Preparation method and application of composite filler

High oxygen content graphene oxide is prepared by the Hummers method and compounded with solid fillers to form a three-dimensional structure, which solves the problem of poor dispersion and coating of graphene in high-viscosity polymer systems, and significantly improves its performance in polymer materials. Mechanical properties and reinforcement effects.

CN118725613APending Publication Date: 2024-10-01SHANDONG JINLIT NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410717610.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Graphene has poor dispersion in high-viscosity polymer systems and is easily coated or embedded with the filler surface, affecting its reinforcing effect on polymer materials.

Method used

Graphite oxide is prepared using the Hummers method. By controlling the degree of oxidation and acid treatment, graphene oxide forms a high oxygen content and a three-dimensional structure. It is combined with solid fillers to form a three-dimensional graphene oxide/solid filler composite powder, which improves its performance in polymers. Dispersion and enhanced properties in materials.

Benefits of technology

Significantly improves the mechanical properties of graphene oxide in polymer materials, enhances its binding force with polymer materials, reduces the processing cost of polymer materials, and avoids the coating phenomenon between graphene oxide and fillers , improving the overall performance of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725613A_ABST
    Figure CN118725613A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a composite filler, and relates to the field of filler preparation, the preparation method comprises the following steps: S1, preparing graphite oxide: taking graphite, concentrated sulfuric acid and potassium permanganate as raw materials, preparing a graphite oxide filter cake according to a hummers method, and controlling the oxygen content in the obtained graphite oxide to be greater than 41%; s2, adding pure water into the graphite oxide obtained in the step S1, and fully stripping to obtain graphene oxide slurry A with a certain concentration; S3, dropwise adding acid into the slurry A, and continuously stirring until clear liquid or obvious granular aggregates appear, so as to obtain slurry B; s4, taking solid filler, adding water, and pulping to obtain filler slurry; uniformly mixing filler slurry with the slurry B obtained in the step S3 to obtain mixed slurry C; s5, standing and layering the slurry C, taking lower-layer precipitate, performing filter pressing to obtain a three-dimensional graphene oxide / solid filler composite filter cake, and performing crushing and drying to obtain three-dimensional graphene oxide / solid filler composite powder; the preparation method comprises the following steps: fully stripping graphite oxide to obtain graphene oxide with a high single-layer rate, protonating the single-layer graphene oxide into flower-shaped three-dimensional graphene oxide in an acid adding manner, and finally compounding the flower-shaped three-dimensional graphene oxide with a solid filler, so that the structure with abundant wrinkles has a stronger anchoring effect on a macromolecular chain after being infiltrated by macromolecules, and the high-molecular-weight three-dimensional graphene oxide is obtained. The application performance of the graphene oxide in a high polymer material is more favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filler preparation, and in particular to a preparation method of a composite filler and application thereof. Background Art

[0002] Graphene is a two-dimensional carbon nanomaterial composed of carbon atoms in a hexagonal honeycomb lattice with sp2 hybrid orbitals. It has excellent optical, electrical and mechanical properties and has important application prospects in materials science, micro-nano processing, energy, biomedicine and drug delivery. At present, many scholars have modified polymers such as rubber products, plastic products, and resin-based composite materials by adding a small amount of graphene to improve their thermodynamic properties, electrical properties, air tightness, etc.

[0003] As we all know, the performance of graphene has a huge relationship with its number of layers, and in the field of graphene, researchers and technical R&D personnel generally believe that the fewer the number of layers, or even when it reaches a single layer, the more outstanding the performance. For example, in the master's thesis "Preparation and Performance Research of Graphene-Enhanced Natural Rubber" published in 2022, P8-P20 disclosed the effect of different numbers of GO (graphene oxide) layers on the performance of filled rubber composites. The results showed that compared with multi-layer GO, rubber composites with few layers of GO as fillers have better mechanical properties, heat generation properties and wear resistance. However, the application process of graphene still has the problem of how to effectively disperse a very small amount of graphene in the polymer, as mentioned in patent 201710583823.5, which is the technical bottleneck currently faced by the application of few-layer graphene. The reason is that the graphene surface with a complete structure is a two-dimensional crystal composed of six-membered rings without any unstable bonds. Its surface is inert and is a typical amphiphobic structure with little interaction with polymers. In addition, there is a strong van der Waals force between graphene sheets, which is easy to aggregate and difficult to disperse in the polymer matrix, which seriously affects the application of graphene in polymer modification. The existing conventional dispersion technology is difficult to overcome the current defects. Using oxygen-containing groups such as carboxyl, hydroxyl and epoxy groups on the graphene oxide sheet structure, covalent modification and non-covalent modification can increase dispersibility, but the enhanced performance of oxidized modified graphene is not obvious.

[0004] In view of the excellent performance of graphene polymer composite materials and the obvious shortcomings of the dispersion and compatibility of graphene in the polymer matrix, the prior art generally adopts a method of first compounding graphene with fillers such as calcium carbonate and then mixing it into the polymer material. The compounding process is generally as follows:

[0005] 1. Coprecipitation or in-situ composite method: For example, the preparation of nano calcium carbonate and reduced graphene oxide composite in patent 202210561014.5: the prepared graphene oxide dispersion is used as the reaction liquid, calcium chloride and urea with a mass ratio of 1:1 are added as the reactants of calcium carbonate, and then a surfactant (CTAB) and a surface inhibitor (T-20) are added. After ultrasonic stirring, the mixture is placed in a reactor for hydrothermal reaction at 140-160°C for a period of time, and then the composite is obtained after centrifugation, washing, and drying. Patent 201710958043.4 discloses the following process steps: A) graphene oxide, an organic solvent miscible with water, and water are dispersed to obtain a graphene oxide dispersion; B) the graphene oxide dispersion obtained in the above step is mixed with a zinc source to obtain a precursor solution; C) the precursor solution obtained in the above step is reacted with stearic acid to obtain a zinc stearate / graphene oxide composite material. Patent 201810107839.3 discloses the following process steps: (1) mixing graphene quantum dots with calcium salt solution and dimethyl carbonate; (2) heating in a water bath at 20-22°C and stirring for 1-5 min; (3) adding sodium hydroxide solution to the mixed solution obtained in step (2), stirring for 30 s, and standing; (4) filtering, washing with anhydrous ethanol, flushing the product from the filter membrane into a centrifuge tube with anhydrous ethanol, and vacuum drying at 30°C-80°C for 24 h to obtain graphene quantum dots and calcium carbonate composite nanospheres; Patent 202111682572.9 S1: stirring and digesting quicklime and tap water, filtering and removing slag to prepare Ca(OH) 2 Slurry; S2: Ca(OH) 2 The slurry is mixed with graphene, and a surfactant containing dimethyl sulfoxide is added; the temperature is raised to 60-80°C, maintained for 3-4 hours, and then cooled to 25°C; S3: CO is introduced 2Mix the gas, control the reaction temperature to react at a constant temperature under ultrasonic conditions; add a crystal control agent, and stop the reaction when the pH is 7; S4: peel and separate the product, add rare earth stearate, and stir the reaction; filter while hot, grind, and dry to obtain graphene-calcium carbonate nanocomposite powder. The process in patent 202210561014.5: (1) Preparation of graphene oxide dispersion: disperse graphene oxide (GO) prepared by the improved Hummers method in a polar solvent, stir and ultrasonically exfoliate the graphene oxide to obtain a uniformly dispersed graphene oxide dispersion; (2) Preparation of a composite of nano-calcium carbonate and reduced graphene oxide: use the prepared graphene oxide dispersion in (1) as the reaction liquid, add a mixed liquid of calcium chloride and urea prepared in a mass ratio of 1:1 to 1.5 and stirred evenly, then add hexadecyltrimethylammonium bromide (CTAB) and Tween-20 (T-20) and continue stirring until uniform, then place the reactants in a reactor for hydrothermal reaction for 4 to 8 hours, and finally obtain the composite after washing, centrifugation and drying.

