Polyethylene-based anti-static and flame-retardant composite material for rotational molding and preparation method thereof

By using chemically modified carbon nanotubes and ionic liquids in polyethylene materials, combined with a twin-screw extrusion process, composite materials with antistatic and flame retardant properties are prepared, which solves the problem of insufficient flame retardant and antistatic properties of traditional materials. problem, achieving high-efficiency mechanical properties and improved flame retardant properties of the material.

CN118725437AInactive Publication Date: 2024-10-01CIXI AIDIWEI ROTOMOLDING EQUIP TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410854227.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional rotomolded polyethylene materials have deficiencies in flame retardant and antistatic properties, which limits their application in special fields. Adding low-resistance materials will lead to a decrease in dielectric strength and loss of insulation. Intumescent flame retardants will It is easy to foam when exposed to water, affecting material properties.

Method used

A polyethylene-based composite material is used to chemically modify and functionalize carbon nanotubes, and combine with ionic liquids to form functional carbon nanotubes, which are used to prepare flame-retardant and antistatic masterbatch, combining LLDPE, LDPE and Other additives are used to prepare composite materials with antistatic and flame retardant properties through twin-screw extrusion and grinding processes.

Benefits of technology

It achieves the permanent antistatic/flame retardant characteristics of composite materials, optimizes the mechanical properties and flame retardant properties, overcomes the foaming problem of traditional materials at high temperatures, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917641760000031
    Figure BDA0004917641760000031
  • Figure BDA0004917641760000051
    Figure BDA0004917641760000051
  • Figure BDA0004917641760000061
    Figure BDA0004917641760000061
Patent Text Reader

Abstract

The invention relates to the field of polymer materials, and discloses an antistatic and flame-retardant composite material based on polyethylene rotational moulding and a preparation method thereof, the antistatic and flame-retardant composite material comprises the following components: 25.0%-35.0% of LLDPE, 35.0%-55.0% of LDPE, and 20%-40% of flame-retardant antistatic master batch; wherein the flame-retardant antistatic master batch is prepared from the following components in percentage by mass: 30.0%-55.0% of LLDPE (Linear Low Density Polyethylene), 2.0%-8.0% of CNT (Carbon Nanotubes), 7.0%-50.0% of functional carbon nanotubes, 6.0%-10.0% of a toughening agent, 6.0%-10.0% of PE (Polyethylene) wax and 6.0%-10.0% of an antioxidant. According to the invention, the flame retardant property of the ionic liquid and the conductivity of the carbon nanotube are utilized to overcome the difficulty of the existing carbon nanotube thermoplastic composite material, the prepared composite material has a lower percolation threshold value, the mechanical property of the composite material can be optimized, and the composite material has the characteristic of permanent antistatic / flame retardant property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer high molecular materials, in particular to a composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, belonging to the technical field of high molecular composite materials. Background Art

[0002] Roto-molding is a unique process that produces products without internal stress without pressure, which enables the manufacture of large, super-large, multi-color, multi-wall military packaging products. For example, military equipment packaging boxes (missiles, shells, rockets, grenades, mines, etc.), military food airdrop packaging, etc. However, in addition to meeting the function of packaging, such special products are often required to have different functions in different applications (such as anti-static flame retardancy, high impact and weather resistance, or high strength and light weight, etc.).

[0003] The deficiencies of traditional roto-molded polyethylene products in flame retardancy and antistatic properties have greatly limited the application of their products in special fields (such as electronic and electrical packaging, fuel chemical storage and transportation). Traditional polyolefin flame retardant methods are not suitable for roto-molding processing and cannot be used for the production of roto-molded products due to the large dosage of flame retardants added and the large decline in product performance. On the other hand, due to the high resistance of polyethylene, static charges will accumulate on the surface of the product when it encounters contact, friction, collision, etc. during use, and the generated static charges are difficult to transfer. When accumulated to a certain extent, it will bring safety hazards. Usually, antistatic agents, carbon black, metal powders and other low-resistance substances are added to polyethylene materials to reduce the surface resistance and volume resistance of polyethylene materials to achieve antistatic effects. However, under current technical conditions, the addition of low-resistance materials to the materials will directly cause a significant decrease in the dielectric strength (electrical breakdown strength) of the plastic material, causing the plastic to lose its insulation.

