Two-component flame retardant as well as preparation method and application thereof

Through the design of a two-component flame retardant, modified starch and aerogel are used to improve the water resistance, heat resistance and low temperature resistance of the flame retardant, and solve the intolerance problem of existing flame retardants in different environments. , and expanded its application to the construction field to achieve a wider range of fire protection effects.

CN118725656AActive Publication Date: 2024-10-01ASIA CUANON TECH SHANGHAI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410936701.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Existing flame retardants show intolerance in high temperature, low temperature and water environments, and their use areas are limited, making it difficult to effectively prevent the recurrence of forest and grassland fires and the occurrence of building fires.

Method used

A two-component flame retardant is used, including component A (starch phosphate, calcium chloride, surfactant, propylene glycol and aerogel) and component B (bone glue and water). Through the use of modified starch and aerogel, Improve the water resistance, heat resistance and low temperature resistance of flame retardants, and expand their application in the field of building exterior walls.

Benefits of technology

The water resistance, heat resistance and low temperature resistance of the flame retardant are significantly improved, ensuring effective fire protection under different environmental conditions, expanding its application scope and reducing safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004941541310000081
    Figure BDA0004941541310000081
  • Figure BDA0004941541310000091
    Figure BDA0004941541310000091
  • Figure BDA0004941541310000101
    Figure BDA0004941541310000101
Patent Text Reader

Abstract

The invention provides a two-component flame retardant as well as a preparation method and application thereof, and relates to the technical field of flame retardants. The double-component flame retardant comprises a component A and a component B, wherein the component A comprises starch phosphate, calcium chloride, a surfactant, propylene glycol, aerogel and water; wherein the component B comprises bone glue and water. The two-component flame retardant disclosed by the invention is green and environment-friendly, has no corrosivity, has no influence on plant growth, can be used on trees, leaves, paper, walls and insulation boards, and has excellent performance. The paint is used in rainy seasons in southern areas, cold areas in northern areas and hot areas in summer, is good in weather resistance, does not affect the product quality, and also can play a very good protection role.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardants, and in particular to a two-component flame retardant and a preparation method and application thereof. Background Art

[0002] Forest and grassland fires are a type of natural disaster that is sudden, destructive, and difficult to handle and rescue. Once a fire occurs, the losses to humans and the ecosystem are incalculable and the consequences are disastrous. In order to preserve more or more valuable forests and grasslands, isolation zones will be opened while extinguishing the fire to completely separate the burned area from the unburned area; at the same time, flame retardants will be sprayed on the surface of combustibles to make them difficult to burn or non-combustible, so as to prevent the fire from spreading further.

[0003] However, it is difficult for ordinary fire retardants to have a significant effect. Water-based flame retardants have low surface tension and better fluidity, but most of the water is often lost before it can play a role, resulting in low utilization rate and poor adhesion. Combustibles are easy to reignite under high temperature or smoldering conditions. Foam fire extinguishing agents are easily blown away by flame waves and strong winds due to their specific gravity. Dry powder fire extinguishing agents are more polluting to the environment, have poor flame retardant properties, are easily blown away by the wind when sprayed, and are difficult to adhere to the protected objects.

[0004] For example, CN101037601A discloses a special flame retardant liquid for forest and grassland fire prevention, which is a water-based emulsion made by mixing the following solid and liquid raw materials: alkaline earth metal salts, boric acid, refined quartz powder, powdered chlorinated paraffin, hollow microspheres, penetrants, urea, hydrosols, and animal bone activated carbon. However, there are still the following problems: 1. Water resistance. In view of the characteristics of more rain in the south, whether the water resistance of the flame retardant liquid sprayed on the plants after being rained on has been excellent has not been studied and explained. 2. Heat resistance. In hot and hot areas, whether the heat resistance of the flame retardant liquid sprayed on the plants after being exposed to the sun will fail has not been studied and explained. 3. Low temperature resistance. In the cold northern regions, whether the low temperature resistance of the flame retardant liquid sprayed on the plants after being frozen by rain has not been studied and explained. 4. The field of use is single, and it is only used in forests and grasslands, and cannot be used in the construction field.

