Al2O3, and calcined, and HA coated sintered powder was prepared by ball milling of B2O3, CaCO3 and zirconia. SrTa2O6 was prepared and mixed with BaTi4O9 was prepared by combining Ta2O5 and Sr(NO3)2. , low temperature and high temperature sintering is carried out to improve the bending and dielectric properties of the ceramic.

Benefits of technology

It effectively reduces the pore problems caused by grain growth, improves the density and bending strength of the ceramics, and improves the dielectric properties, ensuring that the bending resistance of the ceramic materials during high-temperature sintering is not reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930228A_ABST
    Figure CN118930228A_ABST
Patent Text Reader

Abstract

The invention relates to the field of ceramic materials, in particular to a high-bending-resistance ceramic material for a 5G communication base station and a preparation method of the high-bending-resistance ceramic material. Comprising the following steps: calcining and preparing an anti-bending sintering aid; preparing HA coated ceramic sintering powder; and compounding the ceramic particles and carrying out compression column sintering. According to the invention, a polyacrylamide / L-dopamine film is used as an organic template for inducing HA mineralization, so that an ordered structure is formed by HA crystals, the crystals have good mechanical properties, the problem that pores are generated in the ceramic due to grain growth is effectively reduced, the density of the ceramic is improved, and the service life of the ceramic is prolonged. And moreover, some pores and cracks are inevitably generated in the sintering process of the ceramic green body, when the finished ceramic is subjected to an external load, the cracks continuously expand, and at the moment, the HA crystals meet the cracks to consume the energy of the external load, so that the strength of the ceramic is enhanced, and the bending resistance of the ceramic material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of ceramic materials, and in particular to a high-bending-resistance ceramic material for a 5G communication base station and a preparation method thereof. Background Art

[0002] With the rapid development of 5G communication technology, higher requirements are placed on the core materials in communication base stations. 5G communication base stations need to process higher frequency signals, larger capacity data transmission, and require the equipment to have a smaller size, higher reliability and longer service life. In this context, high-εr microwave materials that limit the transmission of electromagnetic wave energy, as well as printed circuit boards (PCBs) and metals with large losses will no longer be the preferred materials for promoting the development of mobile communication technology towards higher frequencies. Microwave dielectric ceramics with high Q·f and low dielectric constants have attracted much attention and research. When used as a substrate, this type of material can effectively increase the signal transmission rate and significantly reduce the loss of signal energy in the microwave and millimeter wave bands.

[0003] Common low dielectric constant materials include silicates, phosphates, aluminates and borates. These ceramic materials often need to be sintered at high temperatures, which can easily cause the ceramic grains to be too large, resulting in a serious decrease in the strength of the ceramic materials. Even if the sintering temperature can be lowered by adding low-temperature eutectic sintering aids, most low-temperature eutectic sintering aids have poor dielectric properties and are prone to mutual repulsion with ceramic materials, which not only affects the strength of the ceramics, but also causes a decrease in dielectric properties. Summary of the invention

[0004] In order to solve the above-mentioned technical defects, the present invention has developed a high-bending-resistance ceramic material for 5G communication base stations which has low dielectric constant, high quality factor and high bending resistance, and a preparation method thereof.

[0005] A method for preparing a high bending resistance ceramic material for a 5G communication base station comprises the following steps: S1: Calcination preparation of bending-resistant sintering aid Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 Perform mixed ball milling to obtain a mixed slurry, dry and grind the mixed slurry, sieve the mixed slurry to obtain a mixed fine powder, calcine the mixed fine powder in a muffle furnace, anneal the mixed fine powder quickly, grind the mixed fine powder, sieve the mixed fine powder to obtain a bending-resistant sintering aid; S2: Preparation of HA-coated ceramic sintered powder B 2 O 3 、CaCO 3, anhydrous ethanol and zirconium oxide balls are placed in a ball mill and milled, and then sintered at high temperature after being screened to obtain sintered powder. An aqueous solution of trishydroxymethylaminomethane is placed in a container, polyacrylamide and L-dopamine are added after adjusting the pH, and ultrasonic treatment is performed after stirring to obtain a coating solution. The sintered powder is immersed in the coating solution, filtered and dried to obtain a coated sintered powder, and then the coated sintered powder is immersed in CaCl 2 Buffer, washed and immersed in Na 2 HPO 4 The mixture was washed in a buffer solution, immersed in sodium dodecyl sulfate, and air-dried to obtain HA grain-coated sintered powder; S3: Composite and sintering of ceramic particles Will Ta 2 O 5 and Sr(NO 3 ) 2 Place in a container, add cyclohexane, seal, heat, and filter to obtain SrTa 2 O 6 , weigh HA grain-coated sintered powder, SrTa 2 O 6 and BaTi 4 O 9 , first SrTa 2 O 6 and BaTi 4 O 9 The mixture is ball-milled to obtain a dielectric performance enhancing material, the weighed HA grain-coated sintered powder and the dielectric performance enhancing material are placed in a mortar, and then a bending resistance sintering aid and polyvinyl alcohol are added for grinding, and ceramic particles are obtained after sieving, and the ceramic particles are pressed into a column and first sintered at a low temperature and then sintered at a high temperature, and after cooling, a high bending resistance and low dielectric constant ceramic material is obtained.

