Manufacturing method of silk-screen printing ink with mesh plate wear inhibition effect

By premixing a wear-inhibiting lubricant and an antifoaming leveling agent in low-VOC screen printing inks to create a wear-inhibiting lubricating dispersion, the problem of mesh plate wear in low-VOC inks is solved, and printing stability and Improved cost effectiveness.

CN118725644APending Publication Date: 2024-10-01浙江彩皇精细化工有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062112.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Low-VOC screen printing inks cause mesh plate wear during mass production, affecting printing stability and cost. It is difficult with existing technology to achieve the mesh plate's wear resistance and stability without increasing the VOC mixing ratio.

Method used

By premixing a wear-inhibiting lubricant for mesh plates and an antifoaming leveling agent, a wear-inhibiting lubricating dispersion is produced, and mixed, stirred, and dispersed with other materials to form a low-VOC screen printing ink to ensure uniform dispersion of the mesh plates. and wear resistance.

Benefits of technology

It achieves stable batch production of low-VOC screen printing inks, suppresses mesh plate wear for a long time, maintains printing quality, reduces the frequency of screen plate replacement and ink adjustment, and reduces time and cost consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978984310000141
    Figure BDA0004978984310000141
  • Figure BDA0004978984310000151
    Figure BDA0004978984310000151
Patent Text Reader

Abstract

The present invention provides a manufacturing method which is characterized by comprising a step for mixing, stirring and dispersing materials containing at least a thermoplastic resin, a volatile organic solvent (VOC), a defoaming leveling agent, and a wear-inhibiting lubricant for a screen plate, the mixing, stirring and dispersing step comprising: a step for producing a dispersion in which the thermoplastic resin, the volatile organic solvent, the defoaming leveling agent, and the wear-inhibiting lubricant for the screen plate are dispersed; and a process for producing a wear-inhibiting lubricant dispersion for a mesh plate by mixing, stirring and dispersing the wear-inhibiting lubricant for a mesh plate and the defoaming leveling agent in advance, and mixing and stirring the wear-inhibiting lubricant dispersion for a mesh plate with another material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing screen printing ink, wherein the screen printing ink is a screen printing ink widely used for forming decorations and image patterns in the fields of charts, display panels and signs, and electrical / electronic components. In particular, in order to impart good continuous printing adaptability, a lubricating component is added to the ink to prevent wear on the mesh plate during large-scale screen printing, thereby obtaining a consistently stable desired printing effect of decoration, image pattern, and hue. Background Art

[0002] In recent years, the adverse effects of volatile organic solvents (hereinafter referred to as "VOCs") on the global environment and human body have become a major issue. For example, a movement to suppress the emission of VOCs to the global environment is being actively carried out through the implementation of the National Standard of the People's Republic of China "GB 30981-2020".

[0003] Under such circumstances, in the ink field, in order to meet the VOC mixing amount limit values ​​specified in "GB 30981-2020", activities to develop and market various ink products with lower VOC mixing ratios than before (hereinafter referred to as "low-VOC type") are accelerating.

[0004] However, in such low-VOC inks, the VOC blending ratio is reduced, and the VOC contributing to solubility and affinity is reduced, making the viscosity of the ink higher. Therefore, the printing method using a higher printing pressure than before is often adopted, which makes it easy to wear the printing mesh plate during printing. A method of adding an additive that reduces abrasiveness to prevent the wear of the printing mesh plate during mass production printing using the ink is studied, thereby stably maintaining the quality of the printing mesh plate and performing image printing with high precision.

[0005] On the other hand, in the above-mentioned low-VOC type ink, due to the reduction of VOC usage, the dispersion of the additive for reducing abrasion into the target raw material is uneven, and the wear resistance performance becomes insufficient. In similar manufacturing methods, the uniform dispersion of powder materials such as wear-resistant additives added in small amounts is insufficient, and it is difficult to ensure the mass production stability of printed and coated products using the ink.

[0006] In the prior art, when continuous mass printing is performed using screen printing, the wear of the printing mesh plate becomes a problem, and the possibility of poor film thickness and pattern is greatly increased, so the printing mesh plate must be discarded after only a few thousand sheets are printed. Alternatively, in order to reduce the wear of the printing mesh plate, countermeasures such as emulsion hardening treatment need to be taken during the mesh plate manufacturing process.

[0007] However, when using the emulsion hardening treatment method, the screen mesh cannot be reused, or the screen needs to be re-made frequently, which will increase the manufacturing cost of screen printing and increase the environmental load.

[0008] Therefore, now, in the mass production printing process, in order to prevent manufacturing defects caused by friction damage of the screen printing mesh plate, it is necessary to prepare more screens than before, or to ensure sufficient dispersion of additives used to reduce mesh plate friction, which requires more time, labor and cost than before.

[0009] Of course, the same problems as mentioned above also arise in low-VOC screen printing inks, which are a type of ink. In particular, in order to achieve mass production stability during screen printing, that is, to suppress the wear of the mesh plate and obtain a consistently stable printing of the desired decoration or image pattern, an ink is needed that can achieve high and stable printing and has an effect of suppressing mesh plate emulsion wear.

