Carbon-sequestration environment-friendly latex paint for removing metalloid particles in indoor air and preparation method thereof
By coating indoor walls with carbon-fixing and environmentally friendly latex paint, and using synergistic carbon-fixing agents such as iron oxide powder, copper ferrite powder and nano-cerium dioxide powder, the problem of removing arsenic and carbon dioxide from indoor air is solved, and wall insulation is achieved. Dual effect of water layer and air quality optimization.
Patent Information
- Application Number
- CN202410935012.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
At present, there is a lack of simple and easy removal methods for both arsenic and carbon dioxide pollution in indoor air.
A carbon-fixing environmentally friendly latex paint is used. The preparation raw materials include water-based interior wall latex paint, iron oxide powder, copper ferrite powder and nano-cerium dioxide powder, etc. to form a synergistic carbon-fixing agent, which is prepared through steps such as ultrasonic dispersion and magnetic stirring. Coated on interior walls to remove arsenic and carbon dioxide.
The latex paint not only serves as a waterproof layer and decorative layer on the wall, but can also effectively remove arsenic and carbon dioxide in indoor air, improve indoor air quality, and provide a simple and easy removal method.
Smart Images

Figure BDA0004941040550000081 
Figure BDA0004941040550000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of wall coating materials, and in particular to a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air and a preparation method thereof. Background Art
[0002] For people who are forced to live indoors for a long time, excessive arsenic and carbon dioxide in the air are very serious problems. Arsenic is at the boundary between metal elements and non-metal elements in the periodic table, so it is called a metalloid, also called a semi-metal. Its physical and chemical properties are also between metals and non-metals. It has a silver-gray metallic luster and a density of 5.72g / cm 3 Arsenic is also bioaccumulative and non-degradable in the environment. Its toxicity and treatment methods are similar to those of heavy metals, so arsenic is considered a heavy metal in the field of environmental pollution and medicine. my country's "Ambient Air Quality Standard" (GB 3095) limits the concentration of arsenic to 0.006μg / m 3 At the same time, when carbon dioxide is between 1000ppm and 4800ppm, the higher the concentration, the lower the learning and work efficiency of people, and the higher the error rate.
[0003] However, there is currently no simple and easy method to remove both arsenic and carbon dioxide from the air. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air and a preparation method thereof, aiming to solve the problem that there is currently no simple and easy removal method for both arsenic and carbon dioxide pollution in the air.
[0005] To achieve the above object, the present invention provides a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air. The raw materials for preparation include, by weight:
[0006] 95 to 105 parts of water-based interior wall latex paint,
[0007] 1-2 parts of iron oxide powder,
[0008] 0.3 to 1 part of copper ferrite powder,
[0009] 2 to 4 parts of carbon fixer,
[0010] Wherein, the carbon fixing agent comprises nano cerium dioxide powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder.
[0011] Optionally, the carbon fixing agent includes, by weight: 0.05 to 0.2 parts of nano cerium dioxide powder, 1 to 1.5 parts of potassium carbonate, 0.15 to 0.3 parts of L-arginine powder, 0.5 to 1 parts of lithium zirconate, and 0.5 to 1 parts of lithium silicate powder.
[0012] Optionally, the carbon-fixing agent includes N-methyl-2-pyrrolidone.
[0013] Optionally, the particle size of the nano cerium dioxide powder is 20 nm to 50 nm.
[0014] Optionally, the preparation raw materials include aesthetic auxiliary materials and health-care auxiliary materials, the aesthetic auxiliary materials include at least one of calcite powder, purple stone powder, crystal stone powder, and petrified wood powder, and the health-care auxiliary materials include at least one of obsidian powder, sandalwood powder, taimei stone powder, selenium ore powder, and white turquoise.
[0015] In order to achieve the above object, the present invention also provides a method for preparing a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air, comprising the following steps:
[0016] Ultrasonic dispersion of water-based interior wall latex paint for 2 to 3 minutes, adding iron oxide powder and carbon fixer thereto to obtain an intermediate product;
[0017] Copper ferrite fibers are prepared and then crushed to obtain copper ferrite powder;
[0018] Copper ferrite powder is added to the intermediate product, and ultrasonic dispersion is performed for 2 to 3 minutes to obtain a carbon-fixing and environmentally friendly latex paint for removing metal-like particles in indoor air.
