By using a combination of hydrogenated nitrile rubber and polyvinyl chloride and modified nano-magnesium oxide and carbon black fillers in a petrochemical mining environment, the problem of short service life of existing rubber in high-temperature and high-pressure environments has been solved, and high-temperature and oil-resistant properties have been achieved. improvement and cost reduction.

CN118725434APending Publication Date: 2024-10-01CNPC BOHAI EQUIP MFG +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310312087.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing nitrile rubber has a short service life in petrochemical mining environments and cannot effectively cope with high temperature, high pressure and highly corrosive conditions, resulting in increased costs and reduced efficiency. The high cost of fluorine rubber limits its application scope.

Method used

It uses a combination of polymer main material, hydrogenated nitrile rubber and polyvinyl chloride. By adjusting the weight ratio and adding vulcanizing agents, reinforcing agents and antioxidants, it forms a high-temperature and oil-resistant rubber, improving its impact resistance and tensile strength. And through modified nano-magnesia and carbon black reinforced fillers, the mechanical properties and compatibility are improved.

Benefits of technology

It extends the service life of the stator lining rubber, improves high temperature resistance and oil resistance, reduces vulcanization temperature and energy consumption, and ensures stability and efficiency in complex mining environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004148857040000131
    Figure BDA0004148857040000131
  • Figure BDA0004148857040000141
    Figure BDA0004148857040000141
Patent Text Reader

Abstract

The high-temperature-resistant and oil-resistant rubber is prepared from the following components in parts by weight: 100 parts of a macromolecular main body material, 1 to 5 parts of a vulcanizing agent, 50 to 90 parts of a reinforcing agent, 1 to 10 parts of a plasticizer, 1 to 5 parts of an anti-aging agent and 1 to 3 parts of stearic acid, the hydrogenated butadiene-acrylonitrile rubber with the acrylonitrile mass fraction of 40-45%, the Mooney viscosity of 63 and the residual double bond mass fraction of less than 0.9% is adopted as a main body material, and the prepared lining rubber has a higher melting point, can bear higher temperature in the use process of the screw pump, and has the effects of high temperature resistance and oil resistance; by adopting the synergistic effect of the hydrogenated nitrile rubber and the polyvinyl chloride, the lining rubber can achieve good impact resistance and tensile strength and adapt to a complex mining environment; the nano magnesium oxide and the carbon black are introduced as reinforcing agents, so that the stator lining rubber can reach proper hardness, is not easy to embrittle in a low-temperature environment, and has good low-temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer compounds, and in particular relates to high temperature and oil resistant rubber, a preparation method and application thereof. Background Art

[0002] In the oilfield industry, nitrile rubber is often used as the lining rubber on the stator of the mining screw pump. It is widely used due to its high temperature and oil resistance. However, with the reduction of oil resources, the gap in petrochemical resources is getting bigger and bigger. It is necessary to continuously update the mining technology to cope with the increasingly severe mining environment. The high temperature, high pressure and strong corrosive conditions faced by the mining environment of the petrochemical industry shorten the service life of nitrile rubber. It needs to be replaced after 3-6 months of use, which affects the mining efficiency and increases the cost. Now fluororubber is gradually replacing nitrile rubber, but the high cost of fluororubber limits its application range.

[0003] Chinese invention patent CN201410226491.1 discloses a high-performance screw pump stator rubber composition, which uses nitrile rubber and polyurethane as the main materials, uses a combination of an organic peroxide vulcanization system and a sulfur vulcanization system as the vulcanization system, uses hard carbon black as a reinforcing filler, and uses RD / MB as an anti-aging system. The composition has good oil resistance, fatigue resistance and adhesion properties in a diesel environment, but can only adapt to an environment of 70°C, and has poor application performance in a high-temperature environment; Chinese invention patent CN201410491348.5 discloses a low-Mooney high-oil-resistant rubber, a preparation method, and its application in a screw pump stator, which uses hydrogenated nitrile rubber as the main material, adds stearic acid and zinc oxide for modification, so that it has excellent Mooney viscosity and good processing performance, and can better meet the requirements of actual production, but its high-temperature resistance and mechanical properties have a certain degree of decline, affecting the service life of the rubber. Summary of the invention

[0004] The present invention solves the technical problem by adopting the following technical solutions:

[0005] The high temperature and oil resistant rubber comprises, by weight, 100 parts of a polymer main material, 1-5 parts of a vulcanizing agent, 50-90 parts of a reinforcing agent, 1-10 parts of a plasticizer, 1-5 parts of an antioxidant, and 1-3 parts of stearic acid.

