Biodegradable polyethylene composite material under natural environment and preparation method thereof
By adding biodegradation aids such as modified starch/polylactic acid complex to polyethylene, combined with other plasticizers and compatibilizers, the problem of difficult degradation of traditional polyethylene plastics is solved, and efficient biodegradation and environmental protection performance are achieved. promote.
Patent Information
- Application Number
- CN202411020996.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional polyethylene plastic is difficult to degrade, leading to environmental pollution and resource waste. Its production process consumes a large amount of fossil fuels and generates a large amount of carbon dioxide.
Develop a polyethylene composite material that is biodegradable in the natural environment by adding modified starch/polylactic acid complex as a biodegradation aid to polyethylene and combining it with glycerol fatty acid ester, ethylene-vinyl acetate copolymer or maleic acid. Anhydride-grafted polyethylene serves as a compatibilizer and photosensitizer to promote the degradation of materials under the action of microorganisms.
It significantly improves the biodegradability of polyethylene composite materials, shortens the degradation time, reduces carbon emissions and energy consumption, and at the same time improves the material's flexibility and high and low temperature resistance.
Smart Images

Figure CN118725440A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodegradation, in particular to a biodegradable polyethylene composite material in a natural environment and a preparation method thereof. Background Art
[0002] With the rapid development of human society, plastic products are increasingly used in daily life. However, the extensive use of these plastic products has also brought serious environmental problems, especially the "white pollution" caused by non-degradable polyethylene plastics.
[0003] Polyethylene is a widely used plastic material that is used in a wide range of applications including packaging, agricultural films and containers due to its chemical resistance, electrical insulation and good mechanical properties.
[0004] Traditional polyethylene plastics are landfilled in large quantities due to their difficult-to-degrade properties, resulting in large tracts of land being occupied for a long time, seriously affecting the sustainable use of the land.
[0005] Biodegradation of polyethylene plastics helps reduce carbon emissions and energy consumption. The production process of traditional polyethylene plastics consumes a lot of fossil fuels and produces a lot of carbon dioxide emissions. In contrast, biodegradable polyethylene plastics have lower carbon emissions during production and use, and their degradation process can further reduce the negative impact on the environment. The application of biodegradable technology can enable polyethylene plastics to complete the degradation process in a shorter period of time, thereby releasing occupied land resources and providing more space for agricultural production and urban development.
[0006] In summary, the biodegradation of polyethylene plastics is of great significance in alleviating the pressure on land resources, reducing carbon emissions and energy consumption, protecting the ecological environment, and promoting green development.
[0007] Based on this, the present invention provides a polyethylene composite material that can be biodegraded in a natural environment to solve the corresponding problem. Summary of the invention
[0008] In view of the problems in the prior art, the present invention provides a polyethylene composite material that can be biodegraded in a natural environment and a preparation method thereof.
[0009] The technical solution adopted by the present invention to solve the technical problem is: a biodegradable polyethylene composite material in a natural environment, composed of the following components by weight: High density polyethylene: 85-95 parts; Biodegradable additives: 5-10 parts; Plasticizer: 0.1-3 parts; Compatibilizer: 0.2-5 parts; Photosensitizer: 0.01-1 part; Among them, the molecular weight of high-density polyethylene is 100,000.
[0010] As a further technical solution: the biodegradable aid is a modified starch / polylactic acid composite.
[0011] As a further technical solution: the preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep the mixture warm and stir for 10 minutes to obtain a mixed solution; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
[0012] As a further technical solution: the method for preparing the pretreated starch is: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
[0013] As a further technical solution: the starch is soybean starch; The starch mass fraction in the starch emulsion is 30-35%; The starch emulsion is adjusted to pH 3.5 by using a 5% by mass hydrochloric acid aqueous solution; The mixing mass ratio of starch emulsion and sodium sulfite solution is 10:1-1.6; The concentration of the sodium sulfite solution is 1 mol / L; The pH of the reaction system was adjusted to neutral by using a 5% by mass sodium hydroxide solution.
[0014] As a further technical solution: the mixing ratio of the pretreated starch and dimethyl sulfoxide in step (2) is 32-35 g:100 mL.
[0015] As a further technical solution: in step (3), the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL: 1-1.2g: 10-13g; Evacuate to 0.1Pa.
[0016] As a further technical solution: the plasticizer is glycerol fatty acid ester.
[0017] As a further technical solution: the compatibilizer is ethylene-vinyl acetate copolymer or maleic anhydride grafted polyethylene; The photosensitizer is dialkoxyacetophenone.
