High-elasticity damping rubber batten and preparation method thereof
Through the compounding of nitrile rubber and epoxy resin and the use of modified silica filler, the problem of elasticity reduction and aging resistance of rubber slats under extreme conditions is solved, and the service life and performance of the bearing are improved.
Patent Information
- Application Number
- CN202411063487.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-01
AI Technical Summary
The elasticity of existing rubber slats decreases under extreme temperature, light and humidity conditions, resulting in poor sealing performance and shock absorption effect, and insufficient aging resistance, affecting the service life and maintenance frequency of the bearings.
Nitrile rubber is compounded with bisphenol F, bisphenol A and alicyclic epoxy resin to form a complex network structure. Combined with modified silica filler, it improves the elastic recovery, cold resistance and water absorption of the rubber material. , increase mechanical properties and weather resistance.
It improves the vibration damping performance of the rubber slats under low temperature conditions, extends the service life of the bearings, reduces the frequency of maintenance and replacement, and improves the mechanical properties and weather resistance of the material.
Smart Images

Figure BDA0004978684980000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber strips, and in particular relates to a high-elasticity vibration-damping rubber strip and a preparation method thereof. Background Art
[0002] The rubber strips used in water-lubricated bearings are one of the key components. They are usually used to create a water film to reduce the direct contact between two relatively moving surfaces, thereby reducing friction and wear. The design and performance of the rubber strips directly affect the lubrication efficiency, load-bearing capacity and service life of the bearing. The main technical problems of rubber strips in the prior art are as follows: (1) Material selection: The rubber strips need to be made of suitable elastomeric materials, which must be able to withstand chemical corrosion in the working environment, such as the salinity of seawater, changes in pH, and temperature fluctuations. (2) The elasticity and durability of the material are also crucial to ensure stable performance during long-term operation. (3) Water film formation: The surface treatment of the rubber strips affects the formation of the water film. The surface finish helps to optimize the stability of the water film, which in turn affects the lubrication effect and the friction coefficient. (4) Wear and fatigue: During long-term operation, the rubber strips may become thinner due to wear, resulting in a decrease in the thickness of the water film, affecting the lubrication effect. The strips may also be damaged by fatigue, especially under high load and vibration conditions.
[0003] Therefore, developing a rubber strip with excellent comprehensive performance meets the market demand and has extremely high market value. Summary of the invention
[0004] The invention provides a high-elasticity vibration-damping rubber strip and a preparation method thereof.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a high-elastic vibration-damping rubber strip, the method comprising the following steps:
[0007] (1) Weighing the raw materials by weight: 70-75 parts of nitrile rubber, 13-18 parts of composite epoxy resin, 10-15 parts of modified filler, 12-18 parts of plasticizer A, 1-3 parts of antioxidant, 0.4-0.9 parts of insoluble sulfur, 2-4 parts of vulcanization accelerator, 4-7 parts of epoxy active toughening agent, 3-6 parts of dispersant and 4-9 parts of plasticizer B; wherein the composite epoxy resin is obtained by compounding bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin in a weight ratio of 1:1.2-1.6:0.4-0.8;
[0008] (2) placing the nitrile rubber in a kneading machine and kneading it at 125-130° C. for 6-9 minutes; mixing the kneaded nitrile rubber with the modified filler, plasticizer A, antioxidant, dispersant and plasticizer B, heating the mixture to 120-130° C. and stirring for 5-10 minutes to obtain a nitrile rubber mixture;
[0009] (3) adding the composite epoxy resin and the epoxy active toughening agent to the nitrile rubber mixture, stirring at 70-80° C. for 20-25 min, and then placing in an open mill for kneading, while adding insoluble sulfur and a vulcanization accelerator, stirring at 40-50° C. for 5-10 min, to obtain a rubber material;
[0010] (4) The rubber material is made into a high-elastic vibration-damping layer, and the high-elastic vibration-damping layer and the polymer hard plate are bonded to form a rubber strip.
[0011] Furthermore, the epoxy equivalent of the bisphenol F epoxy resin is 165-175 g / eq.
[0012] Furthermore, the epoxy value of the bisphenol A epoxy resin is 0.39±0.02 mol / 100g.
[0013] Furthermore, the epoxy equivalent of the alicyclic epoxy resin is 170-200 g / eq.
[0014] Furthermore, the material of the polymer hard plate is ultra-high molecular weight polyethylene.