[0006] Furthermore, step S1, calcination preparation of the bending-resistant sintering aid, comprises the following steps: S1.1: Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 Place in a ball mill, add an equal amount of deionized water and mix and ball mill for 3-4 hours, set the ball mill speed to 250-300rpm, to obtain a mixed slurry, dry the mixed slurry and grind it, and pass it through a 100-120 mesh sieve to obtain a mixed fine powder; S1.2: The mixed fine powder is placed in a muffle furnace and calcined at a temperature of 1200-1300°C for 4-4.5 hours. After being taken out, it is quickly put into cold water for annealing. After grinding, it is passed through a 100-120 mesh sieve to obtain a bending-resistant sintering aid.

[0007] Furthermore, step S2 prepares HA-coated ceramic sintered powder, comprising the following steps: S2.1: Weigh B with a molar ratio of 1:(2.4-2.6) 2 O 3 and CaCO 3 The raw materials are mixed with anhydrous ethanol and zirconium oxide balls in a mass ratio of 1: (1-1.5): (2-2.5) and added into a ball mill, the speed is adjusted to 250-300 rpm for ball milling for 6-8 hours, and after passing through an 80-100 mesh sieve, the mixture is placed in a muffle furnace and heated to 1000-1100° C. at a heating rate of 5-6° C. / min, and the temperature is maintained for sintering for 8-10 hours to obtain a sintered powder; S2.2: 80-100 parts by weight of an aqueous solution of tris(hydroxymethyl)aminomethane with a concentration of 8-10 g / L is placed in a container, the pH is adjusted to 8-8.5, and then 0.1-0.3 parts by weight of polyacrylamide and 0.2-0.3 parts by weight of levodopa are added, and after stirring for 30-35 minutes, ultrasonic treatment is performed at an ultrasonic frequency of 20-25 kHz for 50-60 minutes to obtain a coating solution, and the sintered powder is immersed in the coating solution for 25-30 minutes, and filtered and dried to obtain a coated sintered powder; S2.3: Immerse the coated sintered powder in CaCl 2 Buffer for 20-25 minutes, rinse 1-2 times with deionized water and immerse in Na 2 HPO 4 The mixture was placed in a buffer solution, allowed to stand for 20-25 minutes, then rinsed with deionized water 1-2 times, and then immersed in sodium dodecyl sulfate, allowed to stand at room temperature for 1-1.5 hours, and air-dried to obtain HA grain-coated sintered powder.

[0008] Furthermore, step S3 of compounding and sintering ceramic particles into a pressed column comprises the following steps: S3.1: Ta 2 O 5 and Sr(NO 3 ) 2 Mix in a container at a molar ratio of 1: (1-1.2), then add 15-20 times the mass of cyclohexane, seal and heat to 400-450°C for 1-1.5 hours, and filter to obtain SrTa 2 O 6 ; S3.2: Weigh HA grain-coated sintered powder and SrTa in a mass ratio of 1: (0.02-0.03): (0.02-0.03) 2 O 6 and BaTi 4 O 9 , the weighed SrTa2 O 6 and BaTi 4 O 9 Place in a ball mill, add 1.5-2 times the weight of anhydrous ethanol and 2.5-3 times the weight of zirconia balls with a diameter of 2-3 mm, and ball mill at a ball milling speed of 250-300 rpm for 4-5 hours to obtain a dielectric performance enhancing material, place the weighed HA grain-coated sintered powder and the dielectric performance enhancing material in a mortar, add 2-3wt% of a bending resistance sintering aid and 18-20wt% of polyvinyl alcohol, grind until uniform spherical small particles are formed, and pass through a 95-100 mesh sieve to obtain ceramic particles; S3.3: Place the ceramic particles in a die, use a tablet press to apply a pressure of 8-10MPa, maintain for 30-40 seconds to obtain a columnar ceramic green body, place the columnar ceramic green body in a box-type resistance furnace and heat it to 500-600℃ at a heating rate of 1-1.5℃ / min, then place it in a muffle furnace and heat it to 780-800℃ at a heating rate of 4-5℃ / min, keep it warm for 6-8 hours, and naturally cool it in the furnace to obtain a high bending resistance and low dielectric constant ceramic material.