[0006] 2. Wet mixing: The process disclosed in Patent 202210487549.2 includes the following steps: 1) firstly preparing calcium carbonate into calcium carbonate / ethanol slurry by ball milling; 2) then adding graphene / ethanol dispersion to 1); 3) after co-ball milling, freeze-drying the slurry to obtain graphene / heavy calcium carbonate composite filler.

[0007] In both of the above processes, graphene or graphene oxide is first uniformly dispersed to prepare a dispersion, and then calcium carbonate is precipitated in the graphene / graphene oxide dispersion or mixed with the calcium carbonate slurry to ensure uniform (few layers) dispersion of graphene in the generated graphene / calcium carbonate composite material.

[0008] Although the above process solves the dispersibility problem of graphene, it has the following defects: first, graphene or graphene oxide is completely dispersed, then the graphene or graphene oxide in the dispersion liquid mostly exists in the form of a single layer or a few layers, and the lamellar structure of graphene is very flexible, and it is very easy to form a coating on the surface of calcium carbonate, or to be closely combined with calcium carbonate particles. Especially in the process of in-situ precipitation, calcium carbonate will grow on the surface of graphene. After this composite material is added to a polymer system such as plastic or rubber, a high-viscosity polymer material wants to contact with graphene and first has to overcome the solid phase interface between graphene and calcium carbonate before it can diffuse to the graphene surface. This process is undoubtedly difficult, so the role that graphene can play will also be greatly reduced.

[0009] Therefore, in response to the above problems, a new preparation process is urgently needed, which can not only solve the dispersion problem of graphene in high-viscosity polymer systems, but also avoid the coating and embedding of graphene on the surface of commonly used fillers, thereby affecting the reinforcement effect on polymer materials. Summary of the invention

[0010] The present invention aims at solving the above problems existing in the prior art and provides a method for preparing a composite filler, so as to simultaneously solve the dispersion problem of graphene in a high-viscosity polymer system and avoid the formation of coating and embedding of graphene on the surface of the filler to affect the reinforcing effect on the polymer material.

[0011] The technical solution of the present invention to solve the above technical problems is as follows:

[0012] In one aspect, the present invention provides a method for preparing a composite filler, characterized in that it comprises the following steps:

[0013] S1. Preparation of graphite oxide: Using graphite, concentrated sulfuric acid and potassium permanganate as raw materials, prepare graphite oxide filter cake according to the Hummers method, and control the oxygen content in the obtained graphite oxide to be greater than 41%. At this time, a slightly exfoliated graphite oxide filter cake is obtained. The degree of exfoliation in step S2 is controlled by controlling the oxygen content in the graphite oxide. The higher the degree of oxidation, the more oxygen-containing functional groups there are, the higher the degree of exfoliation in S2, and the stronger the binding force between the graphite oxide and the polymer in subsequent use.

[0014] S2, adding pure water to the graphite oxide obtained in step S1 and fully exfoliating it into a graphene oxide slurry A of a certain concentration. The common purpose of steps S1 and S2 is to increase the degree of exfoliation in this step as much as possible, so that the graphene oxide in this step exists in a single layer as much as possible, so that the amount of graphene oxide used can be minimized to achieve the same effect.

[0015] S3, adding acid dropwise to slurry A, and continuously stirring until a clear liquid or granular aggregates appear, to obtain slurry B. In this step, the microstructure of graphene oxide in the slurry is transformed from a two-dimensional sheet structure to a three-dimensional structure with rich wrinkles.

[0016] S4, adding water to the solid filler and beating the solid filler to obtain a filler slurry; mixing the filler slurry with the slurry B obtained in step S3 to obtain a mixed slurry C;

[0017] S5, allowing slurry C to stand for stratification, taking out the lower precipitate and filtering it to obtain a three-dimensional graphene oxide / solid filler composite filter cake, and crushing and drying it to obtain a three-dimensional graphene oxide / solid filler composite powder.

[0018] Furthermore, in step S1, graphite oxide is prepared by the Hummers method: graphite is added to concentrated sulfuric acid under stirring and mixed; potassium permanganate is added to the mixture, and the temperature is controlled not to be higher than 10°C during the addition process, and stirred; the temperature is raised to 30-40°C and kept stirred; pure water is added to the mixed solution under stirring, and then the temperature is raised to 80-100°C and stirred; after the reaction is completed, the temperature is lowered to room temperature and hydrogen peroxide is added, filtered, and the obtained graphite oxide filter cake is acid-washed and washed with water.

[0019] Furthermore, in step S1, the mass ratio of graphite to concentrated sulfuric acid is 1:165-1:55, and the mass ratio of graphite to potassium permanganate is 0.1:6-1:2.5.

[0020] Furthermore, in step S2, the concentration of graphene oxide slurry A is 0.1%-10%.

[0021] Furthermore, in step S3, the acid added dropwise is at least one of sulfuric acid and hydrochloric acid.

[0022] Furthermore, the solid filler in step S4 is a mixture of one or more of calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, silicon dioxide, clay, talc, attapulgite, kaolin, diatomaceous earth, fly ash, carbon black, carbon nanotubes, mica powder, zinc oxide, silicon carbide, and aluminum hydroxide.

[0023] Furthermore, in step S4, the mass ratio of solid filler to water in pulping is 1:4-1:1.5, and the mass ratio of graphene oxide to solid filler in slurry C is 0.1:100-1:2. The loading concentration of graphene oxide in the filler is controlled by controlling the material ratio. If the loading concentration of graphene oxide is too low, the amount of composite filler used will be large and the cost will be high; if the loading concentration is too high, it cannot be guaranteed.