[0019] Optionally, the preparation method of the copper ferrite fiber comprises:
[0020] S1: Weigh a ferric iron source, citric acid monohydrate and a copper source, add them into deionized water, and stir at 25-40° C. for 24-36 hours to obtain a dark green solution;
[0021] S2: Concentrating the dark green solution under reduced pressure at 40-70° C. to obtain a sol;
[0022] S3: adding the sol into a mixed solvent of water and low-carbon alcohol to dilute it, adding a spinning aid, stirring and aging it, to obtain a copper ferrite precursor spinning solution;
[0023] S4: electrospinning the copper ferrite precursor spinning solution, injecting the spinning solution into a syringe with a stainless steel needle, and obtaining copper ferrite precursor fibers under the action of a high voltage power supply;
[0024] S5: using a muffle furnace to heat-treat the copper ferrite precursor fiber to obtain copper ferrite fiber.
[0025] Optionally, the molar ratio of ferric iron source: citric acid monohydrate: copper source is 2: (2-4): 1.
[0026] Optionally, in step S3, the stirring time is 4 hours, and the aging time is 6 hours to 12 hours.
[0027] Optionally, in step S5, the heating rate of the heat treatment is 0.5-5°C / min, the heat treatment temperature is 750-850°C, and the temperature is kept at the highest temperature for 1-5 hours.
[0028] Beneficial effects of the present invention: The carbon-fixing environmentally friendly latex paint for removing metallic particles in indoor air provided by the present invention removes trivalent arsenic and inorganic arsenic particles in the air by adding iron oxide powder and copper ferrite powder respectively, and forms a synergistic carbon-fixing agent with nano cerium dioxide powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder. After being coated on the indoor wall, it not only serves as a wall waterproof layer and decorative layer, but also has the effect of optimizing the indoor air. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0030] Unless otherwise specified, all technical and scientific terms used herein have the common meanings in the art to which the claimed subject matter belongs, and all reagents used are industrial or analytically pure.
[0031] For people who are forced to live indoors for a long time, excessive arsenic and carbon dioxide in the air are very serious problems. Arsenic is at the boundary between metal elements and non-metal elements in the periodic table, so it is called a metalloid, also called a semi-metal. Its physical and chemical properties are also between metals and non-metals. It has a silver-gray metallic luster and a density of 5.72g / cm 3 Arsenic is also bioaccumulative and non-degradable in the environment. Its toxicity and treatment methods are similar to those of heavy metals, so arsenic is considered a heavy metal in the field of environmental pollution and medicine. my country's "Ambient Air Quality Standard" (GB 3095) limits the concentration of arsenic to 0.006μg / m 3 .
[0032] However, there is currently no simple and easy method to remove both arsenic and carbon dioxide from the air.
[0033] To solve the above problems, the present invention proposes a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air. The preparation raw materials include, by weight: 5 to 105 parts of water-based interior wall latex paint, 1 to 2 parts of iron oxide powder, 0.3 to 1 part of copper ferrite powder, and 2 to 4 parts of a carbon-fixing agent, wherein the carbon-fixing agent includes nano cerium dioxide powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder.
[0034] Interior wall latex paint refers to the paint used for indoor walls, which can be mainly divided into water-soluble paint and latex paint. In this solution, water-based interior wall latex paint is a commercially available product, and the material can include polyurethane, acrylic acid and other materials, such as German Kanamei water-based paint. Preferably, the main material of water-based interior wall latex paint is acrylic acid.
[0035] Iron oxide powder is magnetic and has a strong adsorption affinity for arsenic, especially for the removal of pentavalent arsenic, but its removal effect on trivalent arsenic is poor, so this solution introduces copper ferrite powder to synergistically remove trivalent arsenic. Nano cerium dioxide powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder form a synergistic carbon fixer. After coating the indoor wall, it not only serves as a wall waterproof layer and decorative layer, but also has the effect of optimizing indoor air.