[0015] Furthermore, the molecular weight of ultra high molecular weight polyethylene is 3 million.
[0016] Furthermore, the plasticizer A is a polyester plasticizer A.
[0017] Furthermore, plasticizer A is plasticizer ARS-107.
[0018] Furthermore, the plasticizer B is one or more of dibutyl dioctyl phthalate and dibutyl sebacate.
[0019] Furthermore, the antioxidant is NBC. CAS: 13927-77-0.
[0020] Furthermore, the vulcanization accelerator is TMTD. CAS: 137-26-8.
[0021] Furthermore, the dispersant is sodium dimethylbenzenesulfonate.
[0022] The stern shaft in the ship propulsion system is a key component connecting the engine output end and the propeller. During the navigation of the ship, the stern shaft will be subjected to various dynamic loads, including vibration caused by waves, impact of water flow, unbalanced force of the propeller, and vibration of the engine. The elasticity of the rubber strip can absorb and buffer these impacts, reducing direct damage to the shaft and bearings. Nitrile rubber is used as a material for rubber strips, but nitrile rubber, as a rubber strip material, is used as a stern shaft in the ship propulsion system, and has the problem of poor low temperature resistance. Nitrile rubber hardens and its elasticity decreases under low temperature conditions, affecting its sealing performance and shock absorption effect under cold conditions. At the same time, as time goes by, NBR will harden, lose elasticity or crack, especially under extreme temperature, light and humidity conditions. The present invention improves the vibration reduction performance of nitrile rubber at low temperatures by compounding nitrile rubber with bisphenol F type epoxy resin, bisphenol A type epoxy resin and alicyclic epoxy resin, reduces the relative movement and wear between the internal components of the bearing, helps to extend the service life of the bearing, and reduces the frequency of maintenance and replacement. The analysis shows that epoxy resin, as a rigid component, can form a more complex network structure when combined with nitrile rubber, thereby improving the elastic recovery and cold resistance of the composite material. Bisphenol A and bisphenol F epoxy resins have high crosslinking density and excellent mechanical strength. Alicyclic epoxy resins have higher glass transition temperatures and can still maintain good mechanical properties at higher temperatures. When nitrile rubber is mixed with compounded epoxy resins, an interpenetrating network structure can be formed through appropriate crosslinking and curing processes. This structure can effectively disperse stress, reduce the brittleness of the material, and improve its toughness. At the same time, when using parameters of bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin, the aging resistance of nitrile rubber can be improved.
[0023] Furthermore, the preparation method of the modified filler is: by weight,
[0024] (1) adding 1 part of silicon dioxide to 60-70 parts of 35-40 wt% aqueous hydrogen peroxide solution, reflux reacting at 100° C. for 2-2.5 hours, filtering and drying to obtain modified silicon dioxide A;
[0025] (2) 1 part of modified silica A, 1 part of water, 6-9 parts of ethanol, 90-100 parts of 25-28 wt% ammonia water and 1.5-2.5 parts of KH590 were mixed, reacted at 40-45° C. for 4-6 hours, filtered and dried to obtain modified silica B;
[0026] (3) 2-3 parts of modified silica B, 1 part of dimethyldiallylammonium chloride, 0.04-0.08 parts of azobisisobutyronitrile and 70-80 parts of 90-95 wt% ethanol aqueous solution are mixed, reacted at 80-90° C. for 12-15 hours under nitrogen protection, filtered, washed and dried to obtain a modified filler.
[0027] Furthermore, the silicon dioxide is composed of a mixture of silicon dioxide I, silicon dioxide II and silicon dioxide III in a mass ratio of 1:1.4-1.9:0.3-0.8, and the average particle size of silicon dioxide I is less than the average particle size of silicon dioxide II and less than the average particle size of silicon dioxide III.
[0028] Specifically, the average particle size of silicon dioxide I is 10 nm and the average specific surface area is 380 m 2 / g; the average particle size of silicon dioxide II is 50nm and the average specific surface area is 210m 2 / g; the average particle size of silicon dioxide III is 300nm and the average specific surface area is 17m 2 / g.