[0024] On the other hand, the present invention provides an application of the method for preparing the composite filler, characterized in that the obtained three-dimensional graphene oxide / solid filler composite powder is used as a filler, and the filler is added to the polymer material system according to the formula of the polymer material system to prepare the graphene-enhanced polymer material. For example, in the processing stage of the polymer material, the filler is added to the polymer material system by mixing, kneading, and high-speed dispersion.

[0025] Furthermore, the polymer material system is a rubber system, a thermoplastic plastic system or a thermosetting resin system.

[0026] The beneficial effects of the present invention are as follows: the present invention changes the conventional process route of first preparing graphene oxide products and then using them for downstream products, and instead uses graphene oxide obtained by preliminary exfoliation of graphite by the Hummers method as a raw material, first fully exfoliates the graphene oxide to obtain graphene oxide with a high monolayer rate, then protonates the monolayer graphene oxide into flower-shaped three-dimensional graphene oxide by adding acid, and finally compounds with solid fillers. This technical solution can bring the following beneficial effects:

[0027] 1) The graphene oxide used in the composite filler has a high degree of oxidation, that is, it contains rich functional groups. When used, it can form a richer bonding structure with the polymer, and has a better reinforcement effect on the polymer.

[0028] 2) After the graphene oxide is fully peeled off, an acid is added to the slurry to protonate the functional groups (-COO-, -O-, etc.) on the surface of the nearly monolayer graphene oxide that have been ionized in water into -COOH, -OH, etc., thereby curling up into a three-dimensional graphene oxide structure with rich wrinkles. The formed three-dimensional graphene oxide is a three-dimensional structure, and it is not easy to form a coating or embedding structure with the solid filler during the composite process with the solid filler, which is further conducive to the contact and infiltration of the polymer with the graphene oxide surface. After being infiltrated by the polymer, this wrinkled structure has a stronger anchoring effect on the polymer chain, which is more conducive to improving the application performance of graphene oxide in polymer materials.

[0029] 3) The preparation scheme of composite fillers is extensive and has a wide range of composite concentrations. It is applicable to many fillers and the appropriate filler type can be selected according to the polymer system to be modified.

[0030] 4) The use of composite fillers is simple and generally does not require changes to the polymer processing technology. They can be used in the same way as the original fillers.

[0031] 5) The composite filler prepared by the present invention is applied to rubber, resin, and plastic to significantly improve their mechanical properties, with the improvement reaching more than 20%. Compared with the traditional method of simply mixing graphene and fillers as reinforcing and modifying agents for polymer materials, this method has a significant improvement in the increase in mechanical properties.

[0032] 7) The whole process is simple and easy to operate. During the composite process, graphene oxide has been pre-dispersed in the composite filler. When adding it to the polymer system, there is no need to use a dispersant to effectively disperse the graphene oxide. That is, the problem of poor dispersibility of graphene oxide in the polymer system is solved without the need to add an additional dispersant, and the modification cost is lower. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a SEM image of the three-dimensional graphene oxide / carbon black composite filler prepared in step S4 of Example 6 of the present invention;

[0034] Figure 2 This is a SEM image of the graphene oxide / carbon black composite filler prepared in step S4 of comparative example 5 of the present invention. DETAILED DESCRIPTION

[0035] The principles and features of the present invention are described below. The examples given are only used to explain the present invention but not to limit the scope of the present invention.

[0036] Details of the main materials used in the following examples and comparative examples are shown in Tables 1 to 3.

[0037] Table 1 Graphite information table used in the examples and comparative examples

[0038]

[0039]

[0040] Table 2 Filler information table used in examples and comparative examples

[0041] Filling name Manufacturer Product Model Calcium carbonate Yixing Huakai Calcium Carbonate Co., Ltd. Light calcium carbonate 1200 mesh Attapulgite Hebei Fangji New Materials Technology Co., Ltd. 1200 mesh Clay Lingshou County Zhongxin Mineral Products Processing Factory Rubber filled clay 800 mesh Calcium sulfate Shandong Jinlite New Materials Co., Ltd. Sedimentation method, 800 mesh Barium sulfate Shandong Jinlite New Materials Co., Ltd. Sedimentation method, 1200 mesh Titanium dioxide Shijiazhuang Jiatuo Chemical Technology Co., Ltd. R-248 Carbon Black Tianjin Tianyi Century Chemical Products Technology Development Co., Ltd. N990 talcum powder Dongguan Sanlong New Material Technology Co., Ltd. 5000 mesh Fly ash Lingshou County Xuyang Mining Co., Ltd. Level 1 Kaolin Lingshou County Kexu New Materials Co., Ltd. Calcinated 1200 mesh diatomite Lingshou County Qianfu Mineral Products Processing Factory 325 mesh Silicon dioxide Evonik Official Flagship Store R972 Carbon Nanotubes Shandong Dazhan Nanomaterials Co., Ltd. GT-300 Mica powder Chuzhou Pagoda Sericite Mining Co., Ltd. 800 mesh Zinc Oxide Shijiazhuang Duoyi Chemical Technology Co., Ltd. Rubber Grade Silicon Carbide Hebei Ruihuang Metal Materials Co., Ltd. Nanoscale Aluminum hydroxide Henan Hongjia Chemical Products Co., Ltd. 1250 mesh

[0042] Table 3 Information of polymer materials used in Examples and Comparative Examples

[0043]

[0044]

[0045] Example 1

[0046] The preparation of the composite filler in this embodiment is carried out according to the following steps:

[0047] S1. Preparation of graphite oxide: using graphite, concentrated sulfuric acid and potassium permanganate as raw materials, graphite oxide is prepared according to the Hummers method, and the oxygen content of the obtained graphite oxide is controlled to be greater than 41%. Specifically:

[0048] Weigh graphite and concentrated sulfuric acid at a mass ratio of 1:165, inject concentrated sulfuric acid into the reactor first, add graphite into the concentrated sulfuric acid under continuous stirring, and continue stirring for 30 minutes to mix the two evenly;

[0049] Start the cold cycle, and slowly add potassium permanganate to the above mixture under continuous stirring. The mass ratio of potassium permanganate to graphite is 6:0.1, and the temperature is controlled not higher than 10°C during the addition process. Maintain the low temperature stirring for 3 hours; then, raise the temperature to 30°C and keep stirring for 2 hours;

[0050] Add pure water 100 times the mass of graphite to the above mixed solution, and keep stirring during the addition process. After the addition is completed, heat the mixed solution to 100°C and stir for 30 minutes; after the reaction is completed, cool it to room temperature and add hydrogen peroxide until no bubbles are generated; filter, and then wash the obtained graphite oxide filter cake with hydrochloric acid and water for multiple times to ensure thorough washing.

[0051] S2. Add pure water to the graphite oxide obtained in step S1 and fully exfoliate it into slurry A with a concentration of 0.1% using a double planetary disperser.

[0052] S3. Add hydrochloric acid dropwise to slurry A and continue stirring until granular agglomerates appear to obtain slurry B.