[0009] Furthermore, in step S1.1, Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 The molar ratio is 1:1:1:(0.2-0.3).

[0010] Furthermore, the zirconia balls in step 2.1 are composed of zirconia balls with a diameter of 6 mm and zirconia balls with a diameter of 3 mm in a mass ratio of 1:(0.4-0.6).

[0011] Furthermore, the method for adjusting the pH in step S2.2 is to add a hydrochloric acid solution.

[0012] Furthermore, in step S2.3, CaCl 2 The concentration of the buffer is 55-60 g / L, the pH is 7.5-8, and the Na 2 HPO 4 The concentration of the buffer is 35-40 g / L and the pH is 8.5-9.

[0013] Furthermore, the columnar ceramic green body in step S3.3 has a height of 6-8 mm and a diameter of 10-12 mm.

[0014] A high bending-resistance ceramic material for a 5G communication base station is prepared by the above-mentioned method for preparing a high bending-resistance ceramic material for a 5G communication base station.

[0015] The beneficial effects are as follows: 1. The present invention firstly 2 O 3 and CaCO 3 After mixing and grinding, sintering is performed to obtain sintered powder. At this time, Ca is initially formed in the sintered powder. 3 (BO 3 ) 2 The main crystal phase determines the formation direction of the main crystal phase in the subsequent sintering process. Then, a layer of polyacrylamide / L-dopamine film is covered on the surface of the sintered powder as an organic template for subsequent induction of HA mineralization, which ensures that the subsequent HA crystals form an ordered structure and obtain good mechanical properties. In the subsequent sintering process, the HA crystals can not only play a pinning role at the grain boundary, inhibit the movement of the grain boundary, but also prevent Ca 3 (BO 3 ) 2 The growth of ceramic grains effectively reduces the problem of porosity in ceramics caused by grain growth and improves the density of ceramics. In addition, since some pores and cracks are inevitable in the sintering process of the ceramic green body, when the finished ceramic is subjected to an external load, the cracks will continue to expand. When they meet HA crystals with good mechanical properties, they can consume the energy of the external load, thereby enhancing the strength of the ceramic. In summary, the bending resistance of the ceramic material is greatly improved.

[0016] 2. The present invention first passes Ta 2 O 5 and Sr(NO 3 ) 2 Preparation of SrTa 2 O 6 Then with BaTi 4 O 9 The dielectric performance enhancement material is obtained by ball milling. When the HA grain-coated sintered powder is first sintered at low temperature and then sintered at high temperature, the polyacrylamide and L-dopamine in the HA grain-coated sintered powder and the polyvinyl alcohol in the ceramic particles are first discharged by the low temperature sintering, and then the Sr with similar ionic radius and lattice energy is sintered by high temperature. 2+ , Ba 2+ and Ca 2+ They can be doped and replaced with each other without causing distortion of the lattice structure, thus greatly reducing the SrTa 2 O 6 and BaTi 4 O 9 With Ca 3 (BO 3 ) 2 The repulsive ability of the main crystal phase will not only not reduce the bending resistance of the ceramic material, but also 2 O 6and BaTi 4 O 9 It has excellent dielectric properties itself and can also improve the dielectric properties of ceramic materials.

[0017] 3. The present invention will Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 The bending sintering aid was obtained by mixing and calcining. 2 CO 3 Decomposes to generate Li during the sintering process 2 O, can be combined with SiO 2 and Bi 2 O 3 The formation of low eutectic, these low eutectic has a lower melting point, which helps to reduce the overall temperature of subsequent sintering, thereby reducing excessive grain growth and thermal stress of ceramic materials, and adding high-strength Al 2 O 3 The particles serve as a reinforcement phase and can be 2 O 3 and Li 2 The liquid phase generated by O fills the gaps between the grains, improving the density and strength of the ceramic material, thereby further enhancing the bending strength of the ceramic material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a flow chart of the method for preparing high bending-resistant ceramic materials for 5G communication base stations adopted in an embodiment of the present invention. DETAILED DESCRIPTION

[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Embodiment 1: A high bending resistance ceramic material for 5G communication base station and a preparation method thereof, such as Figure 1 As shown, the following steps are included: S1: Calcination preparation of bending-resistant sintering aid S1.1: Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al2 O 3 The mixture was placed in a ball mill at a molar ratio of 1:1:1:0.2, and an equal amount of deionized water was added and mixed and ball milled for 3 hours. The ball mill speed was set to 250 rpm to obtain a mixed slurry. The mixed slurry was dried and then ground, and passed through a 100-mesh sieve to obtain a mixed fine powder. S1.2: The mixed fine powder is placed in a muffle furnace and calcined at 1200°C for 4 hours. After being taken out, it is quickly put into cold water for annealing. After grinding, it is passed through a 100-mesh sieve to obtain a bending-resistant sintering aid.