[0036] Cerium dioxide (CeO 2 ) is a light yellow solid powder with relatively stable properties. It is a widely studied rare earth metal oxide. Potassium carbonate reacts with carbon dioxide to produce potassium bicarbonate. L-arginine is an activator, which can increase the reaction rate by 85%. It reacts with carbon dioxide: K 2 CO 3 +H 2 O+CO 2 =
[0037] 2KHCO 3 During the adsorption reaction of lithium zirconate and lithium silicate powder, the following reaction occurs: Li 4 SiO 4 +CO 2 =Li 2 SiO 3 +Li 2 CO 3 ;Li 2 ZrO 3 +CO 2 =Li 2 CO 3 +ZrO 2 .
[0038] In some embodiments, the carbon fixer has a maximum CO 2 Adsorption amount 50.0087mg(CO 2 ) / g(CeO2 ).
[0039] Furthermore, in parts by weight, the carbon-fixing agent includes: 0.05 to 0.2 parts of nano-cerium dioxide powder, 1 to 1.5 parts of potassium carbonate, 0.15 to 0.3 parts of L-arginine powder, 0.5 to 1 parts of lithium zirconate, and 0.5 to 1 parts of lithium silicate powder.
[0040] In some embodiments, the nano cerium dioxide powder is any value between 0.05 and 0.2 parts, such as 0.05, 0.1, 0.15, 0.2, etc.
[0041] Furthermore, the carbon fixer includes N-methyl-2-pyrrolidone. On the one hand, N-methyl-2-pyrrolidone acts as a solvent to provide a good dispersion environment for many powder materials in the inorganic carbon fixer to prevent agglomeration; on the other hand, N-methyl-2-pyrrolidone also directly acts as a physically adsorbed carbon dioxide removal agent.
[0042] In some embodiments, the weight of N-methyl-2-pyrrolidone is 2 to 3 parts. More preferably, the weight of N-methyl-2-pyrrolidone is 2 to 2.5 parts.
[0043] Furthermore, the particle size of the nano cerium dioxide powder is 20nm to 50nm. The particle size of the nano cerium dioxide powder within the above range can be better dispersed in water-based interior wall latex paint and more easily adhered to the microscopic morphology of copper ferrite powder.
[0044] In some embodiments, the particle size of the nano-cerium dioxide powder is any value between 20 nm and 50 nm, such as 20 nm, 30 nm, 40 nm, or 50 nm.
[0045] In some embodiments, the particle sizes of the iron oxide powder, copper ferrite powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder are 200 mesh to 3000 mesh.
[0046] Furthermore, the preparation raw materials include aesthetic auxiliary materials and health-care auxiliary materials. The aesthetic auxiliary materials include at least one of calcium silicate borate powder, purple stone powder, crystal stone powder, and petrified wood powder. The health-care auxiliary materials include at least one of obsidian powder, sandalwood powder, Taimei stone powder, selenium ore powder, and white turquoise.
[0047] Calcium borate powder, also known as soft calcium borate, is a crystalline aggregate, often in block form, white or grayish white, often with dark gray and black veins, and has a glassy luster; purple stone powder is purple with golden textures; the chemical composition of crystal stone powder is silicon dioxide, which belongs to the trigonal crystal system. The crystals are prismatic with hexagonal cones, and there are horizontal stripes on the cylindrical surface. There are often angular color bands in amethyst; petrified wood powder is stone evolved from wood. The material of petrified wood is as hard as stone, but it is famous for its exquisite wood patterns; the above materials are suitable for use as beautiful auxiliary materials for this plan.