[0053] S4, taking solid filler calcium carbonate, and adding water and beating at a mass ratio of solid filler to water of 1:1.5 to obtain filler slurry; mixing the filler slurry with slurry B obtained in step S3 to obtain mixed slurry C, wherein the mass ratio of graphene oxide to solid filler is 1:50.

[0054] S5. Allow slurry C to stand for stratification, remove the lower precipitate and filter press to obtain a three-dimensional graphene oxide / calcium carbonate composite filter cake, and grind and dry to obtain a three-dimensional graphene oxide / calcium carbonate composite powder.

[0055] S6, the composite filler three-dimensional graphene oxide / calcium carbonate composite powder prepared by S5 is added to the polymer material system PVC to prepare graphene enhanced PVC material. The preparation process is as follows: 100 parts by weight of PVC resin, 12.5 parts of composite filler (composite powder obtained by S5), 3.2 parts of dibutyltin maleate, 0.15 parts of stearic acid, and 0.3 parts of PE wax are weighed and mixed evenly in a high-speed mixer, and then sent to a twin-screw extruder to obtain graphene-modified PVC pipe A1. At the same time, a blank control is performed to obtain PVC pipe B1, that is, graphene oxide is not added in the blank test. The impact strength of pipes A1 and B1 is measured respectively, and the increase in the impact strength of A1 relative to the impact strength of B1 is calculated. The results show that the impact strength of the graphene-modified PVC pipe A1 prepared in this embodiment is 25% higher than that when no graphene is added.

[0056] Example 2

[0057] The preparation of the composite filler in this embodiment is carried out according to the following steps:

[0058] S1. Preparation of graphite oxide: using graphite, concentrated sulfuric acid and potassium permanganate as raw materials, graphite oxide is prepared according to the Hummers method, and the oxygen content of the obtained graphite oxide is controlled to be greater than 41%. Specifically:

[0059] Weigh graphite and concentrated sulfuric acid at a mass ratio of 1:130, inject the concentrated sulfuric acid into the reactor first, add graphite into the concentrated sulfuric acid under continuous stirring, and continue stirring for 30 minutes to mix the two evenly;

[0060] Start the cold cycle, and slowly add potassium permanganate to the above mixture under continuous stirring. The mass ratio of potassium permanganate to graphite is 5:1, and the temperature is controlled not higher than 10°C during the addition process. Maintain the low temperature stirring for 1 hour; then, raise the temperature to 40°C and keep stirring for 3 hours;

[0061] Add pure water 100 times the mass of graphite to the above mixed solution, and keep stirring during the addition process. After the addition is completed, heat the mixed solution to 80°C and keep stirring for 60 minutes; after the reaction is completed, cool it to room temperature and add hydrogen peroxide until no bubbles are generated; filter, and then acid wash (hydrochloric acid) and water wash the obtained graphite oxide filter cake multiple times to wash it thoroughly.

[0062] S2. Add pure water to the graphite oxide obtained in step S1 and fully exfoliate it into slurry A with a concentration of 2% using a double planetary disperser.

[0063] S3. Sulfuric acid is added dropwise to slurry A and stirred continuously until obvious granular agglomerates appear to obtain slurry B.

[0064] S4, taking solid filler attapulgite, and adding water and beating at a mass ratio of solid filler to water of 1:2 to obtain filler slurry; mixing the filler slurry with slurry B obtained in step S3 to obtain mixed slurry C, wherein the mass ratio of graphene oxide to solid filler is 1:30.

[0065] S5. Allow slurry C to stand for stratification, remove the lower precipitate and filter press to obtain a three-dimensional graphene oxide / attapulgite composite filter cake, and grind and dry to obtain a three-dimensional graphene oxide / attapulgite composite powder.

[0066] S6, adding the composite filler prepared in S5 to the polymer material low-density polyethylene system, according to the weight parts of low-density polyethylene 100 parts, ethylene-vinyl acetate copolymer 20 parts, epoxy resin 8 parts, graphene oxide / attapulgite composite filler 2 parts, bis (2, 4-dicumylphenyl) pentaerythritol diphosphite 2 parts, Al (OH) 3 3 parts of each component were weighed and put into a reactor for stirring and mixing, extruded to obtain a PE pipe; sent to a twin-screw extruder, put into the screw extruder for extrusion molding, and obtained PE pipe A2. At the same time, a blank control was carried out to obtain PE pipe B2, that is, no graphene oxide was added in the blank test. The impact strength of pipes A2 and B2 was measured respectively, and the increase in the impact strength of A2 relative to the impact strength of B2 was calculated. The results show that the impact strength of the graphene-modified PE pipe A1 prepared in this embodiment is 26.2% higher than that without adding graphene.

[0067] Example 3

[0068] The preparation of the composite filler in this embodiment is carried out according to the following steps:

[0069] S1. Preparation of graphite oxide: using graphite, concentrated sulfuric acid and potassium permanganate as raw materials, graphite oxide is prepared according to the Hummers method, and the oxygen content of the obtained graphite oxide is controlled to be greater than 41%. Specifically:

[0070] Weigh graphite and concentrated sulfuric acid at a mass ratio of 1:80, inject the concentrated sulfuric acid into the reactor first, add graphite into the concentrated sulfuric acid under continuous stirring, and continue stirring for 30 minutes to mix the two evenly;

[0071] Start the cold cycle, and slowly add potassium permanganate to the above mixture under continuous stirring. The mass ratio of potassium permanganate to graphite is 2.5:1. During the addition process, the temperature is controlled not higher than 10°C, and the low temperature stirring is maintained for 2 hours. Subsequently, the temperature is raised to 35°C and stirred for 5 hours.

[0072] Add pure water 100 times the mass of graphite to the above mixed solution, and keep stirring during the addition process. After the addition is completed, heat the mixed solution to 100°C and stir for 60 minutes; after the reaction is completed, cool it to room temperature and add hydrogen peroxide until no bubbles are generated; filter, and then acid wash (hydrochloric acid) and water wash the obtained graphite oxide filter cake multiple times to wash it thoroughly.

[0073] S2. Add pure water to the graphite oxide obtained in step S1 and fully exfoliate it into slurry A with a concentration of 3% using a double planetary disperser.

[0074] S3. Add hydrochloric acid dropwise to slurry A and continue stirring until obvious granular agglomerates appear to obtain slurry B.

[0075] S4, taking a mixture of solid filler clay and silicon carbide, wherein the mass ratio of clay: silicon carbide = 1:4, and adding water at a mass ratio of solid filler to water of 1:3 and beating to obtain filler slurry; mixing the filler slurry with slurry B obtained in step S3 to obtain mixed slurry C, wherein the mass ratio of graphene oxide to solid filler is 1:20.

[0076] S5. Allow slurry C to stand for stratification, remove the lower precipitate and filter press to obtain a three-dimensional graphene oxide / clay composite filter cake, and grind and dry to obtain a three-dimensional graphene oxide / clay / silicon carbide composite powder.

