Rubber sleeve for charging roller and preparation method thereof

By introducing conductive carbon black and acid absorbers into the charging roller rubber to form a conductive network, combined with vulcanizing agents and accelerators, the problem of acidic substances affecting rubber properties is solved, and the heat resistance and aging resistance of the rubber are improved.

CN118725470APending Publication Date: 2024-10-01HENAN GREEN EXPRESS RUBBER &PLASTIC PROD CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410982495.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The acidic substances generated during the production process of the existing charging roller rubber affect its mechanical properties and heat resistance, leading to performance degradation.

Method used

EPDM rubber and methyl vinyl silicone rubber are blended, and conductive carbon black, acid absorbing agents such as ethanolamine and zeolite powder, accelerators and vulcanizing agents are introduced to form a conductive network and a three-dimensional network structure to neutralize or absorb acid. Substance to improve cross-linking density and vulcanization effect.

Benefits of technology

It significantly improves the heat resistance, aging resistance and mechanical properties of the rubber casing, reduces the damage of acidic substances to the rubber molecular chain, and enhances its anti-aging and anti-wear properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956490740000071
    Figure BDA0004956490740000071
  • Figure BDA0004956490740000081
    Figure BDA0004956490740000081
Patent Text Reader

Abstract

The invention discloses a rubber sleeve for a charging roller and a preparation method of the rubber sleeve, and relates to the technical field of charging rollers. The rubber sleeve is prepared from the following raw materials in parts by weight: 60-80 parts of ethylene propylene diene monomer, 20-40 parts of methyl vinyl silicone rubber, 8-12 parts of conductive carbon black, 1-3 parts of a vulcanizing agent, 1-2 parts of an accelerant, 2-4 parts of an active agent, 30-50 parts of a reinforcing agent and 10-20 parts of an acid acceptor, the acid acceptor is at least one of ethanolamine and zeolite powder. The prepared rubber sleeve can neutralize acidic substances in the rubber production process, reduce the damage of the acidic substances to rubber molecular chains, improve the crosslinking density of rubber to a certain extent, and enhance the mechanical properties and aging resistance of the rubber sleeve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of charging rollers, and in particular to a rubber sleeve for a charging roller and a preparation method thereof. Background Art

[0002] The charging roller is a key component in the printer. Its main function is to conduct static electricity to the photosensitive drum so that the photosensitive drum can absorb toner. Through the function of the charging roller, the printer can realize the function of converting electronic files into paper files. The charging roller is composed of a metal core and a conductive rubber coated on the metal core. Vulcanization is a necessary process in the manufacturing process of rubber products and a unique process in rubber processing. Rubber obtains the necessary physical, mechanical and chemical properties through vulcanization.

[0003] The Chinese invention patent with application publication number CN107118450A discloses a rubber foam hose composition for a charging roller with high elasticity and uniform pore size, which includes the following components by weight: 10 to 50 parts of ultra-fast vulcanized EPDM rubber, 10 to 50 parts of high-elasticity EPDM rubber, 12 to 35 parts of filler, 2 to 10 parts of conductive agent, 10 to 25 parts of plasticizer, 1 to 4 parts of foaming agent, 3 to 6 parts of vulcanizing agent and vulcanizing aid, 1 to 3 parts of stearic acid, 4 to 7 parts of zinc oxide, 1 to 5 parts of antioxidant, 1 to 3 parts of deodorant, and 3 to 5 parts of dehumidifier.

[0004] In the prior art, acidic substances are produced during the production process of rubber, which can reduce the molecular weight of the rubber and affect its mechanical properties and heat resistance. Summary of the invention

[0005] In order to reduce the influence of acidic substances on rubber properties, the present application provides a rubber sleeve for a charging roller and a preparation method thereof.