[0029] The inventors found that the molecular structure and chemical properties of epoxy resins affect the water absorption of nitrile rubber. Analysis shows that bisphenol F and bisphenol A epoxy resins contain phenolic hydroxyl groups, which can form hydrogen bonds with water molecules to increase water absorption. The inventors tried to add silica to improve the water absorption of rubber materials, but silica has poor dispersibility in the system of the present invention, resulting in unsatisfactory results. The present invention can effectively improve the water absorption of rubber materials by modifying silica. Analysis shows that the chemical compatibility between silica and the polymer matrix is improved by modification with thiol and KH590. The presence of quaternary ammonium groups can enhance the dispersibility of silica in polar polymer matrices (such as epoxy resins). At the same time, due to its low hydrophilicity, it helps to reduce the interaction between the composite material and water; a stronger interface bond is formed between the modified silica and the polymer matrix, reducing the path of water penetration, and the silica particles are more evenly distributed in the matrix, reducing micropores and defects, and reducing the channel for water penetration. At the same time, the addition of modified fillers prepared using silica of different particle sizes can improve the mechanical properties and weather resistance of rubber materials.
[0030] The invention also provides a high-elasticity vibration-damping rubber strip prepared by the preparation method.
[0031] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0032] 1. The rubber strips of the present invention are all composed of a high-elastic vibration-damping layer and a high-molecular hard plate bonded together. The rubber bearings produced can be used for the stern shaft of a ship propulsion system or other purposes to achieve vibration reduction, noise reduction and lubrication.
[0033] 2. The present invention improves the vibration reduction performance of the nitrile rubber at low temperature by compounding the nitrile rubber with bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin, reduces the relative movement and wear between the internal components of the bearing, helps to extend the service life of the bearing, and reduces the frequency of maintenance and replacement. At the same time, when the parameters of bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin are used, the aging resistance of the nitrile rubber can be improved.
[0034] 3. The present invention can effectively improve the water absorption rate of the rubber material by modifying the silicon dioxide; at the same time, the addition of the modified filler can improve the mechanical properties and weather resistance of the rubber material. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] This embodiment provides a high-elasticity vibration-damping rubber strip, and the preparation method thereof comprises the following steps:
[0038] (1) Weighing the raw materials by weight: 72 parts of nitrile rubber, 15 parts of composite epoxy resin, 12 parts of modified filler, 16 parts of plasticizer A, 2 parts of antioxidant, 0.7 parts of insoluble sulfur, 3 parts of vulcanization accelerator, 5 parts of epoxy active toughening agent, 4 parts of dispersant and 7 parts of plasticizer B; wherein the composite epoxy resin is obtained by compounding bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin in a weight ratio of 1:1.4:0.6;
[0039] (2) placing the nitrile rubber in a kneading machine and kneading it at 128° C. for 8 minutes; mixing the kneaded nitrile rubber with the modified filler, plasticizer A, antioxidant, dispersant and plasticizer B, heating the mixture to 125° C. and stirring the mixture for 7 minutes to obtain a nitrile rubber mixture;
[0040] (3) adding the composite epoxy resin and the epoxy active toughening agent to the nitrile rubber mixture, stirring at 75° C. for 22 minutes, and then placing in an open mill for kneading, while adding insoluble sulfur and a vulcanization accelerator, stirring at 45° C. for 7 minutes, to obtain a rubber material;
[0041] (4) The rubber material is made into a high-elastic vibration-damping layer, and the high-elastic vibration-damping layer and the polymer hard plate are bonded to form a rubber strip.
[0042] The epoxy equivalent of the bisphenol F epoxy resin is 165-175 g / eq.
[0043] The epoxy value of the bisphenol A epoxy resin is 0.39±0.02 mol / 100g.
[0044] The epoxy equivalent of the alicyclic epoxy resin is 170-200 g / eq.
[0045] The epoxy reactive toughening agent was purchased from Shanghai Sanzuding New Materials Co., Ltd., model 2788A.
[0046] The material of the polymer hard plate is ultra-high molecular weight polyethylene, and the molecular weight of the ultra-high molecular weight polyethylene is 3 million.
[0047] The plasticizer A is plasticizer ARS-107.
[0048] The plasticizer B is dioctyl phthalate.
[0049] The antioxidant is NBC. CAS: 13927-77-0.
[0050] The vulcanization accelerator is TMTD. CAS: 137-26-8.
[0051] The dispersant is sodium dimethylbenzenesulfonate.