[0006] As a preferred embodiment, the polymer main body material is a combination of a polymer resin and a polymer rubber material, and the weight ratio of the polymer resin to the polymer rubber material is (1-5): (0.5-0.8).

[0007] As a preferred embodiment, the weight ratio of the polymer resin to the polymer rubber material is (2-4): (0.6-0.7).

[0008] As a preferred implementation, the weight ratio of the polymer resin to the polymer rubber material is 3:0.65.

[0009] As a preferred embodiment, the polymer resin is selected from one or a combination of at least two of ethylene-vinyl acetate copolymer, polyvinyl chloride, polyethylene, polystyrene, and polyurethane.

[0010] As a preferred embodiment, the polymer resin is polyvinyl chloride.

[0011] As a preferred embodiment, the polymer rubber material is selected from one or a combination of at least two of nitrile rubber, hydrogenated nitrile rubber, fluororubber, EPDM rubber, ethylene vinyl acetate rubber, and epoxy natural rubber.

[0012] As a preferred implementation, the polymer rubber material is hydrogenated nitrile rubber.

[0013] The applicant found during the experiment that the weight ratio of hydrogenated nitrile rubber to polyvinyl chloride (1-5): (0.5-0.8) can maintain good impact resistance and tensile strength of the stator lining rubber. The possible reason is speculated to be that hydrogen bonds are formed between the Cl atom and H between hydrogenated nitrile rubber and polyvinyl chloride, which enhances the intermolecular force between hydrogenated nitrile rubber and PVC. Under the preferred weight ratio, hydrogenated nitrile rubber and PVC can reach a state of nearly complete blending, presenting the properties of a homopolymer, reducing the gaps between the main materials, and improving the mechanical properties.

[0014] As a preferred embodiment, the mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 40-45%, the Mooney viscosity is 60-65, and the mass fraction of residual double bonds is less than 0.9%.

[0015] As a preferred embodiment, the mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 42-44%, the Mooney viscosity is 61-64, and the mass fraction of residual double bonds is less than 0.9%.

[0016] As a preferred embodiment, the mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 43%, the Mooney viscosity is 63, and the mass fraction of residual double bonds is less than 0.9%.

[0017] The applicant found in the experiment that the combination of hydrogenated nitrile rubber with an acrylonitrile content of 40-45% and PVC as the main material can improve the high temperature resistance and oil resistance of the lining rubber and extend the service life of the stator lining rubber. The possible reason is that the hydrogenated nitrile rubber with a residual double bond content of less than 0.9% makes the vast majority of carbon-carbon double bonds on the nitrile rubber molecular chain reach saturation, so that it has excellent heat resistance and aging resistance. The applicant further found that the combination of hydrogenated nitrile rubber with an acrylonitrile content of 43% and PVC has a good compatibility effect and high compatibility, improves the impact resistance of the stator lining rubber, and the hydrogenated nitrile rubber with an acrylonitrile content of 43% has a soft molecular chain, and the -CN bond contained in the molecular chain can also improve the oil resistance of the stator lining rubber, so that it is not easy to be denatured when working in a high temperature and high oil environment for a long time, and extends the service life of the stator lining rubber.

[0018] As a preferred embodiment, the polyvinyl chloride is selected from one or a combination of general-purpose polyvinyl chloride, high-polymerization polyvinyl chloride, and cross-linked polyvinyl chloride, and the viscosity of the polyvinyl chloride is 125-135 mL / g.