[0010] Therefore, in order to avoid the readjustment process during the ink manufacturing process (for example, adding VOC again during the mass production of low-VOC screen printing ink, or adding a redispersion process, etc.), while ensuring the batch stability of the ink during printing, it is strongly desired to create a novel and innovative manufacturing method that can achieve sufficient uniform dispersion of wear-resistant additives, that is, even if the screen printing ink is low-VOC, the wear of the mesh plate can be always stably suppressed, thereby obtaining the desired fine and stable printing of decoration and image patterns.

[0011] Here, the phenomenon of printing defects caused by the wear of the screen printing mesh plate during mass screen printing is described.

[0012] If the effect of suppressing mesh plate wear is lower than that of the prior art, the wear of the screen mesh and emulsion during mass production printing may cause jagged edges of the printed image, or insufficient leveling may occur due to changes in ink extrusion, thereby damaging the smoothness of the image surface.

[0013] In the existing patent documents 1 and 2, screen printing plates that can effectively prevent printing defects are reported, and the use of emulsions or photosensitive resins with excellent wear resistance, or a lamination method with a two-layer structure is disclosed to suppress the wear of the printing mesh plate. These patent documents also reveal the importance of suppressing the wear of the screen. On the other hand, the current situation is that no existing document discloses a method for highly stably ensuring the friction suppression performance of the screen in the manufacturing process of low-VOC screen printing ink.

[0014] The present invention is proposed based on the above, and it can manufacture screen printing inks with more diverse mixing, maintain the good stability of the printing mesh plate by uniformly dispersing the printing mesh plate wear resistance agent and other materials, and can also form the desired decoration and image patterns with high stability during mass production printing.

[0015] Prior art literature

[0016] Patent Literature

[0017] Patent Document 1: Japanese Patent Application Laid-Open No. 2009-274323

[0018] Patent document 2: Japanese Patent Application Laid-Open No. 2022-107073 Summary of the invention

[0019] Problems to be solved by the invention

[0020] The present invention is proposed in view of the above-mentioned problems, and provides a method for manufacturing ink for screen printing, which prevents the scraper from abrading against the mesh and emulsion constituting the mesh plate during mass production printing, thereby maintaining a constant decoration and image pattern during batch printing. Even in batch printing production, a pattern can always be formed stably, and the hue change caused by the change in film thickness can be stabilized.

[0021] Means for solving problems

[0022] The present invention is a method for producing screen printing ink, characterized by comprising the steps of mixing, stirring and dispersing materials,

[0023] The material at least comprises a thermoplastic resin, VOC, a defoaming and leveling agent, and a wear-inhibiting lubricant for a mesh plate.

[0024] The mixing, stirring and dispersing process comprises:

[0025] a dispersion preparation step of separately mixing, stirring and dispersing the mesh plate wear-inhibiting lubricant and the defoaming and leveling agent in advance to prepare a mesh plate wear-inhibiting lubricant dispersion, and

[0026] The mesh plate wear inhibiting lubricant dispersion is mixed and stirred with other materials.

[0027] Effects of the Invention

[0028] The manufacturing method of the present invention realizes the stable batch production of low-VOC screen printing ink, and can suppress the wear of the mesh plate for a long time, so that the mesh plate can always be kept in a normal state during the batch production printing process. Therefore, there is no need to frequently replace the mesh plate due to the wear of the mesh plate, and there is no need to readjust the ink dispersion during the batch production printing process, so that the decoration and image pattern printing output can be kept constant during the batch printing production process, solving the serious problems of time, labor and cost consumption faced by batch production printing in the past. DETAILED DESCRIPTION

[0029] As described above, the present invention is a method for producing a low-VOC screen printing ink, characterized in that it comprises the steps of mixing, stirring and dispersing the materials,

[0030] The material at least comprises a thermoplastic resin, VOC, a defoaming and leveling agent, and a wear-inhibiting lubricant for a mesh plate.

[0031] The mixing, stirring and dispersing process comprises:

[0032] a dispersion preparation step of separately mixing, stirring and dispersing the mesh plate wear-inhibiting lubricant and the defoaming and leveling agent in advance to prepare a mesh plate wear-inhibiting lubricant dispersion, and

[0033] The mesh plate wear inhibiting lubricant dispersion is mixed and stirred with other materials.

[0034] Furthermore, the present invention is a method for manufacturing a low-VOC screen printing ink, characterized in that in the above-mentioned wear-inhibiting lubricating dispersion for mesh plates, the mixing weight ratio of the wear-inhibiting lubricant for mesh plates and the defoaming and leveling agent is 1:10 to 3:1, the mixing and stirring during the manufacture of the dispersion and the temperature during dispersion are in the range of 20 to 90°C, and the dispersion manufacturing process is performed by grinding and dispersing twice using a three-roll disperser.