[0018] A method for preparing a biodegradable polyethylene composite material in a natural environment comprises the following steps: a. uniformly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and melt mix it at a temperature of 160-220°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product.
[0019] Beneficial effects of the present invention: The polyethylene composite material prepared by the invention can be biodegraded in a natural environment with a high degradation rate, which conforms to the contemporary theme of energy conservation and environmental protection.
[0020] The invention can promote the degradation of the polyethylene composite material under the action of microorganisms by introducing a biodegradation aid into the polyethylene composite material. For the polyethylene composite material, the addition of the biodegradation aid can significantly improve its biodegradability and accelerate its degradation process.
[0021] When the polyethylene composite material prepared by the present invention comes into contact with microorganisms and is eroded by microorganisms, the microbial population can better adhere to the surface of the polyethylene composite material under the action of the added biodegradation aid, and erode the polyethylene molecules through a variety of biological or chemical actions or secreted enzymes. These enzymes can recognize and attack specific parts of the polyethylene molecules, making them gradually unstable, which can further induce the breakage of the polyethylene molecular chain and accelerate the degradation process of the polyethylene molecules.
[0022] Under the action of microorganisms, the long-chain molecules of polyethylene are hydrolyzed into short-chain molecules. This is a gradual process that requires a long period of accumulation. The addition of the biodegradation aid introduced in the present invention can greatly improve the efficiency of this process, making the polyethylene molecular chains more easily utilized by microorganisms, greatly accelerating the entire degradation process, so that the manufactured polyethylene composite material product maintains a high biodegradation rate.
[0023] When polyethylene is hydrolyzed into short-chain molecules, the short-chain molecules will be further decomposed and metabolized by microorganisms. The short-chain molecules will continue to break under the action of microorganisms, and eventually generate small molecular compounds such as fatty acids. These small molecular compounds can be further absorbed and utilized by microorganisms to complete the entire degradation process.
[0024] By introducing glycerol fatty acid esters, the interaction force between polyethylene molecules can be reduced, and the distance between molecules can be increased. This increase in distance improves the mobility between polyethylene molecules, thereby increasing the flexibility of the material. Glycerol fatty acid esters can also affect the crystal structure of polyethylene, lowering its glass transition temperature, thereby improving its resistance to high and low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0026] Figure 1 The graph is a time-biodegradation percentage (%) curve of the sample in Example 1 and the positive reference. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application. Example 1
[0028] A biodegradable polyethylene composite material in a natural environment, comprising the following components by weight:
[0029] Among them, the molecular weight of high-density polyethylene is 100,000.
[0030] The biodegradable aid is a modified starch / polylactic acid complex.
[0031] The preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep warm and stir for 10 minutes to obtain a mixed solution; the mixing ratio of the pretreated starch and dimethyl sulfoxide is 32g:100mL; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL:1g:10g; Vacuum to 0.1Pa; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
[0032] The preparation method of pretreated starch is as follows: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
[0033] The plasticizer is glycerol fatty acid ester.
[0034] The compatibilizer is ethylene-vinyl acetate copolymer; The photosensitizer is dialkoxyacetophenone.
[0035] A method for preparing a biodegradable polyethylene composite material in a natural environment comprises the following steps: a. Evenly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and melt mix it at a temperature of 160°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product. Example 2
[0036] A biodegradable polyethylene composite material in a natural environment, comprising the following components by weight:
[0037] Among them, the molecular weight of high-density polyethylene is 100,000.
[0038] The biodegradable aid is a modified starch / polylactic acid complex.
[0039] The preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep warm and stir for 10 minutes to obtain a mixed solution; the mixing ratio of the pretreated starch and dimethyl sulfoxide is 32g:100mL; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL:1g:10g; Vacuum to 0.1Pa; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
[0040] The preparation method of pretreated starch is as follows: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
[0041] The plasticizer is glycerol fatty acid ester.
[0042] The compatibilizer is ethylene-vinyl acetate copolymer; The photosensitizer is dialkoxyacetophenone.
[0043] A method for preparing a biodegradable polyethylene composite material in a natural environment comprises the following steps: a. uniformly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and melt mix it at a temperature of 160°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product. Example 3
[0044] A biodegradable polyethylene composite material in a natural environment, comprising the following components by weight:
[0045] Among them, the molecular weight of high-density polyethylene is 100,000.
[0046] The biodegradable aid is a modified starch / polylactic acid complex.
[0047] The preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep warm and stir for 10 minutes to obtain a mixed solution; the mixing ratio of the pretreated starch and dimethyl sulfoxide is 32g:100mL; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL:1g:10g; Vacuum to 0.1Pa; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
[0048] The method for preparing pretreated starch is as follows: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
[0049] The plasticizer is glycerol fatty acid ester.