[0021] S2: Preparation of HA-coated ceramic sintered powder S2.1: Weigh B with a molar ratio of 1:2.4 2 O 3 and CaCO 3 The raw materials are mixed with anhydrous ethanol and zirconium oxide balls in a mass ratio of 1:1:2 and added into a ball mill, wherein the zirconium oxide balls are composed of zirconium oxide balls with a diameter of 6 mm and zirconium oxide balls with a diameter of 3 mm in a mass ratio of 1:(0.4-0.6), the rotation speed is adjusted to 250 rpm for ball milling for 6 hours, and after passing through an 80-mesh sieve, the mixture is placed in a muffle furnace and heated to 1000°C at a heating rate of 5°C / min, and the temperature is maintained for sintering for 8 hours to obtain a sintered powder; S2.2: 80 parts by mass of an aqueous solution of tris(hydroxymethyl)aminomethane with a concentration of 8 g / L is placed in a container, a hydrochloric acid solution is added to adjust the pH to 8, and then 0.1 parts by mass of polyacrylamide and 0.2 parts by mass of levodopa are added, and after stirring for 30 minutes, ultrasonic treatment is performed at an ultrasonic frequency of 20 kHz for 50 minutes to obtain a coating solution, and the sintered powder is immersed in the coating solution for 25 minutes, and filtered and dried to obtain a coated sintered powder; S2.3: Immerse the coated sintered powder in a CaCl solution with a concentration of 55 g / L and a pH of 7.5. 2 The samples were immersed in the buffer for 20 minutes, rinsed with deionized water once, and then immersed in 35 g / L Na2O3 at a pH of 8.5. 2 HPO 4 The sample was placed in a buffer solution, allowed to stand for 20 minutes, then rinsed with deionized water once, and then immersed in sodium dodecyl sulfate, allowed to stand at room temperature for 1 hour, and air-dried to obtain HA grain-coated sintered powder.

[0022] S3: Composite and sintering of ceramic particles S3.1: Ta 2 O 5 and Sr(NO 3 ) 2 Mix them in a 1:1 molar ratio in a container, then add 15 times the mass of cyclohexane, seal and heat to 400°C for 1 hour, and filter to obtain SrTa 2 O6 ; S3.2: Weigh HA grain-coated sintered powder and SrTa in a mass ratio of 1:0.02:0.02 2 O 6 and BaTi 4 O 9 , the weighed SrTa 2 O 6 and BaTi 4 O 9 The mixture was placed in a ball mill, 1.5 times the weight of anhydrous ethanol and 2.5 times the weight of zirconia balls with a diameter of 2 mm were added, and the mixture was ball-milled at a ball-milling speed of 250 rpm for 4 hours to obtain a dielectric performance enhancing material. The weighed HA grain-coated sintered powder and the dielectric performance enhancing material were placed in a mortar, and 2 wt % of a bending sintering aid and 18 wt % of polyvinyl alcohol were added and ground until uniform spherical small particles were formed, and the particles were passed through a 95 mesh sieve to obtain ceramic particles. S3.3: Place the ceramic particles in a die, use a tablet press to apply a pressure of 8 MPa, hold for 30 seconds, and obtain a columnar ceramic green body with a height of 6 mm and a diameter of 10 mm. Place the columnar ceramic green body in a box-type resistance furnace and heat it to 500°C at a heating rate of 1°C / min, then place it in a muffle furnace and heat it to 780°C at a heating rate of 4°C / min, keep warm for 6 hours, and naturally cool in the furnace to obtain a high bending resistance and low dielectric constant ceramic material.

[0023] Embodiment 2: A high bending resistance ceramic material for 5G communication base station and a preparation method thereof, such as Figure 1 As shown, the following steps are included: S1: Calcination preparation of bending-resistant sintering aid S1.1: Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 The mixture was placed in a ball mill at a molar ratio of 1:1:1:0.3, and an equal amount of deionized water was added and mixed and ball milled for 3 hours. The ball mill speed was set to 250 rpm to obtain a mixed slurry. The mixed slurry was dried and then ground, and passed through a 100-mesh sieve to obtain a mixed fine powder. S1.2: The mixed fine powder is placed in a muffle furnace and calcined at 1200°C for 4 hours. After being taken out, it is quickly put into cold water for annealing. After grinding, it is passed through a 100-mesh sieve to obtain a bending-resistant sintering aid.