[0005] Therefore, it is urgent to study a flame retardant with excellent water resistance, heat resistance and frost resistance, and expand its application field, which will be more conducive to solving the difficulties of product performance, reducing safety hazards, and ensuring human life safety, property safety and ecological balance.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a two-component flame retardant and its preparation method and application. The two-component flame retardant comprises component A and component B; wherein component A comprises starch phosphate, calcium chloride, surfactant, propylene glycol, aerogel and water; wherein component B comprises bone glue and water. The two-component flame retardant of the present invention has excellent water resistance, heat resistance, low temperature resistance and fire resistance; and expands the application field, and can also be used in the field of building exterior walls, effectively reducing safety hazards.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, the present invention provides a two-component flame retardant, the two-component flame retardant comprising component A and component B;

[0010] Wherein, the component A comprises starch phosphate, calcium chloride, a surfactant, propylene glycol, aerogel and water;

[0011] Wherein, the B component includes gelatin and water.

[0012] In the present invention, the components in the two-component flame retardant cooperate with each other and synergistically enhance the effectiveness, so that the water resistance, heat resistance, low temperature resistance and fire resistance of the flame retardant are significantly improved.

[0013] The added starch phosphate is a bio-based flame retardant that improves the fire resistance and adhesion of the flame retardant by changing the thermal stability and pyrolysis process of the starch itself. It is also a new modified starch mixture that uses phosphoric acid and urea to modify natural starch, and connects phosphorus and nitrogen to the molecular chain of starch to change the chemical properties of starch, making it a flame retardant gel containing acid source, carbon source and gas source. It has the ability to expand into carbon.

[0014] Among them, the added aerogel has the characteristics of mesh structure and low density. It is an effective thermal insulation material. It can not only improve the high temperature resistance effect, but also help plants maintain a stable growth environment under extreme temperature conditions, while eliminating harmful substances from plants and maintaining the structural integrity and healthy growth of plants.

[0015] Among them, the added surfactant has excellent surface activity, which can reduce the surface tension of the flame retardant, obtain excellent adhesion and water resistance, and thus improve the water resistance of the flame retardant.

[0016] Among them, the added propylene glycol lowers the freezing point of the flame retardant by mixing with water, thereby providing effective antifreeze protection, maintaining a liquid state without freezing at low temperatures, ensuring normal use, and making the flame retardant resistant to low temperatures.

[0017] Preferably, the component A comprises, by weight: 50-65 parts of starch phosphate, 10-15 parts of calcium chloride, 0.3-0.7 parts of surfactant, 0.5-1.0 parts of propylene glycol, 3-10 parts of aerogel and 15-25 parts of water.

[0018] In the A component, the content of starch phosphate is 50-65 parts, for example, it can be 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, etc. (Wherein, the starch phosphate is a yellow liquid material.)

[0019] In the A component, the content of calcium chloride is 10 to 15 parts, for example, 10 parts, 10.5 parts, 11 parts, 11.5 parts, 12 parts, 12.5 parts, 13 parts, 13.5 parts, 14 parts, 14.5 parts, 15 parts, etc. (wherein, calcium chloride is a white crystal, which can be calcium chloride dihydrate.)

[0020] In the component A, the content of the surfactant is 0.3 to 0.7 parts, for example, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts, 0.7 parts, etc.

[0021] In the component A, the content of propylene glycol is 0.5 to 1.0 parts, for example, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1.0 parts, etc. (The propylene glycol may be industrial 1,2-propylene glycol, with a content of ≥99.7%).

[0022] In the A component, the content of aerogel is 3 to 10 parts, for example, it can be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, etc.

[0023] In the component A, the content of water is 15 to 25 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, etc.

[0024] Preferably, the pH of the starch phosphate is 6 to 8, for example, 6, 6.5, 7, 7.5, 8, etc.

[0025] Preferably, the solid content of the starch phosphate is 30-50wt%, for example, 30wt%, 32wt%, 35wt%, 38wt%, 40wt%, 42wt%, 45wt%, 48wt%, 50wt% and the like.

[0026] Preferably, the surfactant is a water-resistant nonionic surfactant.