[0052] The preparation method of the modified filler is as follows: by weight,
[0053] (1) adding 1 part of silicon dioxide to 65 parts of a 37 wt % aqueous solution of hydrogen peroxide, reflux reacting at 100° C. for 2.2 h, filtering and drying to obtain modified silicon dioxide A;
[0054] (2) 1 part of modified silica A, 1 part of water, 7 parts of ethanol, 93 parts of 27 wt% ammonia water and 2 parts of KH590 were mixed, reacted at 42° C. for 5 h, filtered and dried to obtain modified silica B;
[0055] (3) 2.5 parts of modified silica B, 1 part of dimethyldiallylammonium chloride, 0.06 parts of azobisisobutyronitrile and 75 parts of 92 wt % ethanol aqueous solution were mixed, reacted at 85° C. for 14 h under nitrogen protection, filtered, washed and dried to obtain a modified filler.
[0056] The silicon dioxide is composed of a mixture of silicon dioxide I, silicon dioxide II and silicon dioxide III in a mass ratio of 1:1.6:0.5; wherein the average particle size of silicon dioxide I is 10nm and the average specific surface area is 380m 2 / g; the average particle size of silicon dioxide II is 50nm and the average specific surface area is 210m 2 / g; the average particle size of silicon dioxide III is 300nm and the average specific surface area is 17m 2 / g.
[0057] Example 2
[0058] This embodiment provides a high-elasticity vibration-damping rubber strip, and the preparation method thereof comprises the following steps:
[0059] (1) Weighing the raw materials by weight: 70 parts of nitrile rubber, 18 parts of composite epoxy resin, 10 parts of modified filler, 18 parts of plasticizer A, 1 part of antioxidant, 0.9 parts of insoluble sulfur, 2 parts of vulcanization accelerator, 7 parts of epoxy active toughening agent, 3 parts of dispersant and 9 parts of plasticizer B; wherein the composite epoxy resin is obtained by compounding bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin in a weight ratio of 1:1.2:0.8;
[0060] (2) placing the nitrile rubber in a kneading machine and kneading it at 125° C. for 9 minutes; mixing the kneaded nitrile rubber with the modified filler, plasticizer A, antioxidant, dispersant and plasticizer B, heating the mixture to 120° C. and stirring the mixture for 10 minutes to obtain a nitrile rubber mixture;
[0061] (3) adding the composite epoxy resin and the epoxy active toughening agent to the nitrile rubber mixture, stirring at 70° C. for 25 minutes, and then placing in an open mill for kneading, while adding insoluble sulfur and a vulcanization accelerator, stirring at 40° C. for 10 minutes, to obtain a rubber material;
[0062] (4) The rubber material is made into a high-elastic vibration-damping layer, and the high-elastic vibration-damping layer and the polymer hard plate are bonded to form a rubber strip.
[0063] The epoxy equivalent of bisphenol F epoxy resin is 165-175 g / eq.
[0064] The epoxy value of the bisphenol A epoxy resin is 0.39±0.02 mol / 100g.
[0065] The epoxy equivalent of the alicyclic epoxy resin is 170-200 g / eq.
[0066] The epoxy reactive toughening agent was purchased from Shanghai Sanzuding New Materials Co., Ltd., model 2788A.
[0067] The material of the polymer hard plate is ultra-high molecular weight polyethylene, and the molecular weight of the ultra-high molecular weight polyethylene is 3 million.
[0068] The plasticizer A is plasticizer ARS-107.
[0069] The plasticizer B is dioctyl phthalate.
[0070] The antioxidant is NBC. CAS: 13927-77-0.
[0071] The vulcanization accelerator is TMTD. CAS: 137-26-8.
[0072] The dispersant is sodium dimethylbenzenesulfonate.
[0073] The preparation method of the modified filler is as follows: by weight,
[0074] (1) adding 1 part of silicon dioxide to 60 parts of a 40 wt % aqueous solution of hydrogen peroxide, reflux reacting at 100° C. for 2 h, filtering and drying to obtain modified silicon dioxide A;
[0075] (2) 1 part of modified silica A, 1 part of water, 9 parts of ethanol, 90 parts of 28 wt% ammonia water and 1.5 parts of KH590 were mixed, reacted at 45° C. for 4 h, filtered and dried to obtain modified silica B;
[0076] (3) 3 parts of modified silica B, 1 part of dimethyldiallylammonium chloride, 0.04 parts of azobisisobutyronitrile and 80 parts of 90 wt % ethanol aqueous solution were mixed, reacted at 90° C. for 12 h under nitrogen protection, filtered, washed and dried to obtain a modified filler.