[0019] As a preferred embodiment, the polyvinyl chloride is selected from one or a combination of general-purpose polyvinyl chloride, high-polymerization polyvinyl chloride, and cross-linked polyvinyl chloride, and the viscosity of the polyvinyl chloride is 133 mL / g.

[0020] As a preferred embodiment, the vulcanizing agent is selected from one or a combination of sulfur or peroxide vulcanizing agents, and the peroxide vulcanizing agent is selected from one or a combination of dicumyl peroxide, di-tert-butyl peroxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

[0021] As a preferred embodiment, the vulcanizing agent is a combination of sulfur and di-tert-butyl peroxide.

[0022] As a preferred embodiment, the weight ratio of sulfur to di-tert-butyl peroxide is (2-5):1.

[0023] As a preferred embodiment, the weight ratio of sulfur to di-tert-butyl peroxide is 3:1.

[0024] As a preferred embodiment, the reinforcing agent is a modified filler, and the filler is selected from one or a combination of carbon black, nano zinc oxide, magnesium oxide, silicon dioxide, and silicon powder.

[0025] As a preferred embodiment, the reinforcing agent is carbon black and modified nano magnesium oxide.

[0026] As a preferred embodiment, the weight ratio of the carbon black to the modified nano magnesium oxide is 1:(0.3-0.8).

[0027] As a preferred embodiment, the weight ratio of the carbon black to the modified nano magnesium oxide is 1:0.5.

[0028] As a preferred embodiment, the preparation method of the modified nano magnesium oxide comprises the following steps:

[0029] Mix isopropanol and water, add acetic acid, and then add silane coupling agent to make a solution, stirring for hours until the solution becomes clear and transparent. Soak nano magnesium oxide in the solution, stir thoroughly so that the silane coupling agent can contact the surface of nano magnesium oxide, and then dry it at 120℃.

[0030] As a preferred embodiment, the particle size of the filler is 15-50 nm.

[0031] As a preferred embodiment, the particle size of the nano magnesium oxide is 20 nm, and the particle size of the carbon black is 25 nm.

[0032] The synergistic effect of carbon black with a particle size of 25 nm and modified nano-magnesium oxide can increase the cross-linking network density of the polymer main material and improve the hardness and mechanical properties of the stator lining rubber. The reason may be that the carbon black used has a large structure, good dispersibility, and a large amount of polymer main material, which can improve the overall structural density of the system. The applicant further found that the synergistic effect of carbon black and modified nano-magnesium oxide can avoid short-term scorching of the rubber during processing, which can meet good processing effects.

[0033] The plasticizer is methyl octyl phthalate, and the antioxidant is antioxidant IPPD.

[0034] A second aspect of the present invention provides a method for preparing a high temperature and oil resistant rubber, comprising the following steps:

[0035] Put the polymer main material and the vulcanizing agent into the internal mixer and mix them evenly. The roller distance of the internal mixer is 0.5-1mm.

[0036] Add reinforcing agent, plasticizer and antioxidant, and mix evenly;

[0037] Add stearic acid and mix for 10-15 minutes;

[0038] It flows out from the internal mixer and enters the open mixer for packaging and rolling to produce sheets.

[0039] The rubber can be used for the stator lining rubber of a screw pump.

[0040] The advantages and positive effects of the present invention are:

[0041] (1) The high temperature and oil resistant rubber of the present invention uses hydrogenated nitrile rubber with an acrylonitrile mass fraction of 40-45%, a Mooney viscosity of 63, and a residual double bond mass fraction of less than 0.9% as the main material. The prepared lining rubber has a high melting point, can withstand high temperatures during the use of the screw pump, and has the effects of high temperature resistance and oil resistance;

[0042] (2) The high temperature and oil resistant rubber of the present invention adopts the synergistic effect of hydrogenated nitrile rubber and polyvinyl chloride, which can make the stator lining rubber achieve good impact resistance and tensile strength, and can adapt to complex mining environments;

[0043] (3) The high temperature and oil resistant rubber of the present invention adopts sulfur and peroxide vulcanizing agents as the vulcanization system, which can reduce the vulcanization temperature, achieve the vulcanization effect in a shorter time, and reduce energy consumption;