[0006] The present application provides a method for preparing a rubber sleeve for a charging roller, which adopts the following technical solution: A rubber sleeve for a charging roller is made of the following raw materials in parts by weight: 60-80 parts of EPDM rubber, 20-40 parts of methyl vinyl silicone rubber, 8-12 parts of conductive carbon black, 1-3 parts of vulcanizer, 1-2 parts of accelerator, 2-4 parts of activator, 30-50 parts of reinforcing agent and 10-20 parts of acid absorber; the acid absorber is at least one of ethanolamine and zeolite powder.

[0007] By adopting the above technical solution, after EPDM rubber and methyl vinyl silicone rubber are blended, the crosslinking density becomes larger, which can further improve the heat resistance and aging resistance of EPDM rubber. The surface of conductive carbon black has a strong adsorption capacity, which can adsorb the end or side group of rubber molecules to form a physical adsorption layer. This physical adsorption layer can increase the affinity between carbon black and rubber, and help to form a continuous conductive network. The acid absorber can effectively neutralize or adsorb the acidic substances generated by EPDM rubber and methyl vinyl silicone rubber during the vulcanization process, and can promote the decomposition of peroxides to produce free radicals, enhance the crosslinking efficiency, and thus reduce the damage of acidic substances to the rubber polymer molecular chain.

[0008] At a certain temperature, ethanolamine can also combine with the functional groups on the rubber molecular chain to enhance the crosslinking density of the rubber and improve the heat resistance of the rubber; while the zeolite powder reacts with the vulcanizing agent to form a compound, which accelerates the vulcanization reaction of the rubber and improves the vulcanization effect. Since there are residual hydroxyl groups on the surface of the zeolite powder, there are reactive centers on its surface, which can physically or chemically combine with the silicon oxygen bonds in the silicon skeleton structure of the rubber, forming a silicone rubber molecule adsorption layer on the surface of the zeolite powder, forming a three-dimensional network structure in which the zeolite powder particles and the silicone rubber molecules are integrated, effectively limiting the deformation of the silicone rubber molecular chain, thereby achieving a reinforcing effect.

[0009] Preferably, the acid absorber is a mixture of ethanolamine and zeolite powder, and the mass ratio of the ethanolamine to the zeolite powder is 3-5:1-3.

[0010] By adopting the above technical solution, the type and ratio of the acid absorber are optimized, and the influence of acidic substances on the vulcanization reaction is reduced. Among them, zeolite powder has a good adsorption effect on the amino group in ethanolamine, making the ethanolamine more evenly dispersed. The zeolite powder and ethanolamine are used in synergy, thereby improving the adsorption rate of acidic substances.

[0011] Preferably, the acid absorber further comprises diethylethanolammonium chloride, and the mass ratio of the ethanolamine, zeolite powder and diethylethanolammonium chloride is 3-5:1-3:1-3.

[0012] By adopting the above technical solution, diethyl ethanol ammonium chloride can neutralize part of the acidic substances and further remove the acidic substances in the rubber. Under certain temperature conditions, diethyl ethanol ammonium chloride can also combine with the functional groups on the rubber molecular chain to enhance the heat resistance of the rubber.

[0013] Preferably, the vulcanizing agent is at least one of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

[0014] By adopting the above technical solution, the rubber molecular chain is prompted to undergo a cross-linking reaction to form a three-dimensional network structure, thereby changing the rubber from a linear type to a three-dimensional network structure, reducing its plasticity and increasing its elastic strength. When diisopropylbenzene peroxide and 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane are used together, the vulcanization speed can be increased.

[0015] Preferably, the vulcanizing agent comprises dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane, and the mass ratio of dicumyl peroxide to 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane is 0.1-0.2:0.4-0.6.

[0016] Preferably, the accelerator includes thiazoles and guanidines; the mass ratio of the thiazoles to the guanidines is 1:0.5-0.7; the thiazoles include dibenzothiazyl disulfide and 2-mercaptobenzothiazole; and the guanidine is diphenylguanidine.