[0048] Obsidian is a product of volcanic eruptions. It is a glassy rock with a composition equivalent to that of granite. It is a hexagonal crystal system and is rich in 16 trace elements beneficial to the human body, such as zinc, copper, molybdenum, chromium, cobalt, and manganese. It has high energy, infrared radiation and heat conduction effects, and has health care effects; sandalwood can remove dryness, kill bacteria, prevent mildew, prevent insects, and prevent moths, and has the effects of soothing nerves and refreshing the mind; sandalwood oil extracted from sandalwood has multiple effects such as cooling and astringing, strengthening the heart and nourishing, and lubricating the skin. It is an important medicine for treating skin diseases; Taimei stone powder contains B vitamins, which can promote growth and brain development and is beneficial to the skin; it contains selenium, which can be absorbed from the skin, and contains iron, calcium, and magnesium, which promote bone development, enhance kidney function, and are beneficial to the nervous system; white turquoise contains many trace elements beneficial to the human body; white turquoise can harmonize people's emotions and psychological state; the above materials are suitable for use as health care adjuvants in this plan.
[0049] To solve the above problems, the present invention also provides a method for preparing a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air, comprising the following steps:
[0050] S1: ultrasonically disperse water-based interior wall latex paint for 2 to 3 minutes, add iron oxide powder and carbon fixer thereto to obtain an intermediate product;
[0051] In some embodiments, after adding iron oxide powder and carbon fixer, magnetic stirring is performed using the iron oxide powder and the magnetic force of the magnets in the magnetic stirrer. The stirring time is 1 minute, so that the iron oxide powder and carbon fixer are more evenly dispersed in the water-based interior wall latex paint.
[0052] S2: preparing copper ferrite fibers and then crushing them to obtain copper ferrite powder;
[0053] In this scheme, copper ferrite fibers are prepared by electrospinning.
[0054] The crushing is achieved by high-speed shear force. Under the action of external force, the atomic bonding between the cleavage planes of copper ferrite fibers is destroyed, causing the fibers to break and crush, and copper ferrite powder is obtained. It can be understood that the macroscopic appearance is copper ferrite powder, and the microscopic appearance is short nanofiber strips, and there may be electrostatic agglomeration to form "micropores", which are conducive to the embedding of nano cerium dioxide powder in the carbon fixer and the dispersion of the overall powder in water-based interior wall latex paint.
[0055] S3: Add copper ferrite powder to the intermediate product and disperse it by ultrasonic for 2 to 3 minutes to obtain a carbon-fixing and environmentally friendly latex paint that removes metal-like particles in indoor air.
[0056] Furthermore, the preparation method of the copper ferrite fiber comprises:
[0057] S1: Weigh a ferric iron source, citric acid monohydrate and a copper source, add them into deionized water, and stir at 25-40° C. for 24-36 hours to obtain a dark green solution;
[0058] S2: Concentrating the dark green solution under reduced pressure at 40-70° C. to obtain a sol;
[0059] S3: adding the sol into a mixed solvent of water and low-carbon alcohol to dilute it, adding a spinning aid, stirring and aging it, to obtain a copper ferrite precursor spinning solution;
[0060] S4: electrospinning the copper ferrite precursor spinning solution, injecting the spinning solution into a syringe with a stainless steel needle, and obtaining copper ferrite precursor fibers under the action of a high voltage power supply;
[0061] S5: using a muffle furnace to heat-treat the copper ferrite precursor fiber to obtain copper ferrite fiber.
[0062] In some embodiments, the heat treatment atmosphere is air.
[0063] Further, the molar ratio of ferric iron source: citric acid monohydrate: copper source is 2: (2-4): 1. Preferably, the molar ratio of ferric iron source: citric acid monohydrate: copper source is 2: 3: 1.
[0064] Furthermore, in step S3, the stirring time is 4 hours, and the aging time is 6 hours to 12 hours.
[0065] Furthermore, in step S5, the heating rate of the heat treatment is 0.5-5°C / min, the heat treatment temperature is 750-850°C, and after reaching the highest temperature, the temperature is kept for 1-5 hours.
[0066] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.