[0044] (4) The high temperature and oil resistant rubber of the present invention can make the stator lining rubber reach a suitable hardness by introducing nano magnesium oxide and carbon black as reinforcing agents, and is not easy to become brittle in a low temperature environment, and has good low temperature resistance;

[0045] (5) The high temperature and oil resistant rubber of the present invention introduces nano magnesium oxide modified by a silane coupling agent, which can improve the compatibility between the filler and the polymer main material and avoid the degradation of mechanical properties caused by the presence of voids. DETAILED DESCRIPTION

[0046] First, it should be noted that the specific structure, features and advantages of the present invention are described in detail below by way of example, but all descriptions are only for illustration and should not be understood as limiting the present invention in any way. It should be noted that the embodiments and features in the embodiments in this application can be combined with each other without conflict.

[0047] Example 1

[0048] The high temperature and oil resistant rubber provided in this embodiment includes, by weight, 100 parts of a polymer main material, 1-5 parts of a vulcanizing agent, 50-90 parts of a reinforcing agent, 1-10 parts of a plasticizer, 1-5 parts of an antioxidant, and 1-3 parts of stearic acid.

[0049] As a preferred embodiment, the polymer main body material is a combination of a polymer resin and a polymer rubber material, and the weight ratio of the polymer resin to the polymer rubber material is (1-5): (0.5-0.8).

[0050] As a preferred embodiment, the weight ratio of the polymer resin to the polymer rubber material is (2-4): (0.6-0.7).

[0051] As a preferred implementation, the weight ratio of the polymer resin to the polymer rubber material is 3:0.65.

[0052] As a preferred embodiment, the polymer resin is selected from one or a combination of at least two of ethylene-vinyl acetate copolymer, polyvinyl chloride, polyethylene, polystyrene, and polyurethane.

[0053] As a preferred embodiment, the polymer resin is polyvinyl chloride.

[0054] As a preferred embodiment, the polymer rubber material is selected from one or a combination of at least two of nitrile rubber, hydrogenated nitrile rubber, fluororubber, EPDM rubber, ethylene vinyl acetate rubber, and epoxy natural rubber.

[0055] As a preferred implementation, the polymer rubber material is hydrogenated nitrile rubber.

[0056] The applicant found during the experiment that the weight ratio of hydrogenated nitrile rubber to polyvinyl chloride (1-5): (0.5-0.8) can maintain good impact resistance and tensile strength of the stator lining rubber. The possible reason is speculated to be that hydrogen bonds are formed between the Cl atom and H between hydrogenated nitrile rubber and polyvinyl chloride, which enhances the intermolecular force between hydrogenated nitrile rubber and PVC. Under the preferred weight ratio, hydrogenated nitrile rubber and PVC can reach a state of nearly complete blending, presenting the properties of a homopolymer, reducing the gaps between the main materials, and improving the mechanical properties.

[0057] As a preferred embodiment, the mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 40-45%, the Mooney viscosity is 60-65, and the mass fraction of residual double bonds is less than 0.9%.

[0058] As a preferred embodiment, the mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 42-44%, the Mooney viscosity is 61-64, and the mass fraction of residual double bonds is less than 0.9%.

[0059] As a preferred embodiment, the mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 43%, the Mooney viscosity is 63, and the mass fraction of residual double bonds is less than 0.9%.

[0060] The applicant found in the experiment that the combination of hydrogenated nitrile rubber with an acrylonitrile content of 40-45% and PVC as the main material can improve the high temperature resistance and oil resistance of the lining rubber and extend the service life of the stator lining rubber. The possible reason is that the hydrogenated nitrile rubber with a residual double bond content of less than 0.9% makes the vast majority of carbon-carbon double bonds on the nitrile rubber molecular chain reach saturation, so that it has excellent heat resistance and aging resistance. The applicant further found that the combination of hydrogenated nitrile rubber with an acrylonitrile content of 43% and PVC has a good compatibility effect and high compatibility, improves the impact resistance of the stator lining rubber, and the hydrogenated nitrile rubber with an acrylonitrile content of 43% has a soft molecular chain, and the -CN bond contained in the molecular chain can also improve the oil resistance of the stator lining rubber, so that it is not easy to be denatured when working in a high temperature and high oil environment for a long time, and extends the service life of the stator lining rubber.