[0035] Furthermore, the present invention is a method for producing a low-VOC screen printing ink, characterized in that in the above-mentioned wear-inhibiting lubricating dispersion for the mesh plate, the wear-inhibiting lubricant for the mesh plate is a micronized wax powder having a melting point of 50 to 130°C at 25°C, and the defoaming and leveling agent is silicone oil or acrylic polymer / vinyl ether polymer / aliphatic ester, paraffin hydrocarbon, or olefin polymer having a pour point of -100°C to -10°C.

[0036] Furthermore, the present invention is a method for producing a low-VOC screen printing ink, characterized in that, relative to the total weight of the low-VOC screen printing ink, the thermoplastic resin is 5 to 70 wt% and is any one of acrylic resin, vinyl chloride-vinyl acetate resin, polyester resin, urethane resin, epoxy resin, and melamine resin, or a combination thereof, the VOC is 20 to 60 wt% and has a boiling point in the range of 100 to 300° C., and is any one of ketone solvent, ester solvent, ether solvent, aromatic hydrocarbon solvent, aliphatic hydrocarbon solvent, polyol solvent, and carboxylic acid solvent, or a combination thereof, the coloring pigment is 0 to 60 wt%, the body pigment is 0 to 60 wt%, and the wear-inhibiting lubricating dispersion for the mesh plate is 0.5 to 5 wt%.

[0037] Furthermore, the present invention is a method for producing a low-VOC screen printing ink, characterized in that the ink or the dispersion is produced by a mixer and a three-roll disperser equipped with a VOC scattering prevention sealing cover having an opening and closing portion, and the area of ​​the opening and closing portion is less than 1 / 3 of the contact area between the VOC scattering prevention sealing cover and the air, and the area of ​​the opening and closing portion is 400 cm 2 above.

[0038] The thermoplastic resin used in the manufacturing method of the present invention is not particularly limited. However, in the low-VOC screen printing ink for decoration and image pattern formation, which is widely used in the fields of graphics, display panels and signs, and electric / electronic components, plastics, glass, and metals are often used as printed materials. In order to maintain strong adhesion to these printed materials, durability against long-term use, and weather resistance, the above-mentioned thermoplastic resin is appropriately selected in consideration of the type and purpose of the printed material, and is preferably an acrylic resin (commercially available example: DOW CHEMICAL COMPANY LIMITED / PARALOID series, Mitsubishi Rayon Co., Ltd. / Diyanal series), vinyl chloride-vinyl acetate resins (commercially available examples: Nissin Chemical Industry Co., Ltd. / Solbiin series, Kaneka Co., Ltd. / Kanebiinal series), polyester resins (commercially available examples: Nippon Yupika Co., Ltd. / Yupika series, Tokyo Bosho Co., Ltd. / Bilon series), urethane resins (commercially available examples: : Tokyo Bosho Co., Ltd. / Bilon UR series, DIC Biel Polymer Co., Ltd. / PANDEX series), epoxy resins (commercially available examples: Mitsui Chemicals, Inc. / Epoxy series, Mitsubishi Chemical Co., Ltd. / jER series), melamine resins (commercially available examples: Showa Denko Materials Co., Ltd. / Melan series, Mitsui Science Co., Ltd. / Simelu series) or any one thereof or a combination thereof.

[0039] The weight average molecular weight of such a thermoplastic resin is preferably 4,000 to 200,000, more preferably 6,000 to 150,000, and even more preferably 8,000 to 100,000.

[0040] If the weight average molecular weight is less than 4,000, the low-VOC screen printing ink coating film is likely to have poor chemical resistance and weather resistance.

[0041] On the other hand, when the weight average molecular weight exceeds 200,000, the solubility in VOC deteriorates, and a large amount of VOC is required to dissolve the thermoplastic resin, making it difficult to produce a low-VOC screen printing ink.

[0042] The amount of such a thermoplastic resin blended is preferably 5 to 70 wt %, more preferably 7 to 60 wt %, and even more preferably 10 to 50 wt % based on the total weight of the low-VOC screen printing ink.

[0043] If the blending amount is less than 5 wt %, the chemical resistance and weather resistance of the low-VOC screen printing ink coating film are poor, and the adhesion to the printed object is deteriorated.

[0044] On the other hand, if the blending amount exceeds 70 wt %, the viscosity of the low-VOC screen printing ink becomes extremely high, and the ink becomes unsuitable for good screen printing.

[0045] The VOC used in the manufacturing method of the present invention is not particularly limited, but in the low-VOC screen printing ink, considering the required solubility in thermoplastic resins and the flow stability on the screen printing plate, it is preferred to contain 20 to 60 wt% of any one of ketone solvents, ester solvents, ether solvents, aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, polyol solvents, and carboxylic acid solvents (trade name example DBE) with a boiling point of 100 to 300°C relative to the total weight of the low-VOC screen printing ink or a combination thereof.

[0046] Here, the boiling point of the VOC is more preferably 120 to 270°C, and further preferably 140 to 250°C.