[0077] The silicon dioxide is composed of a mixture of silicon dioxide I, silicon dioxide II and silicon dioxide III in a mass ratio of 1:1.6:0.5; wherein the average particle size of silicon dioxide I is 10nm and the average specific surface area is 380m 2 / g; the average particle size of silicon dioxide II is 50nm and the average specific surface area is 210m 2 / g; the average particle size of silicon dioxide III is 300nm and the average specific surface area is 17m 2 / g.
[0078] Comparative Example 1
[0079] The difference between this comparative example and Example 1 is that the composite epoxy resin is a compound of bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin in a weight ratio of 1:1:1.
[0080] Comparative Example 2
[0081] The difference between this comparative example and Example 1 is that the bisphenol A epoxy resin is replaced by a glycidyl ether epoxy resin, the epoxy equivalent is 120-150 g / eq, and the viscosity at 25° C. is 7000-10000 cps.
[0082] Comparative Example 3
[0083] The difference between this comparative example and Example 1 is that the epoxy value of the bisphenol F epoxy resin is 165-180 g / mol.
[0084] The epoxy equivalent of bisphenol A epoxy resin is 180-190 g / eq.
[0085] The epoxy equivalent of the alicyclic epoxy resin is 130.0-135.0 g / eq.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 1 is that the preparation method of the modified filler is as follows: by weight, 1 part of silicon dioxide, 1 part of water, 8 parts of ethanol and 2 parts of KH590 are mixed, reacted at 45° C. for 5 hours, filtered and dried to obtain the modified filler.
[0088] Comparative Example 5
[0089] The difference between this comparative example and Example 1 is that the preparation method of the modified filler is: by weight,
[0090] (1) adding 1 part of calcium carbonate to 65 parts of 37 wt % aqueous hydrogen peroxide solution, reflux reacting at 100° C. for 2.2 h, filtering and drying to obtain modified calcium carbonate A;
[0091] (2) 1 part of surface hydroxylated calcium carbonate, 1 part of water, 7 parts of ethanol, 93 parts of 26 wt% ammonia water and 2 parts of KH590 were mixed, reacted at 42° C. for 5 h, filtered and dried to obtain modified calcium carbonate B;
[0092] (3) 2.5 parts of modified calcium carbonate B, 1 part of dimethyldiallylammonium chloride, 0.06 parts of azobisisobutyronitrile and 75 parts of 92 wt % ethanol aqueous solution were mixed, reacted at 85° C. for 14 h under nitrogen protection, filtered, washed and dried to obtain a modified filler.
[0093] The particle size of calcium carbonate is 2000-2500 mesh.
[0094] Comparative Example 6
[0095] The difference between this comparative example and Example 1 is that the silicon dioxide is a mixture of silicon dioxide I, silicon dioxide II and silicon dioxide III in a mass ratio of 1:1:1, and the average particle size of silicon dioxide I is 10nm and the average specific surface area is 380m 2 / g; the average particle size of silicon dioxide II is 50nm and the average specific surface area is 210m 2 / g; the average particle size of silicon dioxide III is 300nm and the average specific surface area is 17m 2 / g.
[0096] Comparative Example 7
[0097] The difference between this comparative example and Example 1 is that the silicon dioxide has an average particle size of 20 nm and an average specific surface area of 240 m 2 / g of silicon dioxide, average particle size 500nm, average specific surface area 15m 2 / g of silica and an average particle size of 1μm and an average specific surface area of 7m 2 / g of silica compound.
[0098] Performance Testing
[0099] The rubber materials prepared in Examples 1-2 and Comparative Examples 1-7 were subjected to performance tests.
[0100] 1. Determine the compression set according to GB / T7759.1-2015.
[0101] 2. Determine the volume change rate of distilled water according to GB / T1690-2010.
[0102] 3. The tensile strength and elongation at break were tested using the method disclosed in GB528-2009.
[0103] 4. Low temperature performance test: GB / T1682-1994 is used to test the brittle temperature and whether it breaks at -40℃.
[0104] 5. Weather resistance test
[0105] (1) Heat aging: Place at 100°C for 70 hours, and then test the change rate of tensile strength using the method disclosed in GB3512-2014.
[0106] (2) Resistance to fuel aging: Place the product in 40°C fuel for 40 hours, and then test the volume change rate using the method disclosed in GB1690-2010.