[0077] S6, adding the composite filler prepared in S5 to the rubber system, according to the weight parts of 25 parts of butyl acrylate rubber, 10 parts of EPDM rubber, 5 parts of diene rubber, 15 parts of styrene butadiene rubber, 10 parts of epoxy resin, 10 parts of graphene oxide / clay / silicon carbide composite filler, 10 parts of white carbon black, 3 parts of di-tert-butyl paracresol, 5 parts of epoxidized soybean oil, Al(OH) 36 parts of each component are weighed, and after preliminary mixing in a kneader, they are put into a twin-screw extruder for secondary mixing. The mixed mixture is poured into a preheated mold for vulcanization to obtain rubber A3 modified with graphene oxide. At the same time, a blank control is carried out to obtain rubber B3, that is, no graphene oxide is added in the blank test. Abrasion tests are performed on modified rubbers A3 and B3 respectively, and the reduction in A3 abrasion relative to B3 abrasion is calculated. The results show that the abrasion of the graphene-modified rubber prepared in this embodiment is reduced by 26.8% compared with when no graphene oxide is added.

[0078] Example 4

[0079] The preparation of the composite filler in this embodiment is carried out according to the following steps:

[0080] S1. Preparation of graphite oxide: using graphite, concentrated sulfuric acid and potassium permanganate as raw materials, graphite oxide is prepared according to the Hummers method, and the oxygen content of the obtained graphite oxide is controlled to be greater than 41%. Specifically:

[0081] Weigh graphite and concentrated sulfuric acid at a mass ratio of 1:55, inject the concentrated sulfuric acid into the reactor first, add graphite into the concentrated sulfuric acid under continuous stirring, and continue stirring for 30 minutes to mix the two evenly;

[0082] Start the cold cycle, and slowly add potassium permanganate to the above mixture under continuous stirring. The mass ratio of potassium permanganate to graphite is 5:1, and the temperature is controlled not higher than 10°C during the addition process. Maintain the low temperature stirring for 3 hours; then, increase the temperature to 40°C and keep stirring for 5 hours;

[0083] Add pure water 100 times the mass of graphite to the above mixed solution, and keep stirring during the addition process. After the addition is completed, heat the mixed solution to 80°C and keep stirring for 60 minutes; after the reaction is completed, cool it to room temperature and add hydrogen peroxide until no bubbles are generated; filter, and then acid wash (hydrochloric acid) and water wash the obtained graphite oxide filter cake multiple times to wash it thoroughly.

[0084] S2. Add pure water to the graphite oxide obtained in step S1 and fully exfoliate it into slurry A with a concentration of 8% using a double planetary disperser.

[0085] S3. Add sulfuric acid dropwise to slurry A and continue stirring until a clear liquid appears to obtain slurry B.

[0086] S4, taking solid filler calcium sulfate, and adding water and beating at a mass ratio of solid filler to water of 1:4 to obtain filler slurry; mixing the filler slurry with slurry B obtained in step S3 to obtain mixed slurry C, wherein the mass ratio of graphene oxide to solid filler is 1:20.

[0087] S5. Allow slurry C to stand for stratification, remove the lower precipitate and filter press to obtain a three-dimensional graphene oxide / calcium sulfate composite filter cake, and grind and dry to obtain a three-dimensional graphene oxide / calcium sulfate composite powder.

[0088] S6, add the composite filler prepared in S5 to the PVC system, according to 90 parts by weight of PVC resin, 3 parts of chlorinated polyethylene, 1 part of tribasic lead sulfate, 3 parts of tribasic lead stearate, 0.5 parts of butyl stearate, 1 part of oxidized polyethylene wax, 0.2 parts of zinc stearate, 1 part of KH-550, 4 parts of graphene oxide / calcium sulfate composite filler, weigh each component and add it to a hot mixer and mix it evenly, and then prepare it into sheet A4 through a conical twin-screw extruder. At the same time, a blank control is carried out to obtain sheet B4, that is, graphene oxide is not added in the blank test. The impact strength of sheets A4 and B4 is tested respectively, and the increase in the impact strength of A4 relative to the impact strength of B4 is calculated. The results show that the impact strength of the graphene-modified PVC sheet prepared in this embodiment is 25.9% higher than that without adding graphene.

[0089] Example 5

[0090] The preparation of the composite filler in this embodiment is carried out according to the following steps:

[0091] S1. Preparation of graphite oxide: the preparation process is the same as that in Example 3.

[0092] S2. Add pure water to the graphite oxide obtained in step S1 and fully exfoliate it to form a slurry A with a concentration of 10%.

[0093] S3-S5 are basically the same as Example 4, except that the solid filler in this embodiment is titanium dioxide; and the mass ratio of graphene oxide to titanium dioxide in S4 is 1:2.

[0094] S6, add the composite filler prepared in S5 to the epoxy resin system, according to the weight of the formula, 120 parts of epoxy resin, 60 parts of polyamide, 5 parts of melamine, 15 parts of ammonium polyphosphate, 15 parts of pentaerythritol, 5 parts of graphene oxide / titanium dioxide composite filler, 50 parts of iron oxide green, 2 parts of BYK-333, 1 part of BYK-024, 1 part of BYK-163, 20 parts of water, weigh each component, first add the graphene oxide / titanium dioxide composite filler to the epoxy resin, disperse it in a high-speed disperser, then add other components and mix them evenly to obtain graphene-modified epoxy floor paint A5. At the same time, a blank control was performed to obtain epoxy floor paint B5, that is, no graphene oxide was added in the blank test. The wear resistance of floor paints A5 and B5 was tested respectively, and the increase in the wear resistance of A5 relative to the wear resistance of B5 was calculated. The results show that the wear resistance of the floor paint modified with graphene oxide prepared in this embodiment is improved by 29.8% compared with the case where no graphene oxide is added.

[0095] Example 6

[0096] The implementation steps of this embodiment are basically the same as those of Embodiment 1, except that the solid filler used in step S4 is carbon black, and the mass ratio of carbon black to water during the preparation of carbon black slurry is 1:4.

[0097] S6, add the composite filler prepared in S5 to the rubber system, and weigh the components according to the weight of the formula: 100 parts of natural rubber, 2 parts of graphene oxide / carbon black composite filler, 38 parts of carbon black, 7 parts of C5 petroleum resin, 5 parts of N,N′-diphenyl-p-phenylenediamine, 6 parts of di-tert-butyl-p-cresol, 15 parts of dithiocarbamate, and 18 parts of p-benzoquinone dioxime. First, put the graphene oxide / carbon black composite filler and natural rubber in a mixer for internal mixing, and then add carbon black, interface modifier, antioxidant, antioxidant, vulcanization accelerator, activator and softener in sequence. After internal mixing for 1 hour, discharge the rubber material, cool it to room temperature, and then mix the rubber material on the open mill for 1 hour, add the vulcanizer, mix well and press it into film A6. At the same time, a blank control is carried out to obtain rubber B6, that is, no graphene oxide is added in the blank test. The tear strength of films A6 and B6 was tested respectively, and the increase of the tear strength of A6 relative to the tear strength of B6 was calculated. The results showed that the tear strength of the graphene oxide modified film prepared in this embodiment was increased by 21.7% compared with the film without adding graphene oxide.