[0047] Furthermore, the VOC blending amount is more preferably 22 to 55 wt %, and further preferably 25 to 50 wt %.

[0048] If the boiling point of VOC is lower than 100° C., the drying and scattering of VOC from the low-VOC screen printing ink on the screen printing plate will be accelerated, thereby causing problems in stable mass production screen printing.

[0049] On the other hand, if the boiling point of VOC is higher than 300° C., the drying and dispersion of VOC from the printed low-VOC screen printing ink coating film will be extremely slow, resulting in a disadvantage that a large amount of energy and time will be required to dry the coating film.

[0050] If the VOC content is less than 20 wt %, the thermoplastic resin cannot be sufficiently dissolved, or the viscosity of the low-VOC screen printing ink increases, thereby causing a problem in which good screen printing cannot be performed.

[0051] On the other hand, if the VOC content is greater than 60 wt %, the VOC content does not comply with the National Standard of the People's Republic of China "GB 30981-2020 (Limits of Hazardous Substances for Industrial Protective Inks)".

[0052] Specific examples of VOCs used in the production method of the present invention include butyl cellosolve acetate, a mixed solvent containing dialkyl adipate (a carboxylic acid solvent, and a commercially available example is "Flexisolv DBE"), isophorone, 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, coal tar naphtha having a boiling point exceeding 170°C, diethylene glycol monoethyl ether (acetate), diethylene glycol monobutyl ether, triethylene glycol monobutyl ether (acetate), cyclohexanone, coal tar naphtha having a boiling point of 160 to 170°C, mineral spirits having a boiling point of 150 to 170°C, 1-methoxy-2-propanol, 1-methoxypropyl-2-acetate, diacetone alcohol, and the like.

[0053] In the manufacturing method of the present invention, there is no particular limitation as long as the coloring pigment and / or the extender pigment can be used at 0 to 60 wt% relative to the total weight of the low-VOC screen printing ink, can be dispersed by a disperser such as a three-roll disperser, and does not cause undesirable phenomena such as a particle size greater than the mesh screen opening diameter. The mixing amount of the coloring pigment and / or the extender pigment is preferably 0 to 60 wt%, more preferably 0 to 55 wt%, and further preferably 0 to 50 wt% relative to the total weight of the low-VOC screen printing ink.

[0054] In addition, the purpose of using coloring pigments is to obtain desired coloring properties, and extender pigments are used to adjust to suitable fluidity and partially replace conventional expensive coloring pigments.

[0055] When producing a colorless and transparent low-VOC screen printing ink, a high degree of colorlessness and transparency can be ensured by setting the blending amount of the coloring pigment and / or the extender pigment to 0 wt %.

[0056] On the other hand, if the desired blending amount of the coloring pigment and / or the extender pigment exceeds 60 wt %, the solid content ratio is too high, making it difficult to uniformly disperse the pigment using a disperser or to perform screen printing.

[0057] Examples of the coloring pigment include azo pigments, disazo pigments, disazo pigments, phthalocyanine pigments, anthraquinone pigments, isoindoline pigments, dihydronaphthalene pigments, Oxazine pigments, quinacridone pigments, perylene pigments, carbon black pigments, lake black pigments, perylene black pigments, aniline black pigments, iron oxide pigments, titanium pigments, zinc sulfide pigments, etc., and one or more of them can be used in combination. In addition, various color dyes can be used for coloring as needed.

[0058] Examples of the extender pigment include silica, talc, calcium carbonate, magnesium carbonate, bentonite, precipitated barium sulfate, zinc oxide, aluminum oxide, and the like, and these may be used alone or in combination.

[0059] Furthermore, in the manufacturing method of the present invention, fillers such as resin beads, metal particles, metal powder, metal oxide powder, graphite, pearlescent pigments, fluorescent pigments, wax particles, protein powder, and ultraviolet absorbing materials, antibacterial materials, heat absorbing materials, refractive index adjusting materials, slip imparting materials, slip preventing materials, light storing materials, polarizing materials, antireflection materials, diffusing materials, etc. can also be mixed. For the same reasons as above, it is sufficient to use an appropriate amount in the range of 0 to 60wt% relative to the total weight of the low-VOC screen printing ink, more preferably 0 to 55wt%, and even more preferably 0 to 50wt%.

[0060] The manufacturing method of the present invention must contain a defoaming leveling agent and a wear-inhibiting lubricant for mesh plates, but the method of the present invention is different from the manufacturing method that has been used so far. In the conventional method, the defoaming leveling agent and the wear-inhibiting lubricant for mesh plates are measured separately and added together with other materials, mixed and stirred, and then dispersed. The manufacturing method of the low-VOC screen printing ink of the present invention is characterized in that the wear-inhibiting lubricant for mesh plates and the defoaming leveling agent are mixed, stirred and dispersed separately in advance to produce a wear-inhibiting lubricant dispersion for mesh plates, and then the wear-inhibiting lubricant dispersion for mesh plates is weighed, added, mixed and stirred with other materials, and then dispersed.