[0017] By adopting the above technical scheme, the use of thiazole accelerators and guanidine weak accelerators can improve the activity of the accelerators, shorten the vulcanization time and reduce the vulcanization temperature, while improving the tensile strength, elongation and wear resistance of the vulcanized rubber.

[0018] Preferably, the reinforcing agent is at least one of silicon carbide, boron nitride, calcium carbonate and carbon black.

[0019] By adopting the above technical solution, the filling of the reinforcing agent in the rubber will not cause obvious internal stress in the rubber body. The reinforcing agent plays a bridge role in connecting the molecular chains of the rubber. The strong mechanical action of rubber refining can also force the reinforcing agent particles to be wrapped by the rubber molecular chains, and the stress transmission ability of the reinforcing agent can be fully exerted.

[0020] Preferably, the active agent includes zinc oxide and stearic acid, and the mass ratio of zinc oxide to stearic acid is 6-8:1-3.

[0021] By adopting the above technical solution, stearic acid has an activation effect, and plays an acidic activation role on the double bonds of rubber molecules, thereby accelerating the formation of cross-linking bonds and increasing the cross-linking density of rubber. Stearic acid can form a soluble salt with zinc oxide, increasing the activation ability of metal zinc oxide on the accelerator. In addition, stearic acid can also improve the dispersibility of zinc oxide and conductive carbon black in rubber.

[0022] Preferably, the raw materials further include 3 to 5 parts by weight of maleic anhydride.

[0023] By adopting the above technical scheme, the effect of maleic anhydride polar groups reduces the oxidation activity of rubber, reduces the ability to generate free radicals under the action of oxygen, reduces the auto-catalytic free radical chain reaction during the oxidation process, reduces the performance change of the blend after aging, and improves the aging resistance.

[0024] Preferably, the raw materials also include 6 to 8 parts by weight of magnesium hydroxide.

[0025] Preferably, the raw material further comprises 15 to 20 parts by weight of silicon powder.

[0026] By adopting the above technical solution, silicon powder can effectively absorb a number of functional groups on the surface of conductive carbon black, and can react with the hydroxyl, carbonyl and carboxyl groups on the surface of conductive carbon black, while binding these functional groups, thereby preventing these functional groups from coming into contact with oxygen in the air and scattering in the sunlight to form the risk of flooding.

[0027] Preferably, the raw materials further include 6 to 8 parts by weight of barium sulfate.

[0028] The present application also provides a method for preparing a rubber sleeve for a charging roller.

[0029] Preferably, the method for preparing the rubber sleeve for the charging roller comprises the following steps: S1: EPDM rubber, methyl vinyl silicone rubber, conductive carbon black, activator, reinforcing agent and part of acid absorbent are mixed to obtain a primary rubber compound; S2: The primary rubber compound, the accelerator, the vulcanizing agent and another part of the acid absorbent are mixed to obtain a secondary rubber compound; S3: Install the corresponding mold according to the specifications, and extrude the secondary rubber material to obtain the primary rubber sleeve; S4: vulcanizing the primary rubber sleeve to obtain the rubber sleeve.

[0030] In summary, the present application includes at least one of the following beneficial technical effects: 1. By introducing acid absorbents such as ethanolamine, zeolite powder and diethylethanol ammonium chloride, the acidic substances in rubber and rubber production process can be adsorbed and neutralized, and the cross-linking density of rubber can be increased to a certain extent, thereby enhancing the mechanical properties and anti-aging properties of rubber casing.

[0031] 2. With the help of maleic anhydride, the performance change of the blend after aging is reduced and the anti-aging performance of the rubber casing is improved. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] The embodiment of the rubber sleeve for the charging roller of the present application is as follows: Example 1 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 60kg of EPDM rubber, 40kg of methyl vinyl silicone rubber, 8kg of conductive carbon black, 1kg of dicumyl peroxide, 0.34kg of dibenzothiazole disulfide, 0.33kg of 2-mercaptobenzothiazole, 0.33kg of diphenylguanidine, 1.33kg of zinc oxide, 0.67kg of stearic acid, 30kg of carbon black, and 10kg of ethanolamine.