[0024] S2: Preparation of HA-coated ceramic sintered powder S2.1: Weigh B with a molar ratio of 1:2.6 2 O 3and CaCO 3 The raw materials are mixed with anhydrous ethanol and zirconium oxide balls in a mass ratio of 1:1.5:2.5, and added into a ball mill, wherein the zirconium oxide balls are composed of zirconium oxide balls with a diameter of 6 mm and zirconium oxide balls with a diameter of 3 mm in a mass ratio of 1:(0.4-0.6), the rotation speed is adjusted to 250 rpm for ball milling for 6 hours, and after passing through an 80-mesh sieve, the mixture is placed in a muffle furnace and heated to 1000°C at a heating rate of 5°C / min, and the temperature is maintained for sintering for 8 hours to obtain a sintered powder; S2.2: 100 parts by mass of an aqueous solution of tris(hydroxymethyl)aminomethane with a concentration of 8 g / L is placed in a container, a hydrochloric acid solution is added to adjust the pH to 8, and then 0.3 parts by mass of polyacrylamide and 0.3 parts by mass of levodopa are added, and after stirring for 30 minutes, ultrasonic treatment is performed at an ultrasonic frequency of 20 kHz for 50 minutes to obtain a coating solution, and the sintered powder is immersed in the coating solution for 25 minutes, and the coated sintered powder is obtained after filtering and drying; S2.3: Immerse the coated sintered powder in a CaCl solution with a concentration of 55 g / L and a pH of 7.5. 2 The samples were immersed in the buffer for 20 minutes, rinsed with deionized water once, and then immersed in 35 g / L Na2O3 at a pH of 8.5. 2 HPO 4 The sample was placed in a buffer solution, allowed to stand for 20 minutes, then rinsed with deionized water once, and then immersed in sodium dodecyl sulfate, allowed to stand at room temperature for 1 hour, and air-dried to obtain HA grain-coated sintered powder.

[0025] S3: Composite and sintering of ceramic particles S3.1: Ta 2 O 5 and Sr(NO 3 ) 2 Mix them in a container at a molar ratio of 1:1.2, then add 20 times the mass of cyclohexane, seal and heat to 400°C for 1 hour, and filter to obtain SrTa 2 O 6 ; S3.2: Weigh HA grain-coated sintered powder and SrTa in a mass ratio of 1:0.03:0.03 2 O 6 and BaTi 4 O 9 , the weighed SrTa 2 O 6 and BaTi 4 O 9The mixture was placed in a ball mill, and 2 times the weight of anhydrous ethanol and 3 times the weight of zirconia balls with a diameter of 2 mm were added, and the mixture was ball-milled at a ball-milling speed of 250 rpm for 4 hours to obtain a dielectric performance enhancing material. The weighed HA grain-coated sintered powder and the dielectric performance enhancing material were placed in a mortar, and 3 wt % of a bending resistance sintering aid and 20 wt % of polyvinyl alcohol were added and ground until uniform spherical small particles were formed, and the particles were passed through a 95 mesh sieve to obtain ceramic particles. S3.3: Place the ceramic particles in a die, use a tablet press to apply a pressure of 8 MPa, hold for 30 seconds, and obtain a columnar ceramic green body with a height of 6 mm and a diameter of 10 mm. Place the columnar ceramic green body in a box-type resistance furnace and heat it to 500°C at a heating rate of 1°C / min, then place it in a muffle furnace and heat it to 780°C at a heating rate of 4°C / min, keep warm for 6 hours, and naturally cool in the furnace to obtain a high bending resistance and low dielectric constant ceramic material.

[0026] Embodiment 3: A high bending resistance ceramic material for 5G communication base station and a preparation method thereof, such as Figure 1 As shown, the following steps are included: S1: Calcination preparation of bending-resistant sintering aid S1.1: Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 The mixture was placed in a ball mill at a molar ratio of 1:1:1:0.2, and an equal amount of deionized water was added and mixed and ball milled for 4 hours. The ball mill speed was set to 300 rpm to obtain a mixed slurry. The mixed slurry was dried and then ground, and passed through a 120-mesh sieve to obtain a mixed fine powder. S1.2: The mixed fine powder is placed in a muffle furnace and calcined at 1300°C for 4.5 hours. After being taken out, it is quickly put into cold water for annealing. After grinding, it is passed through a 120-mesh sieve to obtain a bending-resistant sintering aid.