[0061] The inventors of the present invention have found that by using such a wear-inhibiting lubricating dispersion for mesh plates found through a new concept in the manufacturing process of low-VOC screen printing ink, it is possible to easily ensure that the wear-inhibiting lubricant for mesh plates is fully and evenly dispersed in the low-VOC screen printing ink, and thus it is possible to stably mass-produce low-VOC screen printing inks that can continue to maintain the normal production state of the printing plate even during mass printing production. The ink produced by it can suppress the wear of the mesh plate for a long time during the mass production printing process, and always keep the mesh plate in a normal state during the mass production printing process. Therefore, there is no need to frequently replace the mesh plate due to the wear of the mesh plate, and there is no need to readjust the ink dispersion during the mass production printing process, and thus a constant decorative and image pattern printing output is maintained during the mass printing production process, solving the serious problems of time, labor and cost consumption faced by mass production printing in the past.

[0062] In addition, the problem of unstable wear resistance of printing mesh plates during mass production due to insufficient dispersion of the wear-reducing lubricant for mesh plates is described in the first paragraph from the bottom on page 2 and the first paragraph on page 3 of the present specification.

[0063] Here, the reasons why the wear-inhibiting lubricant dispersion for mesh plates is prepared by using the wear-inhibiting lubricant for mesh plates and the defoaming and leveling agent are explained as follows:

[0064] Low VOC screen printing ink contains at least thermoplastic resin, VOC, defoaming and leveling agent and mesh plate wear inhibiting lubricant, but since the thermoplastic resin is solid, it is not easy to mix and stir and disperse it evenly with the mesh plate wear inhibiting lubricant. The same is true for coloring pigments, extender pigments, fillers, etc. that can be contained in low VOC screen printing ink.

[0065] In addition, since VOC has low viscosity, it is difficult to disperse it using a disperser. In addition, there is a problem that part of VOC is easily volatilized during the production process of the wear-reducing lubricant dispersion for mesh plates.

[0066] In addition, it has been considered to add a wear-inhibiting lubricant for mesh plates to a resin varnish prepared by dispersing and dissolving a thermoplastic resin in VOC, but VOC will partially volatilize during the varnish manufacturing process. In addition, depending on the type of low-VOC screen printing ink, the types of thermoplastic resins and VOCs used are various. In addition, the viscosity of the resin varnish is also different. Therefore, it is necessary to prepare many types of wear-inhibiting lubricant dispersions for mesh plates, which will seriously affect the manufacturing production efficiency.

[0067] In view of the above situation, the inventors of the present invention have repeatedly thought about and experimented and found that the most suitable way to manufacture a wear-inhibiting lubricating dispersion for mesh plates is to mix it with a defoaming and leveling agent that contains almost no VOC, has low viscosity and moderate viscosity, and is commonly used in many types of low-VOC screen printing inks.

[0068] Regarding the mesh plate wear-inhibiting lubricant dispersion in the production method of the present invention, the blending weight ratio of the mesh plate wear-inhibiting lubricant to the defoaming and leveling agent is preferably 1:10 to 3:1, more preferably 1:6 to 2:1, and even more preferably 1:3 to 1:1.

[0069] If the mixing weight ratio of the wear-inhibiting lubricant for mesh plates to the defoaming and leveling agent is lower than 1:10, when manufacturing low-VOC screen printing ink and adding the required amount of friction-inhibiting lubricant dispersion, the defoaming agent content ratio will be too high, and poor adhesion of the low-VOC screen printing ink coating to the printed object will easily occur.

[0070] On the other hand, if the mixing weight ratio of the wear inhibiting lubricant for mesh plates to the defoaming and leveling agent is greater than 3:1, the ratio of the defoaming and leveling agent is too small, the viscosity of the wear inhibiting lubricant dispersion for mesh plates is too high during production, and poor dispersion is likely to occur, making production difficult.

[0071] The temperature during mixing and stirring and dispersion during the production of such a wear-inhibiting lubricant dispersion for mesh plates is preferably within the range of 20 to 90° C., more preferably 30 to 90° C., further preferably 35 to 75° C., and further preferably 40 to 60° C., and it is desirable to perform grinding and dispersion twice using a three-roll disperser. By producing the wear-inhibiting lubricant dispersion for mesh plates within the above temperature range, the agglomeration of the wear-inhibiting lubricant for mesh plates can be easily eliminated, and low-VOC screen printing ink can be supplied more stably.

[0072] If the temperature is lower than 20° C., aggregation of the wear-inhibiting lubricant for a mesh plate may not be sufficiently eliminated, or more time may be required for sufficient dispersion.

[0073] On the other hand, if the temperature is higher than 90° C., a high boiling point solvent, a lubricant, and VOC contained in a small amount in the defoaming and leveling agent may be scattered, and the defoaming and leveling function may not be fully exhibited.