[0034] The method for preparing the rubber sleeve for the charging roller of this embodiment comprises the following steps: S1: Add EPDM rubber, methyl vinyl silicone rubber, conductive carbon black, activator, reinforcing agent, and one-third of acid absorbent into an internal mixer, and mix at 150°C for 15 minutes to obtain a primary rubber compound; S2: The primary rubber material is transported to an open mixing mill, and then an accelerator, a vulcanizing agent, and two-thirds of an acid absorber are added and mixed for 15 minutes to obtain a secondary rubber material; S3: Install the corresponding mold according to the specifications, set the working temperature of each section of the extruder to 60°C, add the secondary rubber material into the extruder and extrude it to obtain the primary rubber sleeve; S4: The primary rubber sleeve is continuously transported to the tunnel air vulcanization furnace for vulcanization. The vulcanization temperature is 220°C and the vulcanization speed is 8m / min.

[0035] Among them, the unsaturation degree of EPDM rubber is about 0.45-0.55 mol / kg.

[0036] Example 2 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 80kg of EPDM rubber, 20kg of methyl vinyl silicone rubber, 12kg of conductive carbon black, 3kg of diisopropylbenzene peroxide, 0.67kg of dibenzothiazole disulfide, 0.67kg of 2-mercaptobenzothiazole, 0.66kg of diphenylguanidine, 2.66kg of zinc oxide, 1.34kg of stearic acid, 50kg of carbon black, and 20kg of ethanolamine.

[0037] The rest is the same as in Example 1.

[0038] Example 3 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 2kg of diisopropylbenzene peroxide, 0.5kg of dibenzothiazole disulfide, 0.5kg of 2-mercaptobenzothiazole, 0.5kg of diphenylguanidine, 2kg of zinc oxide, 1kg of stearic acid, 40kg of carbon black, and 15kg of ethanolamine.

[0039] The rest is the same as in Example 1.

[0040] Example 4 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 0.3kg of diisopropylbenzene peroxide, 1.7kg of 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.44kg of dibenzothiazole disulfide, 0.44kg of 2-mercaptobenzothiazole, 0.62kg of diphenylguanidine, 2.67kg of zinc oxide, 0.33kg of stearic acid, 30kg of carbon black, 10kg of silicon carbide, and 15kg of zeolite powder.

[0041] The rest is the same as in Example 1.

[0042] Example 5 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 0.29kg of diisopropylbenzene peroxide, 1.71kg of 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.44kg of dibenzothiazole disulfide, 0.44kg of 2-mercaptobenzothiazole, 0.62kg of diphenylguanidine, 2.6kg of zinc oxide, 0.4kg of stearic acid, 30kg of carbon black, 10kg of silicon carbide, 7.5kg of zeolite powder, and 7.5kg of ethanolamine.

[0043] The rest is the same as in Example 1.

[0044] Example 6 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 0.67kg of diisopropylbenzene peroxide, 1.33kg of 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.47kg of dibenzothiazole disulfide, 0.47kg of 2-mercaptobenzothiazole, 0.56kg of diphenylguanidine, 2.33kg of zinc oxide, 0.67kg of stearic acid, 20kg of carbon black, 10kg of silicon carbide, 10kg of calcium carbonate, 12.5kg of zeolite powder, and 2.5kg of ethanolamine.

[0045] The rest is the same as in Example 1.

[0046] Example 7 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 0.46kg of diisopropylbenzene peroxide, 1.54kg of 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.47kg of dibenzothiazole disulfide, 0.47kg of 2-mercaptobenzothiazole, 0.56kg of diphenylguanidine, 2.33kg of zinc oxide, 0.67kg of stearic acid, 20kg of carbon black, 10kg of silicon carbide, 10kg of calcium carbonate, 10kg of zeolite powder, 5kg of ethanolamine, 6kg of magnesium hydroxide, 15kg of silicon powder, and 6kg of barium sulfate.