[0061] As a preferred embodiment, the polyvinyl chloride is selected from one or a combination of general-purpose polyvinyl chloride, high-polymerization polyvinyl chloride, and cross-linked polyvinyl chloride, and the viscosity of the polyvinyl chloride is 125-135 mL / g.

[0062] As a preferred embodiment, the polyvinyl chloride is selected from one or a combination of general-purpose polyvinyl chloride, high-polymerization polyvinyl chloride, and cross-linked polyvinyl chloride, and the viscosity of the polyvinyl chloride is 133 mL / g.

[0063] As a preferred embodiment, the vulcanizing agent is selected from one or a combination of sulfur or peroxide vulcanizing agents, and the peroxide vulcanizing agent is selected from one or a combination of dicumyl peroxide, di-tert-butyl peroxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.

[0064] As a preferred embodiment, the vulcanizing agent is a combination of sulfur and di-tert-butyl peroxide.

[0065] As a preferred embodiment, the weight ratio of sulfur to di-tert-butyl peroxide is (2-5):1.

[0066] As a preferred embodiment, the weight ratio of sulfur to di-tert-butyl peroxide is 3:1.

[0067] As a preferred embodiment, the reinforcing agent is a modified filler, and the filler is selected from one or a combination of carbon black, nano zinc oxide, magnesium oxide, silicon dioxide, and silicon powder.

[0068] As a preferred embodiment, the reinforcing agent is carbon black and modified nano magnesium oxide.

[0069] As a preferred embodiment, the weight ratio of the carbon black to the modified nano magnesium oxide is 1:(0.3-0.8).

[0070] As a preferred embodiment, the weight ratio of the carbon black to the modified nano magnesium oxide is 1:0.5.

[0071] As a preferred embodiment, the preparation method of the modified nano magnesium oxide comprises the following steps:

[0072] Mix 87mL of isopropanol and 10mL of water, add 0.5mL of acetic acid, and then add 2mL of silane coupling agent KH550 to make a solution, stir for 1 hour while adding, until the solution becomes clear and transparent. Soak the nano-magnesium oxide in the solution, stir well for 3 hours, so that the silane coupling agent can contact the surface of the nano-magnesium oxide, and then dry it at 120℃.

[0073] As a preferred embodiment, the particle size of the filler is 15-50 nm.

[0074] As a preferred embodiment, the particle size of the nano magnesium oxide is 20 nm, and the particle size of the carbon black is 25 nm.

[0075] The synergistic effect of carbon black with a particle size of 25 nm and modified nano-magnesium oxide can increase the cross-linking network density of the polymer main material and improve the hardness and mechanical properties of the stator lining rubber. The reason may be that the carbon black used has a large structure, good dispersibility, and a large amount of polymer main material, which can improve the overall structural density of the system. The applicant further found that the synergistic effect of carbon black and modified nano-magnesium oxide can avoid short-term scorching of the rubber during processing, which can meet good processing effects.

[0076] The plasticizer is methyl octyl phthalate, and the antioxidant is antioxidant IPPD.

[0077] A second aspect of the present invention provides a method for preparing a high temperature and oil resistant rubber, comprising the following steps:

[0078] Put the polymer main material and the vulcanizing agent into the internal mixer and mix them evenly. The roller distance of the internal mixer is 0.5-1mm.

[0079] Add reinforcing agent, plasticizer and antioxidant, and mix evenly;

[0080] Add stearic acid and mix for 10-15 minutes;

[0081] It flows out from the internal mixer and enters the open mixer for packaging and rolling to produce sheets.

[0082] The rubber can be used for the stator lining rubber of a screw pump.

[0083] Example 2

[0084] The high temperature and oil resistant rubber is prepared by raw materials including, by weight, 100 parts of a polymer main material, 4.5 parts of a vulcanizing agent, 55 parts of a reinforcing agent, 2 parts of a plasticizer, 2 parts of an antioxidant, and 1 part of stearic acid.