[0074] The mixing and stirring process during the manufacture of the wear-inhibiting lubricating dispersion for mesh plates can usually be performed using a blade mixer or a vibration mixer under appropriate shear conditions for about 15 to 60 minutes.

[0075] On the other hand, in the dispersion process, a bead mill or a three-roll disperser can be generally used as a disperser, but according to experimental studies by the present inventors, it has been found that a three-roll disperser is more suitable.

[0076] The reason is still uncertain, but it is presumed that the dispersion principle of the three-roll disperser, such as the fracture stress and shear stress, improves the wettability of the mesh plate wear suppressing lubricant and the defoaming and leveling agent, thereby suppressing the reaggregation of the mesh plate wear suppressing lubricant.

[0077] The above describes a suitable device for mixing, stirring and dispersing the wear-inhibiting lubricant dispersion for mesh plates. This device is also applicable to the production process of low-VOC screen printing ink.

[0078] Wax powders used as wear-inhibiting lubricants for mesh plates in the manufacturing method of the present invention include amides, polyethylene waxes, waxes, paraffin waxes (commercially available examples: CERAFLUOR series from Bicchemie Japan, AQUACER series from Bicchemie Japan, Luwax series from BASF, Paraffin Wax series from Nippon Seira Co., Ltd.), etc. However, in order to reduce the excellent wear resistance of the plate, it is preferred to use wax powders having a melting point of 50 to 130°C.

[0079] If the melting point of such a wear-inhibiting lubricant for mesh plates is lower than 50°C, it will have an adverse effect on the uniform dispersibility when manufacturing the wear-inhibiting lubricant dispersion for mesh plates. In addition, if the melting point of the wear-inhibiting lubricant for mesh plates exceeds 130°C, it will be difficult for a low-VOC screen printing ink to which the wear-inhibiting lubricant dispersion for mesh plates is added to obtain excellent wear resistance to the mesh plates.

[0080] Examples of the defoaming and leveling agent used in the production method of the present invention include silicone oil, polysiloxane derivatives (commercially available examples: Shin-Etsu Chemical Co., Ltd. / KF, KS series, Bic Chemi Japan Co., Ltd. / BYK series), fluorine-based surfactants, high molecular weight acrylic polymer derivatives, vinyl ether polymers, aliphatic esters, paraffin hydrocarbons, olefin polymers, and high boiling point polyether compounds (AGC Seimi Chemi Kalu Co., Ltd. / Sarfluon series, Kyoeisha Chemical Co., Ltd. / Florlen series), etc. However, in order to achieve a variety of good defoaming effects and leveling effects for various types of low-VOC screen printing inks by adding as little as possible, silicone oil is preferred and has a pour point of -100°C to -10°C, more preferably -90°C to -30°C, and even more preferably -85°C to -35°C.

[0081] If the pour point of such a defoaming and leveling agent is less than -100°C, the viscosity of the leveling agent generally circulated in the market becomes small, making it difficult to disperse the wear-inhibiting lubricant for mesh plates, and it is difficult to obtain the defoaming and leveling effect brought about by adding a small amount. On the other hand, if the pour point is greater than -10°C, when the low-VOC screen printing ink is placed at low temperatures during the manufacturing, printing, and storage process, it will have an adverse effect on the dispersion of the wear-inhibiting lubricant for mesh plates, making it difficult to stably provide high-quality low-VOC screen printing inks.

[0082] Here, the suitable addition amount of the above-mentioned wear-inhibiting lubricant dispersion for mesh plate is 0.5wt% as the lower limit, preferably 1.0wt%, more preferably 1.9wt%, and further preferably 2.0wt% relative to the total weight of the low-VOC screen printing ink, and the upper limit is 5.3wt%, preferably 5.0wt%, more preferably 4.0wt%, and further preferably 3.0wt%. In addition, the mixing weight ratio of the wear-inhibiting lubricant for mesh plate and the defoaming and leveling agent in the wear-inhibiting lubricant dispersion for mesh plate is preferably 1:10 to 3:1. Therefore, in the above-mentioned wear-inhibiting lubricant dispersion for mesh plate of 0.5 to 5.3wt%, the addition amount of the wear-inhibiting lubricant for mesh plate relative to the total weight of the low-VOC screen printing ink is in the range of 0.045 to 3.97wt%, and similarly, the addition amount of the defoaming and leveling agent is in the range of 0.125 to 4.82wt%.

[0083] If the amount of the wear-inhibiting lubricant for mesh plates added is too small (for example, when the amount of the wear-inhibiting lubricant dispersion for mesh plates is less than 0.5 wt % relative to the total weight of the low-VOC screen printing ink and the weight ratio of the wear-inhibiting lubricant for mesh plates to the defoaming and leveling agent is 1:10, the amount of the wear-inhibiting lubricant for mesh plates added is less than 0.045 wt %), it is difficult to achieve the desired mesh plate wear-inhibiting effect. On the other hand, if the amount of the defoaming and leveling agent added is too large (for example, when the amount of the wear-inhibiting lubricant dispersion for mesh plates is more than 5.3 wt % relative to the total weight of the low-VOC screen printing ink and the weight ratio of the wear-inhibiting lubricant for mesh plates to the defoaming and leveling agent is 1:10, the amount of the defoaming and leveling agent added exceeds 4.82 wt %), poor adhesion to the printed body is likely to occur.

