A high-strength flame-retardant composite material for reducer and preparation method thereof
By adding alkylphosphinates, nanodiatomaceous earth and graphene to nylon materials, a flame retardant system of phosphorus-silicon-carbon is formed, which solves the problem of low flame retardant performance of nylon materials and realizes high temperature High-efficiency flame retardant and mechanical performance improvement in the environment.
Patent Information
- Application Number
- CN202411197550.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-29
AI Technical Summary
Nylon materials have low flame retardant properties and poor fire resistance, which limits their application in high temperature environments, especially in manufacturing.
Using a high-strength flame retardant composite material, including nylon 12T, fiber reinforced filler, alkyl phosphinate, nanodiatomaceous earth, pentaerythritol and graphene, the method is prepared through the twin-screw extrusion mechanism to form phosphorus- Silicon-carbon flame retardant system improves flame retardant performance and mechanical properties.
It significantly improves the flame retardant performance of nylon materials, combines excellent processing and mechanical properties, and can effectively prevent combustion and flue gas diffusion in high temperature environments, meeting the requirements of mechanical equipment such as reducers.
Smart Images

Figure JRUJQUCEFGNQFYW9TXS1UEQUNCUWSUBGXWMPWSUX 
Figure ZQCURX0OF5IY9PLZNKMQBEWFEXMWWVGEPR84CICL
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a high-strength flame-retardant composite material for a reducer and a preparation method thereof. Background Art
[0002] High-strength flame-retardant plastics are not only an important basic industry of the national economy, but also an important pillar of the future manufacturing industry and a key area for obtaining technological competitive advantages. In recent years, with the rapid development of the manufacturing industry, the pace of product upgrading has been accelerating, and intelligence, new materials and new processes have jointly promoted the continuous development of the plastics industry. Plastics account for about 40% of the production of parts, which shows that high-strength flame-retardant plastics are key materials in the modern manufacturing process.
[0003] Polyamide, commonly known as nylon, is a general term for polymers that contain amide groups in the repeating structure of the macromolecular main chain and can form a certain density of hydrogen bonds. Initially, nylon was only used as a raw material for making fibers. Later, with the development of processing technology, and the advantages of nylon itself such as toughness, wear resistance, good self-lubrication, and a wide operating temperature range, its use in the fields of automobiles, electronics, sports goods, machinery, packaging, etc. has increased year by year, and it occupies an important position in engineering plastics.
[0004] Nylon can replace copper and nonferrous metals in some fields to make mechanical, chemical and electrical parts, such as reducer pump gears, high-pressure seals, plastic pipes, etc. In the 1950s, people began to use nylon in reducer peripheral parts to replace metal to meet the requirements of lightweight mechanical equipment and reduce costs.
[0005] Aliphatic polyamides are widely used in all aspects of life due to their advantages such as fast crystallization rate, high crystallinity and excellent mechanical properties. However, their heat resistance is generally not high and they cannot be used under high temperature conditions for a long time, which also limits their application. Fully aromatic polyamides have good high and low temperature resistance and are mainly used in high-tech fields such as bulletproof vests, aerospace, and atomic energy industry. Semi-aromatic polyamides, such as nylon 12T, make up for the shortcomings of insufficient heat resistance of aliphatic polyamides to a certain extent. They are heat-resistant polyamides and have better processing performance than fully aromatic nylon. They are mainly widely used in the field of mechanical equipment. Although nylon has good comprehensive properties, its flame retardant properties are low and there is a technical problem of poor fire resistance. Limited by its molecular structure, nylon is easy to burn and is accompanied by melt droplets and thick smoke when burning, and cannot be self-extinguished away from the fire. In recent years, with the continuous improvement of people's requirements for fire safety and environmental protection, the flame retardant research of nylon has become increasingly urgent. Summary of the invention
[0006] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to provide a high-strength flame-retardant composite material for a reducer and a preparation method thereof. The composite material significantly improves the flame retardant properties of nylon materials and has excellent processing properties and mechanical properties. It can be used to manufacture related accessories in the field of machinery such as reducers, and meet the high-strength and flame-retardant technical requirements of its use environment.