[0027] Preferably, the water-resistant nonionic surfactant is selected from any one or a combination of at least two of perfluoroalkyl polyoxyethylene ether, polyether-modified polysiloxane or fluoroalkyl polysiloxane, preferably Polyether modified polysiloxane .

[0028] Preferably, the surface tension of the surfactant is 20 to 30 mN / m, for example, 20 mN / m, 21 mN / m, 22 mN / m, 23 mN / m, 24 mN / m, 25 mN / m, 26 mN / m, 27 mN / m, 28 mN / m, 29 mN / m, 30 mN / m, etc.

[0029] Preferably, the aerogel is silicon dioxide nano-aerogel powder particles.

[0030] Preferably, the B component comprises, by weight: 15 to 30 parts of bone glue and 70 to 85 parts of water.

[0031] In the B component, the content of bone glue is 15 to 30 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.

[0032] In the B component, the water content is 70 to 85 parts, for example, it can be 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, etc.

[0033] Preferably, the bone glue is selected from animal bone glue (main components are gelatin and protein).

[0034] Preferably, the mass ratio of component A to component B is (3-5):1, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, etc., preferably 4:1.

[0035] In a second aspect, the present invention provides a method for preparing the two-component flame retardant as described in the first aspect, the preparation method comprising the following steps:

[0036] Mix starch phosphate, calcium chloride, a surfactant, propylene glycol, aerogel and water, and stir to obtain the component A;

[0037] The gelatin is dissolved in water and stirred to obtain the B component.

[0038] It should be noted that the flame retardant of the present invention is a two-component flame retardant. During the preparation process, the component A and the component B are first prepared separately, and then the component A and the component B are mixed during use.

[0039] Preferably, during the preparation of the component A, the stirring speed is 300-600 rpm, for example, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, etc.

[0040] Preferably, during the preparation of the component A, the stirring time is 15 to 20 min, for example, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, etc.

[0041] Preferably, the dissolution temperature of the bone glue is 20-60°C, for example, it can be 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.

[0042] Preferably, the dissolution time of the bone glue is 0.5 to 5 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, etc.

[0043] Preferably, during the preparation of the B component, the stirring speed is 200-500 rpm, for example, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, etc.

[0044] Preferably, during the preparation of the B component, the stirring time is 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc.

[0045] In a third aspect, the present invention provides a use of the two-component flame retardant as described in the first aspect in flame retardancy of plants, walls or thermal insulation boards.

[0046] In a fourth aspect, the present invention provides a method for using the two-component flame retardant as described in the first aspect, the method comprising the following steps:

[0047] The component A and the component B are mixed to obtain a mixture, and then diluted with water to obtain a diluent of the two-component flame retardant;

[0048] A sprayer is used to spray the diluted solution of the two-component flame retardant onto the surface of the base material to form a flame retardant layer.

[0049] Preferably, the mass ratio of component A to component B is (3-5):1, for example, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, etc., preferably 4:1.

[0050] Preferably, the mass ratio of the mixture to water is 10:(3-4), for example, it can be 10:3, 10:3.1, 10:3.2, 10:3.3, 10:3.4, 10:3.5, 10:3.6, 10:3.7, 10:3.8, 10:3.9, 10:4, etc., preferably 10:3.5.

[0051] Preferably, the base material includes any one of plants, walls or thermal insulation boards.

[0052] Preferably, the spraying amount of the diluent of the two-component flame retardant is 0.02-0.04 mL / cm 2 , for example, it can be 0.02 mL / cm 2 , 0.025mL / cm 2 , 0.03mL / cm 2 , 0.035mL / cm 2 , 0.04mL / cm 2 wait.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The two-component flame retardant of the present invention has excellent water resistance, heat resistance, low temperature resistance and fire resistance; it can be used as a fire retardant for plants in forests and grasslands.

[0055] (2) The two-component flame retardant of the present invention is used in the field of building exterior walls to improve the flame retardant properties of walls and insulation boards. After the flame retardant is sprayed on the walls and insulation boards, a carbonized protective layer will form on the surface when encountering fire, which effectively retards flames and forms a second line of defense, achieving double flame retardancy insurance. DETAILED DESCRIPTION

[0056] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0057] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0058] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0059] The present invention will be further described below by way of examples. Unless otherwise specified, the materials in the examples.