[0004] Based on this, polyethylene needs to be modified to improve its performance. At present, some patents involve flame-retardant and antistatic roto-molded polyethylene materials, but the flame retardant types involved in these patents are mainly intumescent flame retardants, which require a large amount of addition to achieve a certain flame retardant level, significantly reducing the physical properties of the material (for example, impact resistance); and intumescent flame retardants are prone to foaming at high temperatures to produce molding defects, which is an important unfavorable factor in the roto-molding process.

[0005] In carbon nanotube / polymer composites, the dispersion of fillers and the interaction between interfaces are important factors affecting the mechanical properties of materials. Among them, one of the important challenges is the uniform dispersion of carbon nanotubes in the polymer matrix, because the van der Waals force between carbon nanotubes causes the carbon nanotubes to aggregate and agglomerate, reducing the improvement of the performance of the composite material. The performance of carbon nanotubes can be further improved by chemically modifying and functionalizing carbon nanotubes. The chemical modification of the surface of carbon nanotubes has its unique advantages. After chemical modification, the structure of carbon nanotubes will basically not be damaged and the original structure can be better maintained. Chemical modification can increase the interface effect between carbon nanotubes and polymer matrix, and can realize stress transfer between the interface of polymer and filler. Applying carbon nanotube fibers as functional additives to mixed systems can simultaneously enhance the mechanical properties, electrical conductivity and thermal stability of composite materials. Summary of the invention

[0006] The present invention aims to provide a composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof.

[0007] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is:

[0008] A composite material with both antistatic and flame retardancy for polyethylene rotational molding, comprising the following components:

[0009] LLDPE 25.0%~35.0%

[0010] LDPE 35.0%~55.0%

[0011] Flame retardant antistatic masterbatch 20%~40%

[0012] Wherein, the flame retardant antistatic masterbatch comprises the following components:

[0013] LLDPE 30.0%~55.0%

[0014] CNT 2.0%~8.0%

[0015] Functional carbon nanotubes 7.0%~50.0%

[0016] Toughening agent 6.0%~10.0%

[0017] PE wax 6.0%~10.0%

[0018] Antioxidant 6.0%~10.0%

[0019] The above proportions are all mass percentages.

[0020] A method for preparing a composite material with antistatic and flame retardancy for polyethylene rotational molding comprises the following steps:

[0021] (1) Preparation of additives:

[0022] Step 1: Synthesis of polyionic liquid: Using monomers represented by formula (III), formula (IV) and formula (V), a polyionic liquid PIL is synthesized by free radical polymerization, and the structural formula is shown in formula (I):

[0023]

[0024] Step 2: Preparation of functional carbon nanotubes:

[0025] Under ultrasonic conditions, the carbon nanotubes are cleaned with acetone, and then immersed in 10-30 wt. / v% of the polyionic liquid PIL prepared in the first step, stirred for 2-8 hours, filtered and dried to obtain polyionic liquid modified functional carbon nanotubes PIL@CNT, wherein the functional carbon nanotubes PIL@CNT are shown in structural formula (II);

[0026] (2) Masterbatch preparation:

[0027] Weigh carbon nanotubes and PE wax according to weight ratio and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 5-8 minutes; then add LLDPE, functional carbon nanotubes, toughening agent, and antioxidant and blend at about 80°C for 3-5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant antistatic masterbatch;

[0028] (3) Extrusion granulation:

[0029] Weigh LLDPE, LDPE, carbon nanotubes, and flame retardant and antistatic masterbatch according to the weight ratio, blend them in a high-speed mixer for 3 to 5 minutes, and then put them into a twin-screw extruder for extrusion, cooling, pelletizing, and drying the obtained particles for later use;

[0030] (4) Mechanical grinding:

[0031] Under the protection of nitrogen, the particles obtained in step (3) are ground into powder of about 40 to 50 meshes using a grinding machine to obtain a polyethylene rotational molding composite material with both antistatic and flame retardancy.

[0032] Furthermore, in the structural formula (I), x:y:z=15%-30%:20-40%:30-65%, preferably x:y:z=25%:30%:45%.

[0033] Furthermore, in the structural formula (II), the mass ratio of the polyionic liquid to the carbon nanotubes is 40% to 60%:40% to 60%, preferably 50:50.