[0007] In order to achieve the above object, the first aspect of the present invention discloses a high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0008] 60-70 parts of nylon 12T, 20-30 parts of fiber-reinforced filler, 10-15 parts of alkyl phosphinate, 4-8 parts of nano-diatomaceous earth, 2-4 parts of pentaerythritol, 4-10 parts of graphene, 1-3 parts of coupling agent, and 1-3 parts of flow modifier.
[0009] The present invention selects nylon 12T as the base resin. Nylon 12T is formed by high-temperature and high-compression polymerization of monomers of dodecyl diamine and terephthalic acid, can be formed by injection molding or extrusion molding, and has good high temperature resistance and dimensional stability. The ultra-long flexible chain in the monomer dodecyl diamine reduces the amide bond density of nylon 12T, which not only reduces the water absorption rate of nylon 12T, but also gives nylon 12T a certain toughness, and the impact resistance is also very good, which can meet the use requirements of mechanical equipment in harsh environments.
[0010] Further, the fiber-reinforced filler is one or more of glass fiber, carbon fiber, and whisker fiber. The cross section of the glass fiber can be in various forms, such as circular, elliptical, rectangular or other special shapes, preferably glass fiber with circular and rectangular cross sections. The carbon fiber can be one or more of asphalt-based carbon fiber, polyacrylonitrile-based carbon fiber, and viscose-based carbon fiber. The whisker can be one or more of potassium titanate whisker, zinc oxide whisker, calcium sulfate whisker, aluminum borate whisker, basic magnesium sulfate whisker, and calcium carbonate whisker.
[0011] In order to improve the flame retardant effect of nylon 12T, the present invention adds a certain amount of alkyl phosphinate flame retardant. Alkyl phosphinate has a high percentage of phosphorus, does not contain phosphorus-oxygen groups, has excellent hydrolysis stability and flame retardancy, and the presence of cations can prevent the volatilization loss of flame retardants and pollute the environment. At the same time, the salts of these cations have a good smoke suppression effect. However, the flame retardant effect of a single alkyl phosphinate is limited, and there is a technical problem that it is easy to precipitate in nylon. For this reason, the present invention adds a certain amount of nano diatomaceous earth and pentaerythritol. Diatomaceous earth mainly contains silicon oxide, and a certain amount of metal oxides such as magnesium oxide and aluminum oxide. It has the characteristics of light texture, many pores, strong water absorption, and high chemical stability. It can not only be used as a flame retardant synergist of alkyl phosphinate, but also can effectively improve thermal stability and residual rate. In order to improve the dispersibility of alkyl phosphinate flame retardant and nano diatomaceous earth, the present invention also adds a certain amount of pentaerythritol. Pentaerythritol not only acts as a dispersant, but also is an excellent carbon-forming agent. It can form a phosphorus-silicon-carbon flame retardant system with alkyl phosphinate and diatomite to improve the flame retardant effect. In high-temperature nylon materials, with the effect of high temperature during mechanical processing, alkyl phosphinate flame retardants and pentaerythritol are very likely to precipitate on the surface. Diatomite has excellent adsorption properties, which can improve the dispersion properties of alkyl phosphinate flame retardants and pentaerythritol, prevent the precipitation of alkyl phosphinate flame retardants and pentaerythritol during processing, and improve the surface performance of the product. In addition, diatomite can absorb or hinder the release of combustible gases during combustion, slowing down the spread of flames and the diffusion of smoke.