[0098] Example 7

[0099] The implementation steps S1-S5 of this embodiment are basically the same as those of Embodiment 1, except that the solid filler used in step S4 is a mixture of talcum powder, mica powder and barium sulfate, wherein the mass ratio of talcum powder: mica powder: barium sulfate is 1:1:5, and the mass ratio of graphene oxide to solid filler is 0.1:100.

[0100] S6. Add the composite filler prepared in S5 to the aqueous polyurethane emulsion system, and weigh the components according to the weight parts of the formula: 75 parts of aqueous polyurethane emulsion (solid content 65%), 0.5 parts of tannic acid, 1 part of BYK-035, 0.1 parts of wetting agent CF-10, 2.0 parts of gray paste, 1.5 parts of dipropylene glycol butyl ether, 5 parts of zinc phosphate, and 35 parts of graphene oxide / talcum powder / mica powder / barium sulfate composite filler. First, disperse the graphene oxide / talcum powder composite filler in the aqueous polyurethane by high-speed stirring, and then add other components in sequence until mixed evenly to obtain component A of the polyurethane coating; take 50g of component A, add 35g of curing agent aziridine polymer, mix evenly, and then brush it on a tinplate sheet to form a film, and test the adhesion of the paint film (cross-hatch method). The result shows that the adhesion is 21Mpa. At the same time, a blank control was performed, that is, graphene oxide was not added in the blank test, the paint film adhesion of the blank control was measured, and the increase in the paint film adhesion of this embodiment compared with the blank control was calculated. The results showed that the paint film adhesion of the graphene oxide polyurethane paint film prepared in this embodiment was increased by 22.8% compared with that without adding graphene oxide.

[0101] Example 8

[0102] The implementation steps S1-S5 of this embodiment are basically the same as those of embodiment 3, except that the solid filler used in step S4 is a mixture of fly ash and zinc oxide, wherein the mass ratio of fly ash: zinc oxide is 1:10.

[0103] S6. Add the composite filler prepared in S5 to the rubber system according to the weight parts in the formula: 35 parts of butyl acrylate rubber, 20 parts of EPDM rubber, 30 parts of styrene-butadiene rubber, 20 parts of polyethylene glycol, 10 parts of allyl glycidyl ether solution, 10 parts of graphene oxide / fly ash / zinc oxide composite filler, 10 parts of epoxy resin, 15 parts of calcium carbonate, 10 parts of white carbon black, 8 parts of di-tert-butyl-p-cresol, 8 parts of epoxy soybean oil, Al(OH) 3 7 parts of each component are weighed, and after preliminary mixing in a kneader, they are put into a twin-screw extruder for secondary mixing. The mixed mixture is poured into a preheated mold for vulcanization to obtain rubber A8 modified with graphene oxide. At the same time, a blank control is performed to obtain rubber B8, that is, no graphene oxide is added in the blank test. Abrasion tests are performed on modified rubbers A8 and B8 respectively, and the reduction in abrasion of A8 relative to that of B8 is calculated. The results show that the graphene oxide modified rubber prepared in this embodiment has a 26.4% lower abrasion than the modified rubber without adding graphene oxide.

[0104] Example 9

[0105] The implementation steps S1-S5 of this embodiment are basically the same as those of Embodiment 3, except that the solid filler used in step S4 is a mixture of kaolin and aluminum hydroxide, wherein the mass ratio of kaolin:aluminum hydroxide is 10:7, and the mass ratio of graphene oxide to the mixed filler is 0.1:100.

[0106] S6, add the composite filler prepared in S5 to the rubber system, according to the weight of the formula, 35 parts of butyl acrylate rubber, 20 parts of EPDM rubber, 30 parts of styrene-butadiene rubber, 20 parts of polyethylene glycol, 10 parts of allyl glycidyl ether solution, 17 parts of graphene oxide / kaolin / aluminum hydroxide composite filler, 10 parts of epoxy resin, 15 parts of calcium carbonate, 10 parts of white carbon black, 8 parts of di-tert-butyl-p-cresol, and 8 parts of epoxy soybean oil. Weigh each component, and after preliminary mixing in a kneader, put it into a twin-screw extruder for secondary mixing, pour the mixture after mixing into a preheated mold for vulcanization, and obtain rubber A9 modified with graphene oxide. At the same time, a blank control is performed to obtain rubber B9, that is, graphene oxide is not added in the blank test. Wear tests are performed on modified rubbers A9 and B9 respectively, and the reduction in wear of A9 relative to that of B9 is calculated. The results show that the wear of the graphene oxide modified rubber prepared in this embodiment is reduced by 23.6% compared with the modified rubber without adding graphene oxide.

[0107] Example 10

[0108] The implementation steps S1-S5 of this embodiment are basically the same as those of embodiment 3, except that the solid filler used in step S4 is diatomaceous earth, and the ratio of graphene oxide to diatomaceous earth is 1:2.

[0109] S6, the composite filler prepared in S5 is added to the water-based organosilicon system, according to the formula water-based organosilicon emulsion 50 parts, add graphene oxide / diatomite composite filler 1 part, diacetone alcohol 2 parts, benzyl alcohol 0.5 parts, methyl silicone oil defoamer 0.5 parts, iron oxide 5 parts, phthalocyanine blue 10 parts, by high-speed disperser 1500rpm mechanical stirring 30min, then with 4000rpm number of mechanical stirring 2h to prepare graphene oxide modified water-based organosilicon resin coating. The prepared water-based organosilicon resin coating is applied to the surface of the aluminum alloy substrate, dried and cured to obtain a paint film A10 modified by graphene oxide, and a blank control is carried out to obtain a paint film B10, that is, graphene oxide is not added in the blank test. The modified paint films A10 and B10 are respectively subjected to the weather resistance of the paint films, and the increase in the weathering time of A10 relative to the weathering time of B10 is calculated. The results show that the weathering time of the graphene oxide modified paint film prepared in this embodiment is increased by 218 hours compared with the paint film without adding graphene oxide.

[0110] Embodiment 11

[0111] The implementation steps S1-S5 of this embodiment are basically the same as those of embodiment 4, except that the solid filler used in step S4 is silicon dioxide.