[0085] The polymer main material is a combination of hydrogenated nitrile rubber and polyvinyl chloride, with a weight ratio of 3:0.65. The mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 43%, the Mooney viscosity is 63, and the residual double bond mass fraction is less than 0.9%. It was purchased from ARLANXEO, model 4307; the viscosity of the polyvinyl chloride is 133 mL / g, purchased from Xinjiang Tianye, model SG3.

[0086] The vulcanizing agent is a combination of sulfur and di-tert-butyl peroxide, with a weight ratio of 3:1.

[0087] The reinforcing agent is carbon black and modified nano magnesium oxide, with a weight ratio of 1:0.5. The particle size of the nano magnesium oxide is 20nm, and the particle size of the carbon black is 25nm, purchased from Cabot, USA, model R330R, and is a high-structure carbon black.

[0088] The preparation method of the modified nano magnesium oxide comprises the following steps:

[0089] Mix 87mL of isopropanol and 10mL of water, add 0.5mL of acetic acid, and then add 2mL of silane coupling agent KH550 to make a solution, stir for 1 hour while adding, until the solution becomes clear and transparent. Soak 10mg of nano-magnesium oxide in the solution, stir well for 3h, so that the silane coupling agent can contact the surface of nano-magnesium oxide, and then dry it at 120℃.

[0090] The plasticizer is methyl octyl phthalate, and the antioxidant is antioxidant IPPD.

[0091] The method for preparing high temperature and oil resistant rubber comprises the following steps:

[0092] Put the polymer main material and the vulcanizing agent into an internal mixer and mix them evenly. The roller distance of the internal mixer is 0.5mm.

[0093] Add reinforcing agent, plasticizer and antioxidant, and mix evenly;

[0094] Add stearic acid and mix for 10 minutes;

[0095] It flows out from the internal mixer and enters the open mixer for packaging and rolling to produce sheets.

[0096] The rubber can be used for the stator lining rubber of a screw pump.

[0097] Example 3

[0098] The high temperature and oil resistant rubber provided in this embodiment has the same specific components and steps as in Example 2, except that the main polymer material is a combination of EPDM rubber and polyvinyl chloride in a weight ratio of 1:0.5; the reinforcing agent is carbon black and modified nano magnesium oxide in a weight ratio of 1:0.3.

[0099] Example 4

[0100] The high temperature and oil resistant rubber provided in this embodiment has the same specific components and steps as Example 2, except that the main polymer material is a combination of hydrogenated nitrile rubber and polyethylene in a weight ratio of 5:0.8; the reinforcing agent is carbon black and modified nano magnesium oxide in a weight ratio of 1:0.8.

[0101] Example 5

[0102] The high temperature and oil resistant rubber provided in this embodiment has the same specific components and steps as Example 2, except that the main polymer material is a combination of hydrogenated nitrile rubber and polystyrene in a weight ratio of 3:0.55; the reinforcing agent is carbon black and modified nano magnesium oxide in a weight ratio of 1:0.6.

[0103] Example 6

[0104] The high temperature and oil resistant rubber provided in this embodiment has the same specific components and steps as those in Embodiment 2, except that the main polymer material is hydrogenated nitrile rubber.

[0105] Example 7

[0106] The high temperature and oil resistant rubber provided in this embodiment has the same specific components and steps as those in Embodiment 2, except that the main polymer material is a combination of hydrogenated nitrile rubber and polyethylene; the polyethylene is purchased from SABIC, model number HP4027JN.

[0107] Example 8

[0108] The high temperature and oil resistant rubber provided in this embodiment has the same specific steps as in embodiment 2, except that the reinforcing agent is carbon black and modified nano magnesium oxide, with a weight ratio of 1:0.5. The carbon black is purchased from Cabot, USA, model N326, and is a low structure carbon black.

[0109] Example 9

[0110] The high temperature and oil resistant rubber provided in this embodiment has the same specific steps as in Embodiment 2, except that the vulcanizing agent is sulfur.