[0107] (3) Ozone aging resistance: At 40°C and 50 pphm of ozone, perform 20% stretching according to GB / T7762-2014 and record whether cracking occurs.
[0108] Table 1 Performance test results
[0109]
[0110] The results show that the rubber materials prepared in Examples 1-2 have excellent comprehensive properties. Comparative Examples 1-7 show that the comprehensive properties decrease to varying degrees when the preparation conditions are changed.
[0111] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a high elastic vibration damping rubber strip, characterized in that: The following steps are involved: (1) Weighing the raw materials by weight: 70-75 parts of nitrile rubber, 13-18 parts of composite epoxy resin, 10-15 parts of modified filler, 12-18 parts of plasticizer A, 1-3 parts of antioxidant, 0.4-0.9 parts of insoluble sulfur, 2-4 parts of vulcanization accelerator, 4-7 parts of epoxy active toughening agent, 3-6 parts of dispersant and 4-9 parts of plasticizer B; wherein the composite epoxy resin is obtained by compounding bisphenol F epoxy resin, bisphenol A epoxy resin and alicyclic epoxy resin in a weight ratio of 1:1.2-1.6:0.4-0.8; (2) placing the nitrile rubber in a kneading machine and kneading it at 125-130° C. for 6-9 minutes; mixing the kneaded nitrile rubber with the modified filler, plasticizer A, antioxidant, dispersant and plasticizer B, heating the mixture to 120-130° C. and stirring for 5-10 minutes to obtain a nitrile rubber mixture; (3) adding the composite epoxy resin and the epoxy active toughening agent to the nitrile rubber mixture, stirring at 70-80° C. for 20-25 min, and then placing in an open mill for kneading, while adding insoluble sulfur and a vulcanization accelerator, stirring at 40-50° C. for 5-10 min, to obtain a rubber material; (4) The rubber material is made into a high-elastic vibration-damping layer, and the high-elastic vibration-damping layer and the polymer hard plate are bonded to form a rubber strip.
2. The method for preparing the high elastic vibration damping rubber strip according to claim 1, characterized in that: The plasticizer B is one or more of dibutyl dioctyl phthalate and dibutyl sebacate.
3. The method for preparing the high elastic vibration damping rubber strip according to claim 1, characterized in that: The dispersant is sodium dimethylbenzenesulfonate.
4. The method for preparing the high elastic vibration damping rubber strip according to claim 1, characterized in that: The epoxy equivalent of bisphenol F epoxy resin is 165-175 g / eq.
5. The method for preparing the high elastic vibration damping rubber strip according to claim 1, characterized in that: The epoxy value of the bisphenol A epoxy resin is 0.39±0.02 mol / 100g.
6. The method for preparing the high elastic vibration damping rubber strip according to claim 1, characterized in that: The epoxy equivalent of the alicyclic epoxy resin is 170-200 g / eq.
7. The method for preparing the high elastic vibration damping rubber strip according to claim 1, characterized in that: The preparation method of the modified filler comprises the following steps: (1) adding 1 part by weight of silicon dioxide to 60-70 parts by weight of a 35-40 wt% hydrogen peroxide aqueous solution, reflux reacting at 100° C. for 2-2.5 hours, filtering and drying to obtain modified silicon dioxide A; (2) 1 part by weight of modified silica A, 1 part by weight of water, 6-9 parts by weight of ethanol, 90-100 parts by weight of 25-28 wt% ammonia water and 1.5-2.5 parts by weight of KH590 were mixed, reacted at 40-45° C. for 4-6 hours, filtered and dried to obtain modified silica B; (3) 2-3 parts by weight of modified silica B, 1 part by weight of dimethyldiallylammonium chloride, 0.04-0.08 parts by weight of azobisisobutyronitrile and 70-80 parts by weight of 90-95 wt% ethanol aqueous solution are mixed, reacted at 80-90° C. for 12-15 hours under nitrogen protection, filtered, washed and dried to obtain a modified filler.
8. The method for preparing the high elastic vibration damping rubber strip according to claim 7, characterized in that: The silicon dioxide is composed of a mixture of silicon dioxide I, silicon dioxide II and silicon dioxide III in a mass ratio of 1:1.4-1.9:0.3-0.8, and the average particle size of silicon dioxide I is less than the average particle size of silicon dioxide II and less than the average particle size of silicon dioxide III.
9. A high elastic vibration-damping rubber strip prepared according to the preparation method of claims 1-8.