[0112] S6. Add the composite filler prepared in S5 to the rubber system according to the formula: 100 parts of silicone rubber, 10 parts of graphene oxide / silicon dioxide composite filler, 6 parts of zinc stearate, 20 parts of nano-calcium carbonate, and 5 parts of dioctyl phthalate. After weighing each component, first disperse the graphene oxide / silicon dioxide composite filler in the silicone resin by a high-speed disperser, and then add other components in turn and mix evenly to prepare an organic silicone adhesive. After decompression and degassing, the above-mentioned organic silicone adhesive is coated on a glass plate with a length of 8 cm, a width of 4 cm, and a thickness of 2 mm, and then covered with a glass plate of the same size. After curing, the tensile strength is tested according to GB / T528-2009. The results show that the tensile strength of the sample modified with graphene oxide is 5.6 MPa. At the same time, a blank sample without adding graphene oxide is prepared. Comparison shows that the sample modified with graphene oxide is 2.3 MPa higher than that without adding graphene oxide.

[0113] Example 12

[0114] The implementation steps S1-S5 of this embodiment are basically the same as those of embodiment 4, except that the solid filler used in step S4 is carbon nanotubes.

[0115] S6. Add the composite filler prepared in S5 to the PE system. Weigh the components according to the formula: 100 parts of high-density polyethylene, 10 parts of graphene oxide / carbon nanotube composite filler, 2 parts of silicon carbide whiskers, 0.5 parts of polyethylene wax, and 0.5 parts of tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. Mix the above components evenly through a mixer and then convey them to a twin-screw extruder to prepare polyethylene pipes. At the same time, prepare blank polyethylene pipe samples without adding graphene oxide, and perform impact strength tests on the two pipes. The results show that the impact strength of the modified pipe with added graphene oxide is increased by 25.8% compared with the case without adding graphene.

[0116] Comparative Example 1

[0117] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 2, except that step S3 is removed, that is, after the graphene oxide slurry is prepared, it is directly mixed with the attapulgite slurry to prepare the graphene oxide / attapulgite composite filler. Similarly, the composite filler is added to the low-density polyethylene to prepare a modified PE pipe, and the impact strength of the modified PE pipe is tested. The results show that the impact strength of the graphene-modified PE pipe prepared in this comparative example is increased by 6.8% compared with when no graphene oxide is added.

[0118] Comparative Example 2

[0119] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 3, except that step S3 is removed, that is, after the graphene oxide slurry is prepared, it is directly mixed with the clay and silicon carbide slurries to prepare the graphene oxide / clay / silicon carbide composite filler. Similarly, the composite filler is added to the rubber system to prepare a modified rubber, and the modified rubber is subjected to a wear test. The results show that the wear of the graphene modified rubber prepared in this comparative example is basically the same as that when no graphene oxide is added.

[0120] Comparative Example 3

[0121] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 4, except that step S3 is removed, that is, the graphene oxide slurry is directly mixed with the calcium sulfate slurry after the graphene oxide slurry is prepared to prepare the graphene oxide / calcium sulfate composite filler. Similarly, the composite filler is added to the PVC resin to prepare a modified PVC sheet, and the impact strength of the modified PVC sheet is tested. The results show that the impact strength of the graphene-modified PVC sheet prepared in this comparative example is improved by 3.7% compared with the case without adding graphene oxide.

[0122] Comparative Example 4

[0123] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 5, except that step S3 is removed, that is, after the graphene oxide slurry is prepared, it is directly mixed with the titanium dioxide slurry to prepare the graphene oxide / titanium dioxide composite filler. Similarly, the composite filler is added to the epoxy resin to prepare a modified epoxy resin floor paint, and the modified epoxy resin floor paint is subjected to a wear resistance test. The results show that the wear of the graphene epoxy resin floor paint prepared in this comparative example is reduced by 1.8% compared with when no graphene oxide is added.

[0124] Comparative Example 5

[0125] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 6, except that step S3 is removed, that is, the graphene oxide slurry is directly mixed with the carbon black slurry after the graphene oxide slurry is prepared to prepare the graphene oxide / carbon black composite filler. Similarly, the composite filler is added to the rubber system to prepare a film, and the tear strength of the film is tested. The test results show that the tear strength of the rubber film modified by the comparative example sample is only 2.4% higher than that without adding graphene oxide.

[0126] Comparative Example 6

[0127] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 7, except that step S3 is removed, that is, after the graphene oxide slurry is prepared, it is directly mixed with a mixed slurry of talcum powder, mica powder, and barium sulfate to prepare a graphene oxide / talcum powder / mica powder / barium sulfate composite filler. Similarly, the composite filler is added to the waterborne polyurethane system to prepare a modified polyurethane coating, and the adhesion of the modified polyurethane coating is tested. The results show that the adhesion of the graphene-modified polyurethane coating prepared in this comparative example is 18Mpa, which is 5.3% higher than when no graphene oxide is added.

[0128] Comparative Example 7

[0129] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 8, except that step S3 is removed, that is, after the graphene oxide slurry is prepared, it is directly mixed with the mixed slurry of fly ash and zinc oxide to prepare the graphene oxide / fly ash / zinc oxide composite filler. Similarly, the composite filler is added to the rubber system to prepare a modified rubber, and the modified rubber is subjected to a wear test. The results show that the wear of the graphene modified rubber prepared in this comparative example is only reduced by 3.5% compared with when no graphene oxide is added.

[0130] Comparative Example 8

[0131] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 10, except that step S3 is removed, that is, the graphene oxide slurry is directly mixed with the diatomite slurry after the graphene oxide slurry is prepared to prepare the graphene oxide / diatomite composite filler. Similarly, the composite filler is added to the aqueous silicone emulsion system to prepare a modified silicone resin coating, and the weather resistance of the modified silicone resin coating film is tested. The results show that the weather resistance time of the silicone resin coating film prepared in this comparative example is basically the same as that when no graphene oxide is added.

[0132] Comparative Example 9

[0133] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 11, except that step S3 is removed, that is, the graphene oxide slurry is directly mixed with the silicon dioxide slurry after the graphene oxide slurry is prepared to prepare the graphene oxide / silicon dioxide composite filler. Similarly, the composite filler is added to the silicone rubber system to prepare a modified silicone rubber adhesive, and the tensile strength of the modified silicone rubber adhesive is tested. The results show that the tensile strength of the silicone rubber adhesive prepared in this comparative example is 4.1Mpa, which is 0.8Mpa higher than when no graphene oxide is added.

[0134] Comparative Example 10

[0135] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 12, except that step S3 is removed, that is, the graphene oxide slurry is directly mixed with the carbon nanotube slurry after the graphene oxide slurry is prepared to prepare the graphene oxide / carbon nanotube composite filler. Similarly, the composite filler is added to the high-density polyethylene system to prepare a modified polyethylene pipe, and the impact strength of the modified polyethylene pipe is tested. The results show that the impact strength of the modified polyethylene pipe prepared in this comparative example is 2.9% higher than that when no graphene oxide is added.