[0027] S2: Preparation of HA-coated ceramic sintered powder S2.1: Weigh B with a molar ratio of 1:2.4 2 O 3 and CaCO 3 The raw materials are mixed with anhydrous ethanol and zirconium oxide balls in a mass ratio of 1:1:2 and added into a ball mill, wherein the zirconium oxide balls are composed of zirconium oxide balls with a diameter of 6 mm and zirconium oxide balls with a diameter of 3 mm in a mass ratio of 1:(0.4-0.6), the rotation speed is adjusted to 300 rpm for ball milling for 8 hours, and after passing through a 100 mesh sieve, the mixture is placed in a muffle furnace and heated to 1100°C at a heating rate of 6°C / min, and the temperature is maintained for sintering for 10 hours to obtain a sintered powder; S2.2: 80 parts by mass of a 10 g / L tris(hydroxymethyl)aminomethane aqueous solution was placed in a container, a hydrochloric acid solution was added to adjust the pH to 8.5, and then 0.1 parts by mass of polyacrylamide and 0.2 parts by mass of levodopamin were added, and the mixture was stirred for 35 minutes and then ultrasonically treated at an ultrasonic frequency of 25 kHz for 60 minutes to obtain a coating solution, and the sintered powder was immersed in the coating solution for 30 minutes, and the coated sintered powder was obtained after filtering and drying; S2.3: Immerse the coated sintered powder in a CaCl solution with a concentration of 60 g / L and a pH of 8. 2 The samples were immersed in the buffer for 25 minutes, rinsed twice with deionized water, and then immersed in a 40 g / L, pH 9 Na 2 HPO 4 The sample was placed in a buffer solution, allowed to stand for 25 minutes, and then rinsed twice with deionized water. The sample was then immersed in sodium dodecyl sulfate, allowed to stand at room temperature for 1.5 hours, and air-dried to obtain HA grain-coated sintered powder.

[0028] S3: Composite and sintering of ceramic particles S3.1: Ta 2 O 5 and Sr(NO 3 ) 2 Mix them in a 1:1 molar ratio in a container, then add 15 times the mass of cyclohexane, seal and heat to 450°C for 1.5 hours, and filter to obtain SrTa 2 O 6 ; S3.2: Weigh HA grain-coated sintered powder and SrTa in a mass ratio of 1:0.02:0.02 2 O 6 and BaTi 4 O 9 , the weighed SrTa 2 O 6 and BaTi 4 O 9 The mixture was placed in a ball mill, 1.5 times the weight of anhydrous ethanol and 2.5 times the weight of zirconia balls with a diameter of 3 mm were added, and the mixture was ball-milled at a ball-milling speed of 300 rpm for 5 hours to obtain a dielectric performance enhancing material. The weighed HA grain-coated sintered powder and the dielectric performance enhancing material were placed in a mortar, and 2 wt % of a bending sintering aid and 18 wt % of polyvinyl alcohol were added and ground until uniform spherical small particles were formed, and the particles were passed through a 100 mesh sieve to obtain ceramic particles. S3.3: Place the ceramic particles in a die, use a tablet press to apply a pressure of 10 MPa, hold for 40 seconds, and obtain a columnar ceramic green body with a height of 8 mm and a diameter of 12 mm. Place the columnar ceramic green body in a box-type resistance furnace and heat it to 600°C at a heating rate of 1.5°C / min, then place it in a muffle furnace and heat it to 800°C at a heating rate of 5°C / min, keep warm for 8 hours, and naturally cool in the furnace to obtain a high bending resistance and low dielectric constant ceramic material.

[0029] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 removes step S2.2 and step S2.3, replaces the subsequent HA grain-coated sintered powder with sintered powder, and the remaining steps are the same as Example 1.

[0030] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that in step S3.2, SrTa 2 O 6 and BaTi 4 O 9 A dielectric performance enhancing material was prepared, and no dielectric performance enhancing material was added for blending and sintering. The remaining steps were the same as those in Example 1, and finally a ceramic material was obtained, which was recorded as Comparative Example 2.

[0031] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 removes step S1 and does not add anti-bending sintering aid in step S3.2. The remaining steps are the same as Example 1. Finally, a ceramic material is obtained, which is recorded as Comparative Example 3.