[0067] Embodiment 1:
[0068] The raw materials for preparing the carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air are: 100 parts of water-based interior wall latex paint (commercially available finished product), 1 part of iron oxide powder (300 mesh), 0.3 parts of copper ferrite powder (300 mesh), 0.05 parts of nano cerium dioxide powder (50 nanometers), 1 part of potassium carbonate powder (300 mesh), 0.15 parts of L-arginine powder (300 mesh), 0.5 parts of lithium zirconate powder (300 mesh), 0.5 parts of lithium silicate powder (300 mesh), 0.5 parts of purple stone powder (300 mesh), 0.5 parts of crystal stone powder (300 mesh), 0.5 parts of obsidian powder (300 mesh), 0.5 parts of hydroxysilicon borolith powder (300 mesh), 0.5 parts of wood fossil powder (300 mesh), 0.5 parts of sandalwood powder (300 mesh), 0.5 parts of Taimei stone powder (300 mesh), 1 part of selenium ore powder (300 mesh), and 6 parts of water;
[0069] Preparation process:
[0070] Ultrasonic dispersion of water-based interior wall latex paint for 2 minutes, adding iron oxide powder and carbon fixer thereto, and then magnetic stirring for 1 minute to obtain an intermediate product;
[0071] Preparation of copper ferrite powder: weighing a trivalent iron source, citric acid monohydrate and a copper source in a molar ratio of 2:3:1, adding them to deionized water, and stirring at 25-40°C for 24 hours to obtain a dark green solution; concentrating the dark green solution under reduced pressure at 40-70°C to obtain a sol; diluting the sol with a mixed solvent of water and low-carbon alcohol, adding a spinning aid, stirring and aging to obtain a copper ferrite precursor spinning solution; electrospinning the copper ferrite precursor spinning solution, injecting the spinning solution into a syringe with a stainless steel needle, and obtaining a copper ferrite precursor fiber under the action of a high-voltage power supply; heat-treating the copper ferrite precursor fiber using a muffle furnace, with a heating rate of 2°C / min, a heat treatment temperature of 750-850°C, and keeping the temperature at 850°C for 3 hours to obtain copper ferrite fiber, and crushing the electrospun copper ferrite fiber into a high-speed shearing machine to obtain copper ferrite powder;
[0072] Copper ferrite powder is added to the intermediate product, and ultrasonic dispersion is performed for 2 minutes to obtain a carbon-fixing and environmentally friendly latex paint for removing metal-like particles in indoor air.
[0073] Embodiment 2:
[0074] The same as Example 1, except that: the raw materials for preparing the carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air are: 100 parts of water-based interior wall latex paint (commercially available finished product), 1.5 parts of iron oxide powder (300 mesh), 0.5 parts of copper ferrite powder (300 mesh), 0.1 parts of nano cerium dioxide powder (50 nanometers), 1.2 parts of potassium carbonate powder (300 mesh), 0.2 parts of L-arginine powder (300 mesh), 0.8 parts of lithium zirconate powder, 0.1 parts of cerium dioxide powder (50 nanometers), 0.1 ... 3 parts (300 mesh), 0.8 parts (300 mesh) of lithium silicate powder, 0.5 parts (300 mesh) of purple stone powder, 0.5 parts (300 mesh) of crystal stone powder, 0.5 parts (300 mesh) of obsidian powder, 0.5 parts (300 mesh) of calcium borohydride powder, 0.5 parts (300 mesh) of petrified wood powder, 0.5 parts (300 mesh) of sandalwood powder, 0.5 parts (300 mesh) of Taimei stone powder, 1 part (300 mesh) of selenium ore powder, and 7 parts of water.
[0075] Embodiment 3:
[0076] The same as Example 1, except that: the raw materials for preparing the carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air are: 100 parts of water-based interior wall latex paint (commercially available finished product), 2 parts of iron oxide powder (300 mesh), 1 part of copper ferrite powder (300 mesh), 0.2 parts of nano cerium dioxide powder (50 nanometers), 1.5 parts of potassium carbonate powder (300 mesh), 0.3 parts of L-arginine powder (300 mesh), 1 part of lithium zirconate powder ( 300 mesh), 1 part of lithium silicate powder (300 mesh), 0.5 part of purple stone powder (300 mesh), 0.5 part of crystal stone powder (300 mesh), 0.5 part of obsidian powder (300 mesh), 0.5 part of hydroxysilicon boron calcium stone powder (300 mesh), 0.5 part of wood fossil powder (300 mesh), 0.5 part of sandalwood powder (300 mesh), 0.5 part of Taimei stone powder (300 mesh), 1 part of selenium ore powder (300 mesh), and 8 parts of water.