[0111] Performance Testing

[0112] 1. The tensile properties of the high temperature and oil resistant rubber prepared in Examples 2-6 were tested with reference to GB / T1040-1992 standard.

[0113] 2. The hardness of the high temperature and oil resistant rubber prepared in Examples 2-6 was tested with reference to GB / T531-1999 standard.

[0114] 3. Oil resistance test: The high temperature and oil resistant rubber prepared in Examples 2-6 was immersed in 0# diesel at 110°C and a pressure of 0.1 MPa for 168 hours, and the mass change rate was tested; mass change rate = (mass before immersion - mass after immersion) / mass before immersion × 100%.

[0115] The test results are shown in Table 1.

[0116] Table 1

[0117]

[0118]

[0119] The above embodiments describe the present invention in detail, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.

Claims

1. High temperature and oil resistant rubber, characterized in that: It includes the following components in parts by weight: 100 parts of polymer main material; 1-5 parts of vulcanizing agent; 50-90 parts of reinforcing agent; 1-10 parts of plasticizer; 1-5 parts of antioxidant; 1-3 parts of stearic acid; The polymer main body material is a combination of a polymer resin and a polymer rubber material, and the weight ratio of the polymer resin to the polymer rubber material is (1-5): (0.5-0.8).

2. The high temperature and oil resistant rubber according to claim 1, characterized in that: The polymer resin is one of ethylene-vinyl acetate copolymer, polyvinyl chloride, polyethylene, polystyrene, and polyurethane, or a combination of at least two of them.

3. The high temperature and oil resistant rubber according to claim 1, characterized in that: The polymer rubber material is one of nitrile rubber, hydrogenated nitrile rubber, fluororubber, EPDM rubber, ethylene vinyl acetate rubber, and epoxy natural rubber, or a combination of at least two of them.

4. The high temperature and oil resistant rubber according to claim 3, characterized in that: The mass fraction of acrylonitrile in the hydrogenated nitrile rubber is 40-45%, the Mooney viscosity is 60-65, and the mass fraction of residual double bonds is less than 0.9%.

5. The high temperature and oil resistant rubber according to claim 2, characterized in that: The polyvinyl chloride is one of general-purpose polyvinyl chloride, high-polymerization polyvinyl chloride, and cross-linked polyvinyl chloride, or a combination of at least two thereof, and the viscosity of the polyvinyl chloride is 125-135 mL / g.

6. The high temperature and oil resistant rubber according to claim 1, characterized in that: The vulcanizing agent is one of sulfur or a peroxide vulcanizing agent or a combination of at least two thereof; the peroxide vulcanizing agent is one of diisopropylbenzene peroxide, di-tert-butyl peroxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide or a combination of at least two thereof.

7. The high temperature and oil resistant rubber according to claim 1, characterized in that: The reinforcing agent is carbon black and modified nano magnesium oxide, and the weight ratio of the carbon black to the modified nano magnesium oxide is 1:(0.3-0.8).

8. The high temperature and oil resistant rubber according to claim 7, characterized in that: The preparation method of the modified nano magnesium oxide comprises the following steps: Mix isopropanol and water, add L acetic acid, and then add silane coupling agent to form a solution, stirring while adding until the solution becomes clear and transparent; immerse nano-magnesium oxide in the solution, stir so that the silane coupling agent can contact the surface of the nano-magnesium oxide, and then dry it.

9. The method for preparing the high temperature and oil resistant rubber according to any one of claims 1 to 8, characterized in that: The steps include: Put the polymer main material and the vulcanizing agent into the internal mixer and mix them evenly. The roller distance of the internal mixer is 0.5-1mm. Add reinforcing agent, plasticizer and antioxidant, and mix evenly; Add stearic acid and mix for 10-15 minutes; It flows out from the internal mixer and enters the open mixer for packaging and rolling to produce sheets.

10. Use of the high temperature and oil resistant rubber according to any one of claims 1 to 8, characterized in that: The rubber can be used for the stator lining rubber of a screw pump.

Citation Information

Cited By

  • Rubber composite material as well as preparation method and application thereof

    CN122706002A