[0050] The compatibilizer is ethylene-vinyl acetate copolymer; The photosensitizer is dialkoxyacetophenone.
[0051] A method for preparing a biodegradable polyethylene composite material in a natural environment comprises the following steps: a. Evenly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and perform melt mixing at a temperature of 160°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product. Example 4
[0052] A biodegradable polyethylene composite material in a natural environment, comprising the following components by weight:
[0053] Among them, the molecular weight of high-density polyethylene is 100,000.
[0054] The biodegradable aid is a modified starch / polylactic acid complex.
[0055] The preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep warm and stir for 10 minutes to obtain a mixed solution; the mixing ratio of the pretreated starch and dimethyl sulfoxide is 32g:100mL; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL:1g:10g; Vacuum to 0.1Pa; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
[0056] The preparation method of pretreated starch is as follows: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
[0057] The plasticizer is glycerol fatty acid ester.
[0058] The compatibilizer is ethylene-vinyl acetate copolymer; The photosensitizer is dialkoxyacetophenone.
[0059] A method for preparing a biodegradable polyethylene composite material in a natural environment comprises the following steps: a. Evenly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and melt mix it at a temperature of 160°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product. Example 5
[0060] A biodegradable polyethylene composite material in a natural environment, comprising the following components by weight:
[0061] Among them, the molecular weight of high-density polyethylene is 100,000.
[0062] The biodegradable aid is a modified starch / polylactic acid complex.
[0063] The preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep warm and stir for 10 minutes to obtain a mixed solution; the mixing ratio of the pretreated starch and dimethyl sulfoxide is 32g:100mL; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL:1g:10g; Vacuum to 0.1Pa; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
[0064] The preparation method of pretreated starch is as follows: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
[0065] The plasticizer is glycerol fatty acid ester.
[0066] The compatibilizer is ethylene-vinyl acetate copolymer; The photosensitizer is dialkoxyacetophenone.
[0067] A method for preparing a biodegradable polyethylene composite material in a natural environment comprises the following steps: a. Evenly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and perform melt mixing at a temperature of 160°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product.
[0068] The basic physical and chemical properties of the samples in Example 1 were tested, see Table 1: Table 1
[0069] After testing, the test results of the samples in Example 1 all met the standard requirements.
[0070] Test items: heavy metal content, halogen General requirements for disposable biodegradable tableware: CB / T18006.3-2020 The heavy metal content of the sample in Example 1 was tested; Use method GB / T37837-20191, analyzed by ICP-MS, see Table 2: Table 2
[0071] It can be seen from Table 2 that the polyethylene composite material prepared by the present invention does not contain heavy metals.
[0072] Halogen detection was performed on the sample of Example 1, see Table 3: Test method CB / T18006.3-2020 Table 3
[0073] After testing, the sample of the embodiment is halogen-free, safe and reliable.
[0074] Test items: Degradation performance test: The degradation performance test of the sample in Example 1 was carried out according to the GB / T1922.1-2011 standard: The reference material (positive reference) was subjected to the same degradation test. The reference material used was microcrystalline cellulose, which was sourced from Sinopharm Chemical Reagent Co., Ltd., with molecular formula: (C6H10O5)n, molecular weight (162.14)n, CAS No. 9004-34-6; shape: white or off-white powder; The test was conducted at a constant temperature of 58°C ± 2°C, weak light, and without any conditions that would affect the growth of microorganisms; The inoculum was aerobic compost with an organic matter content of 45%, item number 067, grade a, from Shijiazhuang Gaoyuan Fertilizer Co., Ltd.; Draw a time-biodegradation percentage curve of the sample in Example 1 and the positive reference, as shown in Figure 1 , indicating that the sample in Example 1 has higher biodegradability.
[0075] From day 1 to day 147, the biodegradation status of the sample of Example 1 and the positive reference was detected and recorded every day as shown in Tables 4 to 18; Table 4 1-10 days biodegradation status table
[0076] Table 5 11-20 days biodegradation status table
[0077] Table 6 21-30 days biodegradation status
[0078] Table 7 31-40 days biodegradation status
[0079] Table 8 41-50 days biodegradation status
[0080] Table 9 51-60 days biodegradation status
[0081] Table 10 61-70 days biodegradation status
[0082] Table 11 71-80 days biodegradation status
[0083] Table 12 81-90 days biodegradation status
[0084] Table 13 91-100 days biodegradation status
[0085] Table 14 101-110 days biodegradation status
[0086] Table 15 111-120 days biodegradation status
[0087] Table 16 121-130 days biodegradation status
[0088] Table 17 131-140 days biodegradation status
[0089] Table 18 141-147 days biodegradation status
[0090] It can be seen from Tables 4 to 18 that the polyethylene composite material prepared in the present invention has excellent degradation performance.