[0060] The raw material parameters in the following examples are as follows:

[0061] Starch phosphate is a yellow liquid material with a pH of 7 and a solid content of 40%.

[0062] Calcium chloride is calcium chloride dihydrate, white crystals, calcium chloride dihydrate.

[0063] The surfactant is a water-resistant nonionic surfactant (specific name: polyether modified silicone oil) with a surface tension of 23 mN / m.

[0064] Propylene glycol is industrial 1,2-propylene glycol with a content of ≥99.7% and a relative molecular mass of 76.09.

[0065] Aerogel is a hydrophilic silica nano-aerogel powder particle.

[0066] Bone glue is animal bone.

[0067] Example 1

[0068] This embodiment provides a two-component flame retardant, wherein the two-component flame retardant comprises component A and component B in a mass ratio of 4:1;

[0069] Wherein, the component A comprises the following components by weight:

[0070]

[0071] Wherein, the B component comprises the following components by weight:

[0072] 15 parts of bone glue

[0073] 85 parts of water.

[0074] The two-component flame retardant described in this embodiment is prepared according to the following steps:

[0075] Component A: weigh calcium chloride, surfactant, aerogel, water, propylene glycol and starch phosphate according to the above proportions, add them into a blender, and stir them thoroughly at a uniform speed (400 rpm); after stirring for 15 minutes, take samples for inspection, and package and store them after passing the inspection.

[0076] Component B: Add gelatin into water according to the above proportions, dissolve naturally at room temperature for 5 hours, and then stir at low speed with a mixer; after stirring at low speed (300rpm) for 5 minutes, take samples for inspection, and package and store after passing the inspection.

[0077] Example 2

[0078] This embodiment provides a two-component flame retardant, wherein the two-component flame retardant comprises component A and component B in a mass ratio of 4:1;

[0079] Wherein, the component A comprises the following components by weight:

[0080]

[0081] Wherein, the B component comprises the following components by weight:

[0082] 25 parts of bone glue

[0083] 75 parts of water.

[0084] The two-component flame retardant described in this embodiment is prepared according to the following steps:

[0085] Component A: weigh calcium chloride, surfactant, aerogel, water, propylene glycol and starch phosphate according to the above proportions, add them into a blender, and stir them thoroughly at a uniform speed (400 rpm); after stirring for 20 minutes, take samples for inspection, and package and store them after passing the inspection.

[0086] Component B: Add gelatin into water according to the above proportions, dissolve naturally at room temperature for 5 hours, and then stir at low speed with a mixer; after stirring at low speed (300rpm) for 10 minutes, take samples for inspection, and package and store after passing the inspection.

[0087] Example 3

[0088] This embodiment provides a two-component flame retardant, wherein the two-component flame retardant comprises component A and component B in a mass ratio of 4:1;

[0089] Wherein, the component A comprises the following components by weight:

[0090]

[0091] Wherein, the B component comprises the following components by weight:

[0092] 30 parts of bone glue

[0093] 70 parts of water.

[0094] The two-component flame retardant described in this embodiment is prepared according to the following steps:

[0095] Component A: weigh calcium chloride, surfactant, aerogel, water, propylene glycol and starch phosphate according to the above proportions, add them into a blender, and stir them thoroughly at a uniform speed (500 rpm); after stirring for 20 minutes, take samples for inspection, and package and store them after passing the inspection.

[0096] Component B: Add gelatin into water according to the above proportions, heat the water to 60°C to dissolve for 1 hour, and then stir it at a low speed with a mixer; after stirring at a low speed (400 rpm) for 10 minutes, take samples for inspection, and package and store them after passing the inspection.

[0097] Example 4

[0098] This embodiment provides a two-component flame retardant, which is different from Embodiment 1 only in that the mass ratio of the A component to the B component is 3:1, and other settings are completely consistent with Embodiment 1.

[0099] Example 5

[0100] This embodiment provides a two-component flame retardant, which is different from Embodiment 1 only in that the mass ratio of the A component to the B component is 5:1, and other settings are completely consistent with Embodiment 1.