[0047] S1 also includes the step of adding magnesium hydroxide, silicon powder and barium sulfate.

[0048] The rest is the same as Example 6.

[0049] Example 8 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 0.46kg of diisopropylbenzene peroxide, 1.54kg of 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.47kg of dibenzothiazole disulfide, 0.47kg of 2-mercaptobenzothiazole, 0.56kg of diphenylguanidine, 2.33kg of zinc oxide, 0.67kg of stearic acid, 10kg of carbon black, 10kg of silicon carbide, 10kg of calcium carbonate, 10kg of boron nitride, 8.6kg of zeolite powder, 4.3kg of ethanolamine, 2.1kg of diethylethanolammonium chloride, 8kg of magnesium hydroxide, 20kg of silicon powder, and 8kg of barium sulfate.

[0050] The rest is the same as Example 7.

[0051] Example 9 The present embodiment provides a rubber sleeve for a charging roller, which is mainly made of the following raw materials by weight: 70kg of EPDM rubber, 30kg of methyl vinyl silicone rubber, 10kg of conductive carbon black, 0.46kg of diisopropylbenzene peroxide, 1.54kg of 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.47kg of dibenzothiazole disulfide, 0.47kg of 2-mercaptobenzothiazole, 0.56kg of diphenylguanidine, 2.33kg of zinc oxide, 0.67kg of stearic acid, 10kg of carbon black, 20kg of silicon carbide, 10kg of calcium carbonate, 6.7kg of zeolite powder, 3.3kg of ethanolamine, 5kg of diethylethanolammonium chloride, 7kg of magnesium hydroxide, 18kg of silicon powder, and 7kg of barium sulfate.

[0052] The rest is the same as Example 8.

[0053] Example 10 The difference between this embodiment and embodiment 9 is that the amount of zeolite powder used is 7.4 kg, the amount of ethanolamine used is 3.8 kg, and the amount of diethylethanolammonium chloride used is 3.8 kg.

[0054] The rest is the same as Example 9.

[0055] Embodiment 11 The difference between this embodiment and embodiment 10 is that 3 kg of maleic anhydride is also added to the raw material.

[0056] S1 also includes a step of adding maleic anhydride.

[0057] The rest is the same as Example 10.

[0058] Example 12 The difference between this embodiment and Example 11 is that the amount of maleic anhydride used is 4 kg.

[0059] The rest is the same as Example 11.

[0060] Embodiment 13 The difference between this embodiment and embodiment 12 is that the amount of maleic anhydride used is 5 kg.

[0061] The rest is the same as Example 12.

[0062] Comparative Example 1 The difference between this comparative example and Example 1 is that no zeolite powder, ethanolamine or diethylethanolammonium chloride is added.

[0063] The rest is the same as in Example 1.

[0064] Performance Testing (1) The tensile strength and elongation at break of the samples in Examples 1 to 10 and Comparative Example 1 were tested using an electronic tensile testing machine in accordance with the requirements of GB / T5282009.

[0065] (2) Heat Air Aging Resistance Test According to the requirements of GB / T35122014, the rubber sleeves for charging rollers in Examples 1-10 and Comparative Example 1 were placed in an aging oven for testing at 150° C. for 70 h, and then a secondary test was performed using an electronic tensile testing machine.

[0066] (3) Adhesion and corrosion resistance The samples in Examples 1-10 and Comparative Example 1 were tested according to the requirements of GB / T 14834-2009. The test conditions were 40° C., 50% relative humidity, and 240 h. The appearance was inspected with a magnifying glass to determine the degree of adhesion to the metal surface and the degree of corrosion.

[0067] Table 1 Comparison of the performance of the rubber sleeve for the charging roller in Examples 1-10 and Comparative Example 1 By analyzing the experimental data of Example 10 and Comparative Example 1, it can be seen that the addition of the acid absorber increases the tensile strength and elongation at break of the rubber tube for the charging roller, and the corrosion to the metal core of the charging roller is greatly improved.