[0091] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A biodegradable polyethylene composite material in a natural environment, characterized in that: It is composed of the following components by weight: High density polyethylene: 85-95 parts; Biodegradable additives: 5-10 parts; Plasticizer: 0.1-3 parts; Compatibilizer: 0.2-5 parts; Photosensitizer: 0.01-1 part; Among them, the molecular weight of high-density polyethylene is 100,000.
2. The biodegradable polyethylene composite material in natural environment according to claim 1, characterized in that: The biodegradation aid is a modified starch / polylactic acid complex.
3. The biodegradable polyethylene composite material in natural environment according to claim 2, characterized in that: The preparation method of the modified starch / polylactic acid composite comprises the following steps: (1) pretreating starch to obtain pretreated starch; (2) Add the pretreated starch and dimethyl sulfoxide to the reactor in sequence, then adjust the temperature to 75°C, keep the mixture warm and stir for 10 minutes to obtain a mixed solution; (3) adding a catalyst and lactide to the mixed solution in the reaction kettle, evacuating the reaction kettle, adjusting the temperature to 80° C., and carrying out a heat preservation reaction for 4 hours to obtain a reaction mixture; (4) diluting the reaction mixture with ethanol to 3 times of the original volume, then adding 5 times of the original volume of distilled water to precipitate, filter, and dry to obtain a modified starch / polylactic acid composite; The drying temperature was 60°C and the drying time was 1 hour.
4. The biodegradable polyethylene composite material in natural environment according to claim 3, characterized in that: The method for preparing the pretreated starch is as follows: First, starch was added into a reactor, and then distilled water was added into the reactor, and the mixture was stirred at a speed of 500 r / min for 30 min to obtain a starch emulsion; Adjusting the pH of the starch emulsion to 3.5; Then adjust the temperature to 75°C and stir for 30 min; Then, a sodium sulfite solution is added to the starch emulsion, and the mixture is stirred for 2 hours under heat preservation, and then the pH of the reaction system is adjusted to neutral, and the mixture is filtered and dried to obtain pretreated starch; The drying temperature was 55°C and the drying time was 2 hours.
5. The biodegradable polyethylene composite material in natural environment according to claim 4, characterized in that: The starch is soybean starch; The starch mass fraction in the starch emulsion is 30-35%; The starch emulsion is adjusted to pH 3.5 by using a 5% by mass hydrochloric acid aqueous solution; The mixing mass ratio of starch emulsion and sodium sulfite solution is 10:1-1.6; The concentration of the sodium sulfite solution is 1 mol / L; The pH of the reaction system was adjusted to neutral by using a 5% by mass sodium hydroxide solution.
6. The biodegradable polyethylene composite material in natural environment according to claim 3, characterized in that: The mixing ratio of the pretreated starch and dimethyl sulfoxide in step (2) is 32-35 g:100 mL.
7. The biodegradable polyethylene composite material in natural environment according to claim 3, characterized in that: In step (3), the catalyst is trifluoromethanesulfonic acid; The mixing ratio of the mixed liquid, catalyst and lactide is 100mL: 1-1.2g: 10-13g; Evacuate to 0.1Pa.
8. The biodegradable polyethylene composite material in natural environment according to claim 1, characterized in that: The plasticizer is glycerol fatty acid ester.
9. The biodegradable polyethylene composite material in natural environment according to claim 1, characterized in that: The compatibilizer is ethylene-vinyl acetate copolymer or maleic anhydride grafted polyethylene; The photosensitizer is dialkoxyacetophenone.
10. The method for preparing a biodegradable polyethylene composite material in a natural environment according to claim 1, characterized in that: The following steps are involved: a. Evenly mixing high-density polyethylene, biodegradation aid, compatibilizer, plasticizer and photosensitizer according to the weight parts of each component to obtain a mixed material; b. Add the mixed material into the extruder and perform melt mixing at a temperature of 160°C; c. Extruding the molten mixture through a die to obtain a sheet of desired thickness; d. Cooling and shaping the extruded sheet at room temperature; e. Cut the cooled sheet to obtain the final product.
Citation Information
Cited By
Degradable environment-friendly material cosmetic packaging bottle and preparation method thereof
CN119410051A
Biodegradable polyethylene composite material and preparation method thereof
CN120248465A