[0101] Example 6

[0102] This embodiment provides a two-component flame retardant, which is different from Embodiment 1 only in that the component A includes the following components by weight:

[0103]

[0104] The other settings are exactly the same as those in Example 1.

[0105] Example 7

[0106] This embodiment provides a two-component flame retardant, which is different from Embodiment 1 only in that the component A includes the following components by weight:

[0107]

[0108] The other settings are exactly the same as those in Example 1.

[0109] Example 8

[0110] This embodiment provides a two-component flame retardant, which is different from Embodiment 1 only in that the B component includes the following components in parts by weight:

[0111] 10 parts of bone glue

[0112] 90 parts of water;

[0113] The other settings are exactly the same as those in Example 1.

[0114] Example 9

[0115] This embodiment provides a two-component flame retardant, which is different from Embodiment 1 only in that the B component includes the following components in parts by weight:

[0116] 35 parts of bone glue

[0117] 65 parts of water;

[0118] The other settings are exactly the same as those in Example 1.

[0119] Comparative Example 1

[0120] This comparative example provides a two-component flame retardant, which is different from Example 1 only in that starch phosphate is not added and the water content is increased to 80 parts; other settings are completely consistent with Example 1.

[0121] Comparative Example 2

[0122] This comparative example provides a two-component flame retardant, which differs from Example 1 only in that starch phosphate is replaced with pentaerythritol phosphate of equal mass; other settings are completely consistent with Example 1.

[0123] Comparative Example 3

[0124] This comparative example provides a two-component flame retardant, which is different from Example 1 only in that aerogel is not added and the water content is increased to 21.1 parts; other settings are completely consistent with Example 1.

[0125] Comparative Example 4

[0126] This comparative example provides a two-component flame retardant, which differs from Example 1 only in that the aerogel is replaced with an equal mass of nano-titanium dioxide; other settings are completely consistent with Example 1.

[0127] Comparative Example 5

[0128] This comparative example provides a two-component flame retardant, which is different from Example 1 only in that no water-resistant nonionic surfactant is added and the water content is increased to 15.3 parts; other settings are completely consistent with Example 1.

[0129] Comparative Example 6

[0130] This comparative example provides a two-component flame retardant, which differs from Example 1 only in that the water-resistant nonionic surfactant is replaced with an equal mass of sodium dodecylbenzene sulfonate; other settings are completely consistent with Example 1.

[0131] Comparative Example 7

[0132] This comparative example provides a two-component flame retardant, which differs from Example 1 only in that propylene glycol is replaced with propylene glycol of equal mass; other settings are completely consistent with Example 1.

[0133] Comparative Example 8

[0134] This comparative example provides a two-component flame retardant, which differs from Example 1 only in that calcium chloride is replaced by magnesium chloride of equal mass; other settings are completely consistent with Example 1.

[0135] Comparative Example 9

[0136] This comparative example provides a two-component flame retardant, which is different from Example 1 only in that the bone glue is replaced with xanthan gum of equal mass; other settings are completely consistent with Example 1.

[0137] Test method:

[0138] Test samples: the two-component flame retardants provided in Examples 1 to 9 and the two-component flame retardants provided in Comparative Examples 1 to 9;

[0139] Test method: (1) Under the condition of ambient temperature not lower than 0℃ and relative humidity not higher than 80%RH: Use an electric stirrer to weigh and mix component A and component B in proportion, then add 35% water and stir into liquid; (2) Use a sprayer to spray directly onto plants, walls or insulation boards; the spraying amount is: 0.03mL / cm 2 .

[0140] Test standards: as shown in Table 1 below:

[0141] Table 1

[0142]

[0143] The test results are shown in Table 2 below:

[0144] Table 2

[0145]

[0146]

[0147]

[0148]

[0149] From the performance test results of Tables 1 and 2 above, it can be concluded that the formulations of Examples 1 to 5 have excellent performance, and the flame retardant of the present invention fully meets the standard requirements. The present invention can be used in the field of green plants and building fire protection, and has excellent adhesion, water resistance, heat resistance, frost resistance, and excellent fire protection effect.