[0034] Furthermore, the carbon nanotubes in the flame retardant and antistatic masterbatch are single-arm carbon nanotubes, multi-arm carbon nanotubes or a combination thereof.

[0035] Furthermore, the flame retardant antistatic agent in the flame retardant antistatic masterbatch is functional carbon nanotubes.

[0036] Furthermore, the toughening agent in the flame retardant and antistatic masterbatch is one or a combination of POE-g-MAH, POE-g-GMA, and PE-g-MAH.

[0037] Furthermore, the antioxidant in the flame retardant and antistatic masterbatch is one of 168, 1010, 1098 or a combination thereof.

[0038] Compared with the prior art, the advantages of the present invention are:

[0039] (1) By utilizing the flame retardant properties of ionic liquids and the conductive properties of carbon nanotubes, this filler is endowed with a permanent "dual" function, overcoming the difficulties of existing carbon nanotube thermoplastic composites: the prepared composite material has a low percolation threshold, can also optimize the mechanical properties of the composite material, and has permanent antistatic / flame retardant characteristics.

[0040] (2) The ionic liquid with both imidazole and phosphoric acid structures in the system gives the composite material excellent flame retardant properties. The dehydration of the O-P=O structure in the modified polymer molecules can promote the formation of a dense carbon layer to isolate heat and oxygen. The generated phosphorus-containing oxygen free radical gas dilutes the air and quenches the flame. The modified carbon nanotubes improve the flame retardancy and mechanical properties of the composite material. DETAILED DESCRIPTION

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the embodiments are briefly introduced below. Obviously, the following description only relates to some embodiments of the present invention, but does not limit the present invention.

[0042] The method for preparing the composite material with both antistatic and flame retardancy for polyethylene rotational molding of the present invention comprises the following steps:

[0043] (1) Preparation of additives:

[0044] Step 1: Synthesis of polyionic liquids. The monomers represented by formula (III), formula (IV) and formula (V) are used to synthesize polyionic liquids (PILs) by free radical polymerization (method references: Journal of Membrane Science 574 (2019) 212–221; Journal of Membrane Science 541 (2017) 244–252), and the structural formula is shown in formula (I).

[0045]

[0046]

[0047] Step 2: Preparation of functional carbon nanotubes:

[0048] Under ultrasonic conditions, the carbon nanotubes are cleaned with acetone, and then immersed in 10-30wt. / v% of the polyionic liquid (PIL) prepared in the first step, stirred for 2-8 hours, filtered and dried to obtain functional carbon nanotubes modified with polyionic liquid (PIL@CNT). The functional carbon nanotubes (PIL@CNT, flame retardant and antistatic agent) are shown in structural formula (II).

[0049] (2) Masterbatch preparation:

[0050] Weigh carbon nanotubes and PE wax according to weight ratio and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 5-8 minutes; then add LLDPE, functional carbon nanotubes, toughening agent, and antioxidant and blend at about 80°C for 3-5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant antistatic masterbatch;

[0051] (3) Extrusion granulation:

[0052] Weigh LLDPE, LDPE, carbon nanotubes, and flame retardant and antistatic masterbatch according to the weight ratio, blend them in a high-speed mixer for 3 to 5 minutes, and then put them into a twin-screw extruder for extrusion, cooling, pelletizing, and drying the obtained particles for later use;

[0053] (4) Mechanical grinding:

[0054] Under the protection of nitrogen, the particles obtained in step (3) are ground into powder of about 40 to 50 meshes using a grinding machine to obtain a polyethylene rotational molding composite material with both antistatic and flame retardancy.

[0055] The melt index of the polyethylene rotomolding composite material with both antistatic and flame retardancy prepared by the technical solution provided by the present invention is ≥5g / 10min, the tensile strength is 10-12MPa, and the simply supported beam notched impact strength is 5-10kJ / m 2 , the surface resistance is 10 6 ~10 7 Ω, and the flame retardant grade reaches UL 94V-0 level.