[0012] Graphene can play a role in heat conduction and flame retardancy. The addition of graphene makes the distance between fillers lower and has a higher interface area, which promotes the formation of a dense carbon layer. Since graphene has excellent thermal conductivity, a complete thermal conduction network can be formed inside the polymer. When the polymer is heated, it can accelerate the heat transfer from the high temperature area to the low temperature area, thereby prolonging the ignition time. And graphene has a lamellar structure, which can increase the melt viscosity, play an anti-dripping role, and prevent the occurrence of dripping. Furthermore, the amount of graphene used is 6-8 parts. Within this range, the flame retardant and reinforcing effects of graphene can be fully exerted, and the compatibility problems caused by excessive use of graphene can be avoided.
[0013] Furthermore, the alkyl phosphinate is aluminum diethylphosphinate.
[0014] Furthermore, the particle size of the nano-diatomaceous earth is 50-500nm.
[0015] Furthermore, the coupling agent is one or more of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.
[0016] Furthermore, the flow modifier is one or more of pentaerythritol stearate, talcum powder, and polyethylene wax.
[0017] Furthermore, the high-strength flame-retardant composite material for a reducer includes the following components in parts by weight: 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomaceous earth, 3 parts of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0018] The second aspect of the present invention discloses a method for preparing a high-strength flame-retardant composite material for a reducer, comprising the following steps:
[0019] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0020] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melted and extruded through the twin-screw extruder;
[0021] (3) The product melt-extruded by the twin-screw extruder is cooled, pelletized, sieved, and dried to obtain a high-strength flame-retardant composite material for a reducer.
[0022] Furthermore, the extrusion temperature of the twin-screw extruder is controlled at 310-320° C., and the screw speed is controlled at 400-600 r / min.
[0023] Furthermore, the cooling adopts a water cooling process.
[0024] Compared with the prior art, the advantages and positive effects of the present invention are: providing a high-strength flame-retardant composite material for a reducer and a preparation method thereof. The composite material significantly improves the flame retardant properties of the PA12T material and has excellent processing properties and mechanical properties. The alkyl phosphinate has excellent flame retardancy, and the presence of cations can prevent the volatilization loss of the flame retardant. At the same time, the salts of these cations have a good smoke suppression effect. Nano diatomite can be used as a flame retardant synergist for alkyl phosphinates, and can effectively improve thermal stability and residual rate. Pentaerythritol not only plays the role of a dispersant, but also is an excellent carbon-forming agent itself, which can form a phosphorus-silicon-carbon flame retardant system with alkyl phosphinates and diatomite to improve the flame retardant effect. Among them, diatomite has excellent adsorption properties, and can also improve the dispersion properties of alkyl phosphinate flame retardants and pentaerythritol, prevent the precipitation of alkyl phosphinate flame retardants and pentaerythritol during processing, and affect the surface properties of the product. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the specific structures, process conditions and results described in the examples are only used to illustrate the present invention and should not and will not limit the present invention described in detail in the claims.
[0027] Unless otherwise specified, the component types in the following examples and comparative examples are consistent, wherein the alkyl phosphinate is aluminum diethylphosphinate, the particle size of nano-diatomaceous earth is 100 nm, the coupling agent is KH560, and the flow modifier is talc.
[0028] Example 1
[0029] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0030] 60 parts of nylon 12T, 20 parts of glass fiber, 10 parts of alkyl phosphinate, 4 parts of nano diatomite, 2 parts of pentaerythritol, 5 parts of graphene, 1 part of coupling agent, and 1 part of flow modifier.
[0031] The preparation method comprises the following steps:
[0032] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0033] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 400 r / min.
[0034] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0035] Example 2
[0036] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0037] 70 parts of nylon 12T, 30 parts of carbon fiber, 15 parts of alkyl phosphinate, 8 parts of nano diatomite, 4 parts of pentaerythritol, 8 parts of graphene, 3 parts of coupling agent, and 3 parts of flow modifier.
[0038] The preparation method comprises the following steps:
[0039] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0040] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 500 r / min.