[0150] In the formula provided in Comparative Example 1, starch phosphate was not added, and the flame retardancy, adhesion and storage stability were greatly reduced, which was not as good as the technical solution of the present invention. In the formula of Comparative Example 3, aerogel was not added, and the heat resistance was poor, which was not as good as the technical solution of the present invention. In the formula of Comparative Example 5, surfactant was not added, and the water resistance was poor, which was not as good as the technical solution of the present invention.

[0151] In summary, the two-component flame retardant of the present invention is green and environmentally friendly, non-corrosive, has no effect on plant growth, can be used on trees, leaves, paper, walls, and insulation boards, and the product has excellent performance. It can be used in the rainy season in the south, the cold areas in the north, and the hot areas in summer, has good weather resistance, does not affect the product quality, and can also play a good protective role.

[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A two-component flame retardant, It is characterized in that The two-component flame retardant includes component A and component B; Wherein, the component A comprises starch phosphate, calcium chloride, a surfactant, propylene glycol, aerogel and water; Wherein, the B component includes gelatin and water.

2. The two-component flame retardant according to claim 1, It is characterized in that The component A comprises, by weight: 50-65 parts of starch phosphate, 10-15 parts of calcium chloride, 0.3-0.7 parts of surfactant, 0.5-1.0 parts of propylene glycol, 3-10 parts of aerogel and 15-25 parts of water.

3. The two-component flame retardant according to claim 1 or 2, It is characterized in that The pH of the starch phosphate is 6 to 8, and the solid content of the starch phosphate is 30 to 50 wt %; Preferably, the surfactant is a water-resistant nonionic surfactant; Preferably, the water-resistant nonionic surfactant is selected from any one or a combination of at least two of perfluoroalkyl polyoxyethylene ether, polyether-modified polysiloxane or fluoroalkyl polysiloxane, preferably polyether-modified polysiloxane; Preferably, the surface tension of the surfactant is 20 to 30 mN / m; Preferably, the aerogel is silicon dioxide nano-aerogel powder particles.

4. The two-component flame retardant according to claim 1, It is characterized in that The B component comprises, by weight: 15 to 30 parts of bone glue and 70 to 85 parts of water; Preferably, the glue is selected from animal glue.

5. The two-component flame retardant according to claim 1, It is characterized in that The mass ratio of the component A to the component B is (3-5):1, preferably 4:

1.

6. A method for preparing a two-component flame retardant according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: Mix starch phosphate, calcium chloride, a surfactant, propylene glycol, aerogel and water, and stir to obtain the A component; The gelatin is dissolved in water and stirred to obtain the B component.

7. The method for preparing the two-component flame retardant according to claim 6, It is characterized in that During the preparation of component A, the stirring speed is 300-600 rpm, and the stirring time is 15-20 min; and / or, the dissolution temperature of the bone glue is 20 to 60° C., and the dissolution time of the bone glue is 0.5 to 5 hours; And / or, during the preparation of the B component, the stirring speed is 200 to 500 rpm, and the stirring time is 5 to 10 min.

8. Use of the two-component flame retardant according to any one of claims 1 to 5 in flame retardancy of plants, walls or thermal insulation boards.

9. A method for using the two-component flame retardant according to any one of claims 1 to 5, It is characterized in that The method of use comprises the following steps: The component A and the component B are mixed to obtain a mixture, and then diluted with water to obtain a diluent of the two-component flame retardant; A sprayer is used to spray the diluted solution of the two-component flame retardant onto the surface of the base material to form a flame retardant layer.

10. The method for using the two-component flame retardant according to claim 9, It is characterized in that The mass ratio of component A to component B is (3-5):1, preferably 4:1; Preferably, the mass ratio of the mixture to water is 10:(3-4), preferably 10:3.5; Preferably, the base material includes any one of plants, walls or insulation boards; Preferably, the spraying amount of the diluent of the two-component flame retardant is 0.02-0.04 mL / cm 2 .

Citation Information

Patent Citations

  • Forest, grassland fireproofing special flaming-resistant liquid

    CN101037601A

  • Intumescent fire-retardant coating and preparation method thereof

    CN105131784A

  • Flameproof sheet and method for producing the same

    JP2023089706A