[0077] Embodiment 4:
[0078] The same as Example 3, except that: the raw materials for preparing the carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air are: 100 parts of water-based interior wall latex paint (commercially available finished product), 1 part of iron oxide powder (300 mesh), 0.3 parts of copper ferrite powder (300 mesh), 0.05 parts of nano cerium dioxide powder (50 nanometers), 1 part of potassium carbonate powder (300 mesh), 0.15 parts of L-arginine powder (300 mesh), 0.5 parts of lithium zirconate powder (300 mesh), silicon dioxide powder (0.15 parts of L-arginine powder (300 mesh), 0.5 parts of lithium zirconate powder (300 mesh), 1 part of potassium carbonate powder (300 mesh), 0.05 parts of nano cerium dioxide powder (50 nanometers), 0.05 parts of nano cerium dioxide powder (50 nanometers), 0.05 parts of nano cerium dioxide powder (50 nanometers), 0.05 parts of nano cerium dioxide powder (50 nanometers), 0.05 parts of nano cerium dioxide powder (50 nanometers), 0.05 parts of nano cerium dioxide powder (50 nanometers), 0.05 parts of nano cerium dioxide powder (300 mesh ... 0.5 parts of lithium acid powder (300 mesh), 2.5 parts of N-methyl-2-pyrrolidone, 0.5 parts of purple stone powder (300 mesh), 0.5 parts of crystal stone powder (300 mesh), 0.5 parts of obsidian powder (300 mesh), 0.5 parts of hydroxysilicon boron calcium stone powder (300 mesh), 0.5 parts of wood fossil powder (300 mesh), 0.5 parts of sandalwood powder (300 mesh), 0.5 parts of Taimei stone powder (300 mesh), 1 part of selenium ore powder (300 mesh), and 6 parts of water.
[0079] Embodiment 5:
[0080] The same as Example 1, except that: copper ferrite powder is not prepared, and commercially available micro-spherical 300-mesh copper ferrite powder is used.
[0081] Comparative Example 1:
[0082] Only use water-based interior latex paint indoors.
[0083] Furthermore, a removal effect test was conducted on Examples 1-5 and Comparative Example 1. The test used air from 6 indoor rooms in an abandoned dormitory building. The 6 indoor rooms were painted with latex paints of Examples 1-5 and Comparative Example 1, respectively. Then the doors and windows were closed for one month. The room was 6 meters long, 3.6 meters wide, and 2.8 meters high. Arsenic and its compounds in the indoor air were determined by atomic fluorescence spectrometry, and carbon dioxide was determined by a carbon dioxide detector.
[0084] The test results are summarized in the following table:
[0085]
[0086]
[0087] In the above data, Example 4 is the optimal example, which achieves an arsenic and its compound removal rate of 28.0% and a carbon dioxide removal rate of 19.9% compared with Comparative Example 1; Example 4 adds N-methyl-2-pyrrolidone to the carbon fixer relative to Example 3. On the one hand, N-methyl-2-pyrrolidone acts as a carbon fixer solvent in the system, providing a good dispersion environment for many powder materials in the inorganic carbon fixer, and effectively preventing agglomeration; on the other hand, N-methyl-2-pyrrolidone is also directly used as a physically adsorbed carbon dioxide removal agent.
[0088] The above experimental results prove that the carbon-fixing and environmentally friendly latex paint for removing metallic particles in indoor air provided by the embodiment of the present invention removes trivalent arsenic and inorganic arsenic particles in the air by adding iron oxide powder and copper ferrite powder respectively, and forms a synergistic carbon-fixing agent with nano cerium dioxide powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder. After being coated on the indoor wall, it not only serves as a wall waterproof layer and decorative layer, but also has the effect of optimizing the indoor air, providing a healthy latex paint solution for people who stay indoors for a long time and have difficulty opening doors and windows.