[0068] By comparing and analyzing the experimental data of Examples 1-3, it can be seen that with different acid absorption dosages, the tensile strength and elongation at break show a trend of first increasing and then decreasing.

[0069] Comparative analysis of the experimental data of Examples 3-10 shows that by optimizing the type and ratio of the acid absorber, the retention rates of tensile strength and elongation at break before and after aging are significantly improved, and the adhesion and corrosion properties to the metal core of the charging roller are maintained within a good range.

[0070] Comparative analysis of the experimental data of implementation forces 10-13 shows that, on the one hand, the polarity of maleic anhydride may increase the grafting rate of EPDM rubber; on the other hand, maleic anhydride reduces the oxidation activity of rubber, reduces the ability to generate free radicals under the action of oxygen, and reduces the auto-catalytic free radical chain reaction during the oxidation process, which reduces the performance changes of the blend after aging and improves the aging resistance.

Claims

1. A rubber sleeve for a charging roller, characterized in that: The rubber sleeve is made of the following raw materials in parts by weight: 60-80 parts of EPDM rubber, 20-40 parts of methyl vinyl silicone rubber, 8-12 parts of conductive carbon black, 1-3 parts of vulcanizer, 1-2 parts of accelerator, 2-4 parts of activator, 30-50 parts of reinforcing agent and 10-20 parts of acid absorber; the acid absorber is at least one of ethanolamine and zeolite powder.

2. The rubber sleeve for the charging roller according to claim 1, characterized in that: The acid absorber comprises ethanolamine and zeolite powder, and the mass ratio of the ethanolamine to the zeolite powder is 3-5:1-3.

3. The rubber sleeve for the charging roller according to claim 2, characterized in that: The acid absorber further comprises diethylethanol ammonium chloride, and the mass ratio of the ethanolamine, the zeolite powder and the diethylethanol ammonium chloride is 3-5:1-3:1-3.

4. The rubber sleeve for the charging roller according to claim 3, characterized in that: The vulcanizing agent is at least one of dicumyl peroxide and 2,5-dimethyl-2,5-di(tert-butyl peroxide)hexane.

5. The rubber sleeve for the charging roller according to claim 4, characterized in that: The accelerators include thiazoles and guanidines; the mass ratio of the thiazoles to the guanidines is 1:0.5-0.7; the thiazoles include dibenzothiazyl disulfide and 2-mercaptobenzothiazole; and the guanidines are diphenylguanidine.

6. The rubber sleeve for the charging roller according to claim 5, characterized in that: The reinforcing agent is at least one of silicon carbide, boron nitride, calcium carbonate and carbon black.

7. The rubber sleeve for the charging roller according to claim 6, characterized in that: The active agent includes zinc oxide and stearic acid, and the mass ratio of the zinc oxide to the stearic acid is 6-8:1-3.

8. The rubber sleeve for the charging roller according to claim 7, characterized in that: The raw materials also include 3 to 5 parts by weight of maleic anhydride.

9. A method for preparing the rubber sleeve for a charging roller as claimed in any one of claims 1 to 7.

10. The method for preparing the rubber sleeve for the charging roller according to claim 9, characterized in that: The steps include: S1: EPDM rubber, methyl vinyl silicone rubber, conductive carbon black, activator, reinforcing agent and part of acid absorbent are mixed to obtain a primary rubber compound; S2: The primary rubber compound, the accelerator, the vulcanizing agent and another part of the acid absorbent are mixed to obtain a secondary rubber compound; S3: Install the corresponding mold according to the specifications, and extrude the secondary rubber material to obtain the primary rubber sleeve; S4: vulcanizing the primary rubber sleeve to obtain the rubber sleeve.

Citation Information

Patent Citations

  • High-elasticity and uniform-cell size foamed rubber hose composition for charging roller and preparation method of foamed rubber hose composition

    CN107118450A