[0041] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0042] Example 3
[0043] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0044] 70 parts of nylon 12T, 20 parts of glass fiber, 10 parts of alkyl phosphinate, 4 parts of nano diatomaceous earth, 4 parts of pentaerythritol, 5 parts of graphene, 3 parts of coupling agent, and 3 parts of flow modifier.
[0045] The preparation method comprises the following steps:
[0046] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0047] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 600 r / min.
[0048] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0049] Example 4
[0050] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0051] 60 parts of nylon 12T, 30 parts of glass fiber, 15 parts of alkyl phosphinate, 8 parts of nano diatomite, 2 parts of pentaerythritol, 8 parts of graphene, 1 part of coupling agent, and 1 part of flow modifier.
[0052] The preparation method comprises the following steps:
[0053] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0054] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 500 r / min.
[0055] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0056] Example 5
[0057] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0058] 63 parts of nylon 12T, 28 parts of glass fiber, 12 parts of alkyl phosphinate, 5 parts of nano diatomaceous earth, 2.5 parts of pentaerythritol, 6 parts of graphene, 2.2 parts of coupling agent, and 2.1 parts of flow modifier.
[0059] The preparation method comprises the following steps:
[0060] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0061] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 400 r / min.
[0062] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0063] Example 6
[0064] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0065] 68 parts of nylon 12T, 23 parts of carbon fiber, 14 parts of alkyl phosphinate, 7 parts of nano diatomite, 3 parts of pentaerythritol, 7 parts of graphene, 3 parts of coupling agent, and 1 part of flow modifier.
[0066] The preparation method comprises the following steps:
[0067] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0068] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 500 r / min.
[0069] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0070] Example 7
[0071] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0072] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomite, 3 parts of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0073] The preparation method comprises the following steps:
[0074] (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix;
[0075] (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melt-extruded through the twin-screw extruder; the extrusion temperature of the twin-screw extruder is controlled at 315° C., and the screw speed is controlled at 500 r / min.
[0076] (3) The product melt-extruded by the twin-screw extruder is subjected to water cooling, pelletizing, screening, and drying to obtain a high-strength flame-retardant composite material for a reducer.
[0077] Example 8
[0078] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0079] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomaceous earth, 3 parts of pentaerythritol, 4 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0080] The preparation process is the same as that of Example 7.
[0081] Example 9
[0082] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0083] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomite, 3 parts of pentaerythritol, 10 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0084] The preparation process is the same as that of Example 7.
[0085] Comparative Example 1
[0086] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0087] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 9 parts of nano diatomaceous earth, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0088] The preparation process is the same as that of Example 7.
[0089] Comparative Example 2
[0090] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0091] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 9 parts of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0092] The preparation process is the same as that of Example 7.
[0093] Comparative Example 3
[0094] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0095] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 12 parts of nano diatomaceous earth, 3 parts of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0096] The preparation process is the same as that of Example 7.
[0097] Comparative Example 4
[0098] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0099] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomite, 1 part of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0100] The preparation process is the same as that of Example 7.
[0101] Comparative Example 5
[0102] A high-strength flame-retardant composite material for a reducer, comprising the following components in parts by weight:
[0103] 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomaceous earth, 7 parts of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent, and 2 parts of flow modifier.
[0104] The preparation process is the same as that of Example 7.
[0105] The reducers prepared in the examples and comparative examples were injection molded into standard styles using high-strength flame-retardant composite materials, and the tensile strength MPa, flexural strength MPa, and notched impact strength kJ / m 2 The test results of relevant performance indicators such as flame retardancy, droplets, and surface precipitation are shown in Table 1-2. Among them, the precipitation level is divided into levels 1-5, indicating the precipitation situation on the surface of the sample. Level 1 means no precipitation, and from level 1 to level 5, the precipitation situation becomes increasingly serious.