[0084] Furthermore, the inventors of the present invention have repeatedly conducted experimental studies and have proved that, in the manufacturing method of the present invention, the low-VOC screen printing ink can be manufactured more stably and with high quality in the following case, that is, the low-VOC screen printing ink and the wear-inhibiting lubricating dispersion for mesh plates are manufactured by a mixer and a three-roll disperser equipped with a VOC scattering prevention sealing cover with an opening and closing part, and the area of ​​the opening and closing part is less than 1 / 3 of the area of ​​the sealing cover in contact with air and is 400 cm2 above.

[0085] If the area of ​​the opening and closing part exceeds 1 / 3 of the area where the sealing cover is in contact with the air, the VOC dispersion in the low-VOC screen printing ink or the wear-inhibiting lubricant dispersion for mesh plates will exceed 0.5wt% of the total amount, which will cause VOC environmental emission problems and will have a subtle effect on the uniform dispersion, thixotropy, and flow characteristics of the wear-inhibiting lubricant for mesh plates in the low-VOC screen printing ink.

[0086] On the other hand, if the area of ​​the opening and closing portion is less than 400 cm 2 , it becomes difficult to add various additives required in the process, and it becomes difficult to take small samples of low-VOC screen printing inks or wear-inhibiting lubricating dispersions for mesh plates for inspection during manufacturing and to return the inspection samples.

[0087] In addition, the shape of the opening and closing part is preferably a suitable shape such as a square, a circle, or a semicircle that the operator can easily operate. In addition, there is no particular problem whether the opening and closing mechanism of the opening and closing part is a folding type or a sliding type.

[0088] Example

[0089] Hereinafter, Examples of the present invention and Comparative Examples are shown in [Table 1]. In addition, the present invention is not limited to these Examples.

[0090]

[0091]

[0092] First, the wear-inhibiting lubricating dispersion for a mesh plate described in the present invention is produced as follows.

[0093] The wear-inhibiting lubricant and defoaming leveling agent for mesh plates described in Table 1 were uniformly mixed and stirred using a blade stirrer, and then passed through a three-roll disperser twice to be uniformly ground and dispersed.

[0094] Here, the mixing ratio of the wear-inhibiting lubricant for mesh plates and the defoaming and leveling agent, the temperature during production, and the presence or absence of the VOC scattering prevention sealing cover having an opening and closing portion described in the present invention are as shown in Table 1.

[0095] Next, the low-VOC screen printing ink described in the present invention is produced as follows.

[0096] The prescribed materials listed in Table 1 were uniformly mixed and stirred using a blade stirrer, and then passed through a three-roll disperser twice to be uniformly ground and dispersed.

[0097] Here, the mixing ratio of the specified materials and the presence or absence of the VOC dispersion prevention sealing cover with an opening and closing portion described in the present invention are as described in Table 1. In addition, the sealing cover of the blade type mixer is used to open the opening diameter of 1m (area 7,850cm 2 ) of a cylindrical stirring container having a sealed lid, on which a 2,512 cm 2 The semicircular opening and closing part of the three-roll disperser is used to 2 The rectangular opening is sealed with a cover having an area of ​​6,000 cm 2 A rectangular opening and closing portion.

[0098] In addition, the examples are examples in which the wear-inhibiting lubricant dispersion for mesh plates described in the present invention is blended, and the comparative examples are examples in which the wear-inhibiting lubricant for mesh plates and the defoaming and leveling agent are blended and used separately.

[0099] In addition, mass production printing of low-VOC screen printing ink was performed as follows.

[0100] The low-VOC screen printing ink of the embodiment and the comparative example is screen-printed on the printed object listed in Table 1 using a 360-mesh screen with a wire diameter of 25 μm. The mesh used in the screen is a calendered mesh with a mesh thickness of 29 μm and an opening ratio of 42%. The screen emulsion is 15 μm thick and the emulsion surface is smoothed.

[0101] The screen printing conditions at this time are: scraper hardness 80 degrees (material is urethane), screen gap 5mm, scraper printing pressure is pressed into the screen 1.5mm, scraper angle 75 degrees, scraper speed 150mm / second, and ink return knife pressure is pressed into the screen 1.5mm.

[0102] Furthermore, in the verification of this example, in order to reduce the influence on the final product caused by the volatilization of VOC during continuous printing, the abrasion resistance of the plate was appropriately evaluated, and the ink on the plate was replaced every 500 sheets.

[0103] In addition, as a printing image design, at least a 100 μm vertical and horizontal fine line pattern parallel or perpendicular to the printing direction and a square solid pattern with one side of 100 mm coexist in the screen printing plate.