[0056] Example 1

[0057] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0058] (1) Preparation of additives:

[0059] Synthesis of polyionic liquid: Weigh 5 parts by weight of monomer (III), 6 parts by weight of monomer (IV) and 9 parts by weight of monomer (V), remove the inhibitor from Al2O3, add 1% azobisisobutyronitrile (AIBN), react for 5 hours at 60°C under argon atmosphere, and precipitate in methanol to obtain polyionic liquid (I)

[0060] Preparation of functional carbon nanotubes: Single-walled carbon nanotubes were washed with acetone under ultrasonic conditions, and then immersed in 20 wt. / v% polyionic liquid (I), stirred for 5 hours, filtered and dried to obtain polyionic liquid modified functional single-walled carbon nanotubes (PIL@CNT).

[0061] (2) Masterbatch preparation:

[0062] Weigh 8 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 70 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0063] (3) Extrusion granulation:

[0064] Weigh 200 parts by weight of LLDPE, 500 parts by weight of LDPE, and 300 parts by weight of flame retardant and antistatic masterbatch, blend them in a high-speed mixer for 5 minutes, put them into a twin-screw extruder again for extrusion, cooling, pelletizing, and drying the obtained particles for use; during the extrusion granulation process, the parameters of the twin-screw extruder are: zone 1 165°C, zone 2 170°C, zone 3 180°C, zone 4 190°C, zone 5 190°C, die head 175°C, and screw speed 100r / min.

[0065] (4) Mechanical grinding:

[0066] Under the protection of nitrogen, the particles obtained in step (3) are ground into powder of about 40 to 50 meshes using a grinding machine to obtain a polyethylene rotational molding composite material with both antistatic and flame retardancy.

[0067] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0068] Example 2

[0069] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0070] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0071] (2) Masterbatch preparation:

[0072] 18 parts by weight of CNT and 24 parts by weight of PE wax are weighed and added into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then 150 parts by weight of LLDPE, 60 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant are added and blended at about 80°C for 5 minutes; the above-mentioned uniformly mixed materials are put into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0073] (3) Extrusion granulation method is the same as in Example 1

[0074] (4) Mechanical grinding method is the same as in Example 1

[0075] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0076] Example 3

[0077] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0078] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0079] (2) Masterbatch preparation:

[0080] Weigh 28 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 50 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0081] (3) Extrusion granulation method is the same as in Example 1

[0082] (4) Mechanical grinding method is the same as in Example 1

[0083] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0084] Example 4

[0085] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0086] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0087] (2) Masterbatch preparation:

[0088] Weigh 38 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 40 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0089] (3) Extrusion granulation method is the same as in Example 1

[0090] (4) Mechanical grinding method is the same as in Example 1

[0091] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0092] Example 5

[0093] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0094] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0095] (2) Masterbatch preparation:

[0096] Weigh 48 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 30 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0097] (3) Extrusion granulation method is the same as in Example 1

[0098] (4) Mechanical grinding method is the same as in Example 1

[0099] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0100] Example 6

[0101] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0102] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0103] (2) Masterbatch preparation:

[0104] Weigh 58 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 20 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0105] (3) Extrusion granulation method is the same as in Example 1

[0106] (4) Mechanical grinding method is the same as in Example 1

[0107] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0108] Example 7

[0109] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0110] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0111] (2) Masterbatch preparation:

[0112] Weigh 68 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 10 parts by weight of functional carbon nanotubes (PIL@CNT), 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0113] (3) Extrusion granulation method is the same as in Example 1

[0114] (4) Mechanical grinding method is the same as in Example 1

[0115] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0116] Comparative Example 8

[0117] A composite material with both antistatic and flame retardancy for polyethylene rotational molding and a preparation method thereof, comprising the following steps:

[0118] (1) The preparation method of the auxiliary agent is the same as that of Example 1

[0119] (2) Masterbatch preparation:

[0120] Weigh 78 parts by weight of CNT and 24 parts by weight of PE wax and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 8 minutes; then add 150 parts by weight of LLDPE, 24 parts by weight of toughening agent, and 24 parts by weight of antioxidant and blend at about 80°C for 5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant and antistatic masterbatch.

[0121] (3) Extrusion granulation method is the same as in Example 1

[0122] (4) Mechanical grinding method is the same as in Example 1

[0123] The test devices used were: Instron 5567 (tensile properties, test standard: ASTM D638) produced by Instron Corporation of the United States; XJ-50Z (impact properties, Izod notched impact strength test standard: ASTM D256) produced by Chengde Dahua Company.

[0124]

[0125]

[0126] Table 1 Material ratio table of each embodiment and comparative example.