[0136] Comparative Example 11

[0137] The process steps for preparing the composite material in this comparative example are basically the same as those in Example 1, except that the mass ratio of graphene oxide to calcium carbonate in step S4 is 1:1. It was found during the preparation process that the particles of the composite filler were hard after drying. It is speculated that the reason is that the proportion of graphene oxide is relatively high, and the functional groups between graphene oxides lose water during the drying process, causing agglomeration. Similarly, the prepared composite filler is added to the polymer material system PVC to prepare a pipe. The impact strength of the pipe was tested, and the results showed that the impact strength was reduced by 5.3% compared with when no graphene oxide was added.

[0138] The experimental data of the above embodiments and comparative examples are summarized in Table 4.

[0139] Table 4 Experimental data of various embodiments and comparative examples

[0140]

[0141]

[0142]

[0143] As can be seen from the data in Table 1, the graphene composite filler obtained by the technical solution of the present invention is applied to downstream products, and the reinforcing effect of graphene on composite materials in terms of impact strength, wear resistance, tear strength, adhesion, tensile strength, weather resistance, etc. is significantly improved, especially compared with the conventional mixing method of existing graphene slurry and ordinary filler slurry, the increase / decrease is obvious. Taking Example 6 and Comparative Example 5 as an example, after adding the three-dimensional graphene oxide / carbon black composite filler to the rubber system using the technical solution of the present invention, the tear strength of the obtained product is 46.5N / mm, which is 21.7% higher than when no graphite oxide is added. However, the increase in the tear strength of the rubber by adding the composite filler prepared in Comparative Example 5 is only 2.4%. This is because the three-dimensional graphene oxide prepared in the present invention has a three-dimensional structure, and it is not easy to form a coating or embedding structure with the solid filler during the composite process with the solid filler, which is further conducive to the contact and infiltration of the polymer with the surface of the graphene oxide. After being infiltrated by the polymer, this wrinkled structure has a stronger anchoring effect on the polymer chain, which is more conducive to improving the application performance of graphene oxide in polymer materials.

[0144] In addition, by comparing the experimental results of Example 1 with those of Comparative Example 11, it can be seen that when the mass ratio of graphene oxide to the composite filler is too large, the obtained sample is relatively hard. After being crushed and added to the polymer system (PVC), the performance of the obtained product decreases instead of increases. It is speculated that when the proportion of graphene oxide is high, the graphene oxide in the composite filler cannot be fully dispersed, and the graphene oxides are inevitably in contact and agglomerate, which is not suitable for polymer modification.

[0145] Attached Figure 1 3D graphene oxide / carbon black composite filler prepared in step S4 of Example 6. The SEM images of the three-dimensional graphene oxide / carbon black composite filler prepared in step S4 of other embodiments show that the product structure and morphology are basically the same as those in the attached Figure 1 , which will not be shown one by one here; Figure 2 This is a SEM image of the graphene oxide / carbon black composite filler prepared in step S4 of comparative example 5.

[0146] contrast Figure 1 , Figure 2It can be seen that the graphene oxide compounded with carbon black in the preparation process of the composite filler of the embodiment of the present invention is a three-dimensional structure, and it is not easy to form a coating or embedding structure with carbon black during the composite process. After the composite filler is added to the polymer system, the polymer can fully contact with the graphene oxide to form a composite, thereby exerting a good reinforcement effect; while the state of the graphene oxide compounded with carbon black in the preparation process of Comparative Example 5 is a two-dimensional sheet structure with good peeling. From the SEM image of the obtained sample ( Figure 2 ) It can be clearly seen that the surface of graphene oxide is basically completely attached and buried by carbon black. Therefore, when it is applied to a polymer system, the polymer cannot fully contact with the graphene oxide, and ultimately the enhancement effect cannot be exerted.

Claims

1. A method for preparing a composite filler, characterized in that: The steps include: S1. Preparation of graphite oxide: using graphite, concentrated sulfuric acid and potassium permanganate as raw materials, preparing graphite oxide filter cake according to Hummers method, and controlling the oxygen content in the obtained graphite oxide to be greater than 41%; S2, adding pure water to the graphite oxide obtained in step S1 and fully exfoliating it to form a graphene oxide slurry A of a certain concentration: S3, add acid dropwise to slurry A, and continue stirring until clear liquid or obvious granular agglomerates appear to obtain slurry B; S4, adding water to the solid filler and beating the solid filler to obtain a filler slurry; mixing the filler slurry with the slurry B obtained in step S3 to obtain a mixed slurry C; S5, allowing slurry C to stand for stratification, taking out the lower precipitate and filtering it to obtain a three-dimensional graphene oxide / solid filler composite filter cake, and crushing and drying it to obtain a three-dimensional graphene oxide / solid filler composite powder.

2. The method for preparing a composite filler according to claim 1, characterized in that: In step S1, graphite oxide is prepared by the Hummers method: graphite is added to concentrated sulfuric acid under stirring and mixed; potassium permanganate is added to the mixture, and the temperature is controlled not to be higher than 10° C. during the addition process, and stirred; the temperature is raised to 30-40° C. and stirred at the same temperature; pure water is added to the mixed solution under stirring, and then the temperature is raised to 80-100° C. and stirred; after the reaction is completed, the temperature is lowered to room temperature and hydrogen peroxide is added, filtered, and the obtained graphite oxide filter cake is acid-washed and washed with water.

3. The method for preparing a composite filler according to claim 1 or 2, characterized in that: In step S1, the mass ratio of graphite to concentrated sulfuric acid is 1:165-1:

55.

4. The method for preparing a composite filler according to claim 1 or 2, characterized in that: In step S1, the mass ratio of graphite to potassium permanganate is 0.1:6-1:2.

5.

5. The method for preparing a composite filler according to claim 1, characterized in that: The acid added dropwise in step S3 is at least one of sulfuric acid and hydrochloric acid.

6. The method for preparing a composite filler according to claim 1, characterized in that: The concentration of graphene oxide slurry A in step S2 is 0.1%-10%.

7. The method for preparing a composite filler according to claim 1, characterized in that: The solid filler in step S4 is a mixture of one or more of calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, silicon dioxide, clay, talc, attapulgite, kaolin, diatomaceous earth, fly ash, carbon black, carbon nanotubes, mica powder, zinc oxide, silicon carbide, and aluminum hydroxide.

8. The method for preparing a composite filler according to claim 1 or 7, characterized in that: The mass ratio of solid filler to water in the pulping in step S4 is 1:4-1:1.

5.

9. The method for preparing a composite filler according to claim 1 or 7, characterized in that: The mass ratio of graphene oxide to solid filler in slurry C of step S4 is 0.1:100-1:

2.

10. Application of the method for preparing a composite filler according to any one of claims 1 to 9, characterized in that: The obtained three-dimensional graphene oxide / solid filler composite powder is used as a filler, and the filler is added to the polymer material system according to the formula of the polymer material system to prepare a graphene-reinforced polymer material; the polymer material system is preferably a rubber system, a thermoplastic plastic system or a thermosetting resin system.