[0032] Experiment 1: Take the high bending resistance and low dielectric constant ceramic materials prepared in Examples 1-3, Comparative Example 1, Comparative Example 2 and Comparative Example 3, and take three portions respectively. The bending strength is tested by the method in the national standard "GBT6569-2006". The data are recorded and tabulated, as shown in Table 1. It can be seen that the bending strength of the high bending resistance and low dielectric constant ceramic materials prepared in Examples 1-3 is greater than that of Comparative Example 1 and Comparative Example 3. It can be proved that coating the sintered powder with HA crystal can improve the bending strength of the ceramic material after sintering. At the same time, it can be proved that Li 2 CO 3 、SiO 2 、Bi 2 O 3 and Al 2 O 3 The bending-resistant sintering aid is obtained by blending and calcining, and adding it into the subsequent sintering process can also improve the bending strength of the ceramic material; Table 1: Flexural strength of ceramic materials

[0033] Experiment 2: Take the high bending resistance and low dielectric constant ceramic materials prepared in Examples 1-3 and Comparative Example 2, take three portions respectively, use the open cavity resonant cavity method to test and calculate the dielectric constant, record the data and make a table, as shown in Table 2, and then use the closed cavity resonant cavity method to test and calculate the quality factor Q·f value, record the data and make a table, as shown in Table 3. Combining Table 1, Table 2 and Table 3, it can be seen that the dielectric constants of the high bending resistance and low dielectric constant ceramic materials prepared in Examples 1-3 are smaller than those in Comparative Example 2, while the quality factor Q·f values ​​are greater than those in Comparative Example 2, and the bending strength is slightly greater than that in Comparative Example 2, which can prove that the introduction of SrTa in the ceramic sintering process 2 O 6 and BaTi 4 O 9 The prepared dielectric performance enhancing material can improve the dielectric performance of the ceramic material without reducing its flexural strength.

[0034] Table 2: Dielectric constants of ceramic materials

[0035] Table 3: Quality factor Q·f value of ceramic materials

[0036] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a high bending resistance ceramic material for a 5G communication base station, characterized in that: The following steps are involved: S1: Calcination preparation of bending-resistant sintering aid Li2CO3, SiO2, Bi2O3 and Al2O3 are mixed and ball-milled to obtain a mixed slurry, which is then dried and ground and then sieved to obtain a mixed fine powder, which is then calcined in a muffle furnace and then rapidly annealed, and then ground and sieved to obtain a bending-resistant sintering aid; S2: Preparation of HA-coated ceramic sintered powder B2O3, CaCO3, anhydrous ethanol and zirconium oxide balls are placed in a ball mill for ball milling, and then sintered at high temperature after being sieved to obtain a sintered powder; a tris(hydroxymethyl)aminomethane aqueous solution is placed in a container, polyacrylamide and L-dopamine are added after adjusting the pH, and ultrasonic treatment is performed after stirring to obtain a coating solution; the sintered powder is immersed in the coating solution, filtered and dried to obtain a coated sintered powder; the coated sintered powder is then immersed in a CaCl2 buffer solution, washed and immersed in a Na2HPO4 buffer solution, washed again and immersed in sodium dodecyl sulfate, taken out and air-dried to obtain a HA grain-coated sintered powder; S3: Composite and sintering of ceramic particles Ta2O5 and Sr(NO3)2 are placed in a container, cyclohexane is added, and the container is sealed and heated before filtering to obtain SrTa2O6. HA grain-coated sintered powder, SrTa2O6 and BaTi4O9 are weighed, SrTa2O6 and BaTi4O9 are first mixed and ball-milled to obtain a dielectric performance enhancing material, the weighed HA grain-coated sintered powder and the dielectric performance enhancing material are placed in a mortar, and then a bending resistance sintering aid and polyvinyl alcohol are added for grinding, and ceramic particles are obtained after sieving, and the ceramic particles are pressed into a column and first sintered at a low temperature and then sintered at a high temperature, and then cooled to obtain a high bending resistance and low dielectric constant ceramic material.

2. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 1, characterized in that: Step S1: calcination preparation of bending-resistant sintering aid, comprising the following steps: S1.1: Li2CO3, SiO2, Bi2O3 and Al2O3 are placed in a ball mill, and deionized water of equal mass is added and mixed and ball milled for 3-4 hours. The ball mill speed is set to 250-300rpm to obtain a mixed slurry. The mixed slurry is dried and then ground, and passed through a 100-120 mesh sieve to obtain a mixed fine powder; S1.2: The mixed fine powder is placed in a muffle furnace and calcined at a temperature of 1200-1300°C for 4-4.5 hours. After being taken out, it is quickly put into cold water for annealing. After grinding, it is passed through a 100-120 mesh sieve to obtain a bending-resistant sintering aid.

3. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 2, characterized in that: Step S2 prepares HA-coated ceramic sintered powder, comprising the following steps: S2.1: Weigh B2O3 and CaCO3 raw materials with a molar ratio of 1: (2.4-2.6), mix them with anhydrous ethanol and zirconium oxide balls in a mass ratio of 1: (1-1.5): (2-2.5), add them into a ball mill, adjust the speed to 250-300rpm, ball mill for 6-8 hours, pass through an 80-100 mesh sieve, place in a muffle furnace and heat to 1000-1100℃ at a heating rate of 5-6℃ / min, maintain the temperature and sinter for 8-10 hours to obtain sintered powder; S2.2: 80-100 parts by weight of an aqueous solution of tris(hydroxymethyl)aminomethane with a concentration of 8-10 g / L is placed in a container, the pH is adjusted to 8-8.5, and then 0.1-0.3 parts by weight of polyacrylamide and 0.2-0.3 parts by weight of levodopa are added, and after stirring for 30-35 minutes, ultrasonic treatment is performed at an ultrasonic frequency of 20-25 kHz for 50-60 minutes to obtain a coating solution, and the sintered powder is immersed in the coating solution for 25-30 minutes, and filtered and dried to obtain a coated sintered powder; S2.3: Immerse the coated sintered powder in CaCl2 buffer for 20-25 minutes, rinse with deionized water 1-2 times, immerse in Na2HPO4 buffer, let stand for 20-25 minutes, rinse with deionized water 1-2 times, then immerse in sodium dodecyl sulfate, let stand at room temperature for 1-1.5 hours, and air-dry to obtain HA grain-coated sintered powder.

4. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 3, characterized in that: Step S3, the composite and column pressing sintering of ceramic particles, comprises the following steps: S3.1: Mix Ta2O5 and Sr(NO3)2 in a molar ratio of 1:(1-1.2) in a container, then add 15-20 times the mass of cyclohexane, seal and heat to 400-450℃ for 1-1.5 hours, and filter to obtain SrTa2O6; S3.2: Weigh HA grain-coated sintered powder, SrTa2O6 and BaTi4O9 in a mass ratio of 1: (0.02-0.03): (0.02-0.03), place the weighed SrTa2O6 and BaTi4O9 in a ball mill, add 1.5-2 times the mass of anhydrous ethanol and 2.5-3 times the mass of zirconia balls with a diameter of 2-3 mm, and ball mill at a ball milling speed of 250-300rpm for 4-5 hours to obtain a dielectric performance enhancing material, place the weighed HA grain-coated sintered powder and the dielectric performance enhancing material in a mortar, add 2-3wt% of an anti-bending sintering aid and 18-20wt% of polyvinyl alcohol, grind until uniform spherical small particles are formed, and pass through a 95-100 mesh sieve to obtain ceramic particles; S3.3: Place the ceramic particles in a die, use a tablet press to apply a pressure of 8-10MPa, maintain for 30-40 seconds to obtain a columnar ceramic green body, place the columnar ceramic green body in a box-type resistance furnace and heat it to 500-600℃ at a heating rate of 1-1.5℃ / min, then place it in a muffle furnace and heat it to 780-800℃ at a heating rate of 4-5℃ / min, keep it warm for 6-8 hours, and naturally cool it in the furnace to obtain a high bending resistance and low dielectric constant ceramic material.

5. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 2, characterized in that: The molar ratio of Li2CO3, SiO2, Bi2O3 and Al2O3 in step S1.1 is 1:1:1:(0.2-0.3).

6. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 3, characterized in that: The zirconia balls in step 2.1 are composed of zirconia balls with a diameter of 6 mm and zirconia balls with a diameter of 3 mm in a mass ratio of 1:(0.4-0.6).

7. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 3, characterized in that: The method for adjusting the pH in step S2.2 is to add a hydrochloric acid solution.

8. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 3, characterized in that: In step S2.3, the concentration of the CaCl2 buffer is 55-60 g / L, the pH is 7.5-8, and the concentration of the Na2HPO4 buffer is 35-40 g / L, the pH is 8.5-9.

9. The method for preparing a high bending resistance ceramic material for a 5G communication base station according to claim 4, characterized in that: The columnar ceramic green body in step S3.3 has a height of 6-8 mm and a diameter of 10-12 mm.

10. A high bending resistance ceramic material for a 5G communication base station, characterized in that: The material is prepared by the method for preparing a high bending-resistant ceramic material for a 5G communication base station as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Temperature-stable type ultralow-dielectric-constant microwave dielectric ceramic Ca5LaB3O11

    CN104446374A

  • Microwave dielectric ceramic with medium dielectric constant and low loss

    CN104774008A

  • CBS-class LTCC (low temperature co-fired ceramic) material and preparation method thereof

    CN106187141A

  • Reinforced calcium borosilicate microcrystalline glass composite material and preparation method thereof

    CN110683769A

  • Preparation method of thermal sensitive ceramic material with high stability and negative temperature coefficient

    CN114773034A

Cited By

  • Lightweight domestic ceramic material and preparation method thereof

    CN120554088A

  • Lightweight domestic ceramic material and method for its production

    CN120554088B