[0089] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air, characterized in that: In parts by weight, the raw materials for preparation include: 95 to 105 parts of water-based interior wall latex paint, 1 to 2 parts of iron oxide powder, 0.3 to 1 part of copper ferrite powder, 2 to 4 parts of carbon fixer, Wherein, the carbon fixing agent comprises nano cerium dioxide powder, potassium carbonate, L-arginine powder, lithium zirconate and lithium silicate powder.
2. The carbon-fixing and environmentally friendly latex paint for removing metal-like particles in indoor air as claimed in claim 1, characterized in that: In parts by weight, the carbon fixing agent includes: 0.05 to 0.2 parts of nano cerium dioxide powder, 1 to 1.5 parts of potassium carbonate, 0.15 to 0.3 parts of L-arginine powder, 0.5 to 1 parts of lithium zirconate, and 0.5 to 1 parts of lithium silicate powder.
3. The carbon-fixing and environmentally friendly latex paint for removing metal-like particles in indoor air as claimed in claim 1, characterized in that: The carbon fixer includes N-methyl-2-pyrrolidone.
4. The carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air as claimed in claim 1, characterized in that: The particle size of the nano cerium dioxide powder is 20nm to 50nm.
5. The carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air as claimed in claim 1, characterized in that: The preparation raw materials include aesthetic auxiliary materials and health-care auxiliary materials. The aesthetic auxiliary materials include at least one of calcium silicate powder, purple stone powder, crystal stone powder, and petrified wood powder. The health-care auxiliary materials include at least one of obsidian powder, sandalwood powder, Taimei stone powder, selenium ore powder, and white turquoise.
6. A method for preparing a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air as claimed in claims 1 to 5, characterized in that: The following steps are involved: Ultrasonic dispersion of water-based interior wall latex paint for 2 to 3 minutes, adding iron oxide powder and carbon fixer thereto to obtain an intermediate product; preparing copper ferrite fibers and then crushing them to obtain copper ferrite powder; Copper ferrite powder is added to the intermediate product, and ultrasonic dispersion is performed for 2 to 3 minutes to obtain a carbon-fixing and environmentally friendly latex paint for removing metal-like particles in indoor air.
7. The method for preparing a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air according to claim 6, characterized in that: The preparation method of the copper ferrite fiber comprises: S1: Weigh a ferric iron source, citric acid monohydrate and a copper source, add them into deionized water, and stir at 25-40° C. for 24-36 hours to obtain a dark green solution; S2: Concentrating the dark green solution under reduced pressure at 40-70° C. to obtain a sol; S3: adding the sol into a mixed solvent of water and low-carbon alcohol to dilute it, adding a spinning aid, stirring and aging it, to obtain a copper ferrite precursor spinning solution; S4: electrospinning the copper ferrite precursor spinning solution, injecting the spinning solution into a syringe with a stainless steel needle, and obtaining copper ferrite precursor fibers under the action of a high voltage power supply; S5: using a muffle furnace to heat-treat the copper ferrite precursor fiber to obtain copper ferrite fiber.
8. The method for preparing a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air as claimed in claim 7, characterized in that: The molar ratio of ferric iron source: citric acid monohydrate: copper source is 2:(2-4):
1.
9. The method for preparing a carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air according to claim 7, characterized in that: In step S3, the stirring time is 4 hours, and the aging time is 6 hours to 12 hours.
10. The method for preparing carbon-fixing environmentally friendly latex paint for removing metal-like particles in indoor air according to claim 7, characterized in that: In step S5, the heating rate of the heat treatment is 0.5-5°C / min, the heat treatment temperature is 750-850°C, and the temperature is kept at the highest temperature for 1-5 hours.
Citation Information
Patent Citations
Interior wall latex paint having carbon dioxide absorption function
CN105602304A
Copper ferrite fiber for heterogeneous photo-Fenton catalytic degradation of dye and preparation method of copper ferrite fiber
CN116351420A