[0127]

[0128] Table 2 Performance comparison table of the embodiments.

Claims

1. A composite material with both antistatic and flame retardancy for polyethylene rotational molding, characterized in that The components include: LLDPE 25.0%~35.0% LDPE 35.0%~55.0% Flame retardant antistatic masterbatch 20%~40% Wherein, the flame retardant antistatic masterbatch comprises the following components: LLDPE 30.0%~55.0% CNT 2.0%~8.0% Functional carbon nanotubes 7.0%~50.0% Toughening agent 6.0%~10.0% PE wax 6.0%~10.0% Antioxidant 6.0%~10.0% The above proportions are all mass percentages.

2. A method for preparing a composite material with antistatic and flame retardancy for polyethylene rotational molding as claimed in claim 1, characterized in that The following steps are involved: (1) Preparation of additives: Step 1: Synthesis of polyionic liquid: Using monomers represented by formula (III), formula (IV) and formula (V), a polyionic liquid PIL is synthesized by free radical polymerization, and the structural formula is shown in formula (I): Step 2: Preparation of functional carbon nanotubes: Under ultrasonic conditions, the carbon nanotubes are cleaned with acetone, and then immersed in 10-30 wt. / v% of the polyionic liquid PIL prepared in the first step, stirred for 2-8 hours, filtered and dried to obtain polyionic liquid modified functional carbon nanotubes PIL@CNT, wherein the functional carbon nanotubes PIL@CNT are shown in structural formula (II); (2) Masterbatch preparation: Weigh carbon nanotubes and PE wax according to weight ratio and add them into a high-speed mixer, the blending temperature is 85-110°C, and the blending time is 5-8 minutes; then add LLDPE, functional carbon nanotubes, toughening agent, and antioxidant and blend at about 80°C for 3-5 minutes; put the above mixed materials into a twin-screw extruder for extrusion, cooling, pelletizing, and drying to obtain a flame retardant antistatic masterbatch; (3) Extrusion granulation: Weigh LLDPE, LDPE, carbon nanotubes, and flame retardant and antistatic masterbatch according to the weight ratio, blend them in a high-speed mixer for 3 to 5 minutes, and then put them into a twin-screw extruder for extrusion, cooling, pelletizing, and drying the obtained particles for later use; (4) Mechanical grinding: Under the protection of nitrogen, the particles obtained in step (3) are ground into powder of about 40 to 50 meshes using a grinding machine to obtain a polyethylene rotational molding composite material with both antistatic and flame retardancy.

3. The method for preparing a composite material with antistatic and flame retardancy based on polyethylene rotational molding according to claim 2, characterized in that: In the structural formula (I), x:y:z=15%-30%:20-40%:30-65%, preferably x:y:z=25%:30%:45%.

4. The method for preparing a composite material with antistatic and flame retardancy based on polyethylene rotational molding according to claim 2, characterized in that: The mass ratio of the polyionic liquid to the carbon nanotubes in the structural formula (II) is 40% to 60%:40% to 60%, preferably 50:

50.

5. The method for preparing a composite material with antistatic and flame retardancy for polyethylene rotational molding according to claim 2, characterized in that: The carbon nanotubes in the flame retardant and antistatic masterbatch are single-arm carbon nanotubes, multi-arm carbon nanotubes or a combination thereof.

6. The method for preparing a composite material with antistatic and flame retardancy for polyethylene rotational molding according to claim 2, characterized in that: The flame retardant and antistatic agent in the flame retardant and antistatic masterbatch is functional carbon nanotubes.

7. The method for preparing a composite material with antistatic and flame retardancy for polyethylene rotational molding according to claim 2, characterized in that: The toughening agent in the flame retardant and antistatic masterbatch is one of POE-g-MAH, POE-g-GMA, PE-g-MAH or a combination thereof.

8. The method for preparing a composite material with antistatic and flame retardancy for polyethylene rotational molding according to claim 2, characterized in that: The antioxidant in the flame retardant and antistatic masterbatch is one of 168, 1010, 1098 or a combination thereof.

Citation Information

Patent Citations

  • Flame retardant and antistatic polyethylene composition special for rotational moulding and preparation method thereof

    CN106867080A

  • Carbon nanotube-dispersed polyionic liquid organic solid electrolyte and preparation method thereof