[0106]
[0107]
[0108] As can be seen from Table 1-Table 2, the high-strength flame-retardant composite material for reducer prepared by the present invention significantly improves the flame retardant properties of PA12T material, and has excellent mechanical properties. Nano diatomite can not only be used as a flame retardant synergist of alkyl phosphinate, but also can effectively improve thermal stability and residual rate. Pentaerythritol not only plays the role of a dispersant, but also is an excellent carbon-forming agent itself, which can form a phosphorus-silicon-carbon flame retardant system with alkyl phosphinate and diatomite to improve the flame retardant effect. Among them, diatomite has excellent adsorption properties, and can also improve the dispersibility of alkyl phosphinate flame retardants and pentaerythritol, prevent the precipitation of alkyl phosphinate flame retardants and pentaerythritol during processing, and improve the surface properties of the product. Comparative Examples 1-2 show that nano diatomite and pentaerythritol, as flame retardant synergists of alkyl phosphinate, can effectively improve the flame retardant efficiency. Nano diatomite, as an inorganic filler, has a low compatibility with nylon, and due to the nano effect, its addition amount should be controlled, otherwise it will cause agglomeration, thereby affecting product performance. Pentaerythritol not only acts as a dispersant, but is also an excellent carbon-forming agent. It can form a phosphorus-silicon-carbon flame retardant system with alkyl phosphinates and diatomaceous earth to improve the flame retardant effect. However, similar to alkyl phosphinate flame retardants, pentaerythritol is also prone to surface precipitation during processing. When it is used in excessive amounts, it not only affects the surface properties of the product, but also leads to a decrease in the mechanical properties of the composite material.
[0109] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A high-strength flame-retardant composite material for a reducer, characterized in that: The composition comprises the following components in parts by weight: 60-70 parts of nylon 12T, 20-30 parts of fiber-reinforced filler, 10-15 parts of alkyl phosphinate, 4-8 parts of nano-diatomite, 2-4 parts of pentaerythritol, 4-10 parts of graphene, 1-3 parts of coupling agent, and 1-3 parts of flow modifier; the particle size of the nano-diatomite is 50-500nm.
2. The high-strength flame-retardant composite material for a reducer according to claim 1, characterized in that: The fiber-reinforced filler is one or more of glass fiber, carbon fiber, and whisker fiber.
3. The high-strength flame-retardant composite material for a reducer according to claim 1, characterized in that: The alkyl phosphinate is aluminum diethylphosphinate.
4. The high-strength flame-retardant composite material for a reducer according to claim 1, characterized in that: The coupling agent is one or more of a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.
5. The high-strength flame-retardant composite material for a reducer according to claim 1, characterized in that: The flow modifier is one or more of pentaerythritol stearate, talcum powder and polyethylene wax.
6. The high-strength flame-retardant composite material for a reducer according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 65 parts of nylon 12T, 25 parts of glass fiber, 13 parts of alkyl phosphinate, 6 parts of nano diatomite, 3 parts of pentaerythritol, 6 parts of graphene, 2 parts of coupling agent and 2 parts of flow modifier.
7. A method for preparing a high-strength flame-retardant composite material for a reducer according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weighing each component according to a ratio, and uniformly mixing nylon 12T, alkyl phosphinate, nano-diatomaceous earth, pentaerythritol, graphene, coupling agent, and flow modifier in a high-speed mixer to obtain a premix; (2) adding the premix into a twin-screw extruder through a main feed port, adding the fiber-reinforced filler into the twin-screw extruder through a side feed port, and the materials are melted and extruded through the twin-screw extruder; (3) The product melt-extruded by the twin-screw extruder is cooled, pelletized, sieved, and dried to obtain a high-strength flame-retardant composite material for a reducer.
8. The method for preparing a high-strength flame-retardant composite material for a reducer according to claim 7, characterized in that: The extrusion temperature of the twin-screw extruder is controlled at 310-320° C., and the screw speed is controlled at 400-600 r / min.
9. The method for preparing a high-strength flame-retardant composite material for a reducer according to claim 7, characterized in that: The cooling adopts a water cooling process.