[0104] The evaluation of the quality of printed matter in the above-mentioned mass production printing was performed as follows.

[0105] The 20th, 600th, 2,100th, 3,100th, 5,100th, and 7,600th prints from the start of mass production printing were compared with the second print from the start of mass production printing, and the changes and stability of the printed images were evaluated in the "◎, ○, △, X" format described below. In addition, the reason for not comparing and evaluating the first print from the start of mass production is that the wettability of the first screen printing plate and ink is poor, and the first print from the start of printing is prone to print image defects.

[0106] The quality of the printed image was evaluated based on accurate transferability (no transfer or bleeding of patterns other than the intended pattern) to a 100 μm vertical and horizontal fine line pattern and a 100 mm square solid pattern.

[0107] ◎: Observed using an 8x magnifying glass and compared with the second print, both the fine lines and the solid pattern were of equivalent quality.

[0108] ○: Observed using an 8x magnifying glass and compared with the second print, there was no significant difference in the fine lines and solid pattern.

[0109] △: Visual observation revealed that both fine lines and solid patterns were of comparable quality compared to the second print. However, observation using an 8x magnifying glass revealed that bleeding and transfer occurred compared to the second print.

[0110] ×: Visual observation revealed that both the thin lines and the solid pattern had bleeding and transfer as compared with the second printed product.

[0111] As can be seen from Table 1, by adopting the manufacturing method of the present invention using the wear-inhibiting lubricating dispersion for mesh plates described in the present invention, the wear-inhibiting effect of low-VOC screen printing ink on the mesh plates can be kept sufficiently stable during mass production printing, thereby ensuring the stability of batch printing quality without the need to remake and replace the screen, thereby saving a lot of time, labor and cost.

Claims

1. A method for producing screen printing ink, characterized in that: It has the process of mixing, stirring and dispersing the materials. The material at least comprises a thermoplastic resin, a VOC (volatile organic solvent), a defoaming and leveling agent, and a wear-inhibiting lubricant for a mesh plate. The mixing, stirring and dispersing process comprises: a dispersion preparation step of separately mixing, stirring and dispersing the mesh plate wear-inhibiting lubricant and the defoaming and leveling agent in advance to prepare a mesh plate wear-inhibiting lubricant dispersion, and The mesh plate wear inhibiting lubricant dispersion is mixed and stirred with other materials.

2. The method for producing screen printing ink according to claim 1, characterized in that: In the wear-inhibiting lubricating dispersion for mesh plates, the weight ratio of the wear-inhibiting lubricant for mesh plates to the defoaming and leveling agent is in the range of 1:10 to 3:

1.

3. The method for producing screen printing ink according to claim 1, characterized in that: The temperature during mixing, stirring and dispersing in the dispersion production step is in the range of 20 to 90°C.

4. The method for producing screen printing ink according to claim 1, characterized in that: In the dispersion production step, grinding and dispersion are performed twice using a three-roll disperser.

5. The method for producing a screen printing ink according to any one of claims 1 to 4, characterized in that: In the wear-inhibiting lubricating dispersion for mesh plates, the wear-inhibiting lubricant for mesh plates is a micronized wax powder having a melting point of 50 to 130°C at 25°C, the defoaming and leveling agent is a silicone oil or polysiloxane derivative with a pour point of -100°C to -10°C, a fluorine-based surfactant, an acrylic polymer / vinyl ether polymer / aliphatic ester, a chain alkane hydrocarbon, or an olefin polymer, and the thermoplastic resin is any one of acrylic resin, vinyl chloride-vinyl acetate resin, i.e., vinyl chloride-vinyl acetate copolymer resin, polyester resin, urethane resin, epoxy resin, and melamine resin, or a combination thereof.

6. The method for producing a screen printing ink according to any one of claims 1 to 4, characterized in that: Relative to the total weight of the screen printing ink, the thermoplastic resin is 5 to 70 wt%, and is any one of acrylic resin, vinyl chloride-vinyl acetate resin, i.e., vinyl chloride-vinyl acetate copolymer resin, polyester resin, urethane resin, epoxy resin, and melamine resin, or a combination thereof; the VOC is 20 to 60 wt%, and has a boiling point of 100 to 300° C. and is any one of ketone solvent, ester solvent, ether solvent, aromatic hydrocarbon solvent, aliphatic hydrocarbon solvent, polyol solvent, and carboxylic acid solvent, or a combination thereof; the coloring pigment is 0 to 60 wt%, the body pigment is 0 to 60 wt%, and the wear-inhibiting lubricating dispersion for the mesh plate is 0.5 to 5 wt%.

7. The method for producing a screen printing ink according to any one of claims 1 to 4, characterized in that: The invention is produced by a mixer and a three-roll disperser equipped with a VOC dispersion prevention sealing cover having an opening and closing portion, wherein the area of ​​the opening and closing portion is less than 1 / 3 of the area of ​​the sealing cover in contact with air and 400 cm 2 above.