Hot-melt marking coating prepared based on glass bead grafting modification and marking machine

By using glass microsphere graft modification technology and marking machine heating device in hot-melt marking paint, the problem that existing marking paint is easily damaged in extreme environments is solved, and the toughness and durability of the marking are improved. , ensuring the stability and reflective effect of road markings.

CN118725677APending Publication Date: 2024-10-01TIANTU ROAD IND GRP CO LTD

Patent Information

Application Number
CN202410819725.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing hot-melt road marking paints are prone to cracking and breakage in extreme environments and lack toughness. They are difficult to adapt to harsh conditions such as wind, sun, rain, high temperature, low temperature, high humidity, and high altitude.

Method used

Hot-melt marking paint based on graft modification of glass beads is used. By adding modified petroleum resin, modified plasticizer, thermoplastic elastic materials and other ingredients, combined with the design of a special marking machine, the toughness and adaptability of the paint are improved. Extreme environment capabilities.

Benefits of technology

Significantly improves the toughness and extreme environmental adaptability of the marking paint, extends the service life of the markings, reduces shedding caused by the rolling wear of wheels and anti-skid chains, and ensures the long-term reflective effect of road markings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725677A_ABST
    Figure CN118725677A_ABST
Patent Text Reader

Abstract

The invention discloses a hot-melt marking coating prepared based on glass bead grafting modification and a marking machine, and belongs to the technical field of road marking. The marking paint is prepared from the following raw materials in parts by weight: 115 to 135 parts of petroleum resin, 8 to 10 parts of modified plasticizer, 8 to 12 parts of wax, 15 to 35 parts of pigment, 550 to 850 parts of filler, 1 to 1.5 parts of water, 0.2 to 1.5 parts of antioxidant and 3 to 7 parts of thermoplastic elastic material. The hot-melt marking coating prepared on the basis of grafting modification of the glass beads has high toughness, so that the ability of the coating to adapt to an extreme environment after construction is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road marking, and in particular to a hot-melt road marking paint and a road marking machine prepared based on glass microbead grafting modification. Background Art

[0002] Road markings are mainly drawn on the road surface to regulate the passage of vehicles and pedestrians so that they can go their own way without interfering with each other, thus ensuring safe and smooth traffic.

[0003] The current hot-melt road marking paint has poor toughness, which makes it easy to crack and break when exposed to harsh environments such as wind, sun, rain, high temperature, low temperature, high humidity, high altitude, as well as the rolling and wear of wheels and anti-skid chains.

[0004] Therefore, it is necessary to provide a new hot-melt road marking paint and road marking machine based on glass microbead grafting modification. Summary of the invention

[0005] Based on the above problems existing in the prior art, the purpose of the embodiments of the present invention is to provide a hot-melt road marking paint prepared based on glass microbead grafting modification, which has high toughness and improves the ability of the paint to adapt to extreme environments after construction.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: to provide a hot-melt road marking paint prepared by glass microbead grafting modification, wherein the hot-melt road marking paint prepared by glass microbead grafting modification is prepared from the following raw materials in parts by weight: 115-135 parts of petroleum resin, 8-10 parts of modified plasticizer, 8-12 parts of wax, 15-35 parts of pigment, 550-850 parts of filler, 1-1.5 parts of water, 0.2-1.5 parts of antioxidant, and 3-7 parts of thermoplastic elastic material.

[0007] Furthermore, the petroleum resin is one or more of modified C5 petroleum resin, modified piperyl petroleum resin and modified saturated C9 petroleum resin.

[0008] Furthermore, the modified plasticizer raw material is composed of the following components by mass fraction: 92% paraffin-based white oil and / or cycloalkyl white oil, 5% olefin anhydride, 2.5% emulsifier, 0.35% corrosion inhibitor and 0.25% preservative and bactericide.

[0009] Furthermore, the thermoplastic elastic material is one or more of thermoplastic rubber TPR, thermoplastic elastomer TPE, SEBS thermoplastic elastomer or SEPS thermoplastic elastomer.

[0010] The present invention also provides a road marking machine, which is suitable for the construction of the above-mentioned hot-melt road marking paint prepared based on the grafting modification of glass microbeads. The road marking machine includes a frame and a marking unit arranged on the frame, the frame is provided with a material barrel, the material barrel is provided with a discharge port, the marking unit includes a cavity one, a cavity two, a heating element, a discharge nozzle and a material cup, the cavity set is arranged outside the cavity two, so that the inner cavity wall of the cavity one and the outer wall of the cavity two are separated to form a cavity one, the outer wall of the cavity one is provided with a feed port communicating with the cavity one at an upper position, the outer wall of the cavity one is provided with a spray port communicating with the cavity one at a lower position, the heating element is accommodated and installed in the inner cavity of the cavity two, and the heating element The outer wall of the heating element and the inner wall of the cavity two form the cavity two, the discharge nozzle is arranged at the bottom end of the cavity one, and the discharge nozzle is communicated with at least the cavity two, the material cup is arranged at the upper end of the cavity two, and the inner cavity of the material cup is communicated with the cavity two, when the discharge port is opened, the marking paint flowing out of the discharge port then enters the inner cavity of the material cup, and then enters the cavity two through the material cup, due to the heating element in the cavity two, the paint is heated in the process of falling through the cavity two, and the heat in the cavity two can be transferred to the cavity one through the cavity two, so that the high-temperature paint in the cavity two can increase the temperature of the cavity one through heat transfer, so that the modified glass beads are heated when passing through the cavity one.

[0011] Furthermore, the material cup has a cylindrical structure, and cavity one has a cylindrical structure. The upper end opening of cavity one is sleeved and fixed on the lower end of the material cup, and the upper end of cavity two is also fixedly connected to the lower end of the material cup. The heating element is disposed in cavity two at the center of cavity two.

[0012] Furthermore, the second cavity is made of a material with high thermal conductivity.

[0013] Furthermore, a storage cavity for accommodating paint discharged from a material barrel is provided inside the material cup, and a connecting hole is provided on the material cup and below the storage cavity, and the connecting hole connects the storage cavity and the second chamber.

[0014] Furthermore, the speed of inputting the modified glass microspheres from the feed port into the chamber 1 is not less than the speed of outputting the modified glass microspheres from the spray port.

[0015] Furthermore, the spray port is located on the side of the discharge nozzle facing away from the traveling direction of the road marking machine.

[0016] The beneficial effects of the present invention are as follows: the present invention provides a hot-melt road marking paint prepared based on glass microbead grafting modification, wherein the hot-melt road marking paint prepared based on glass microbead grafting modification is prepared from the following raw materials in parts by weight: 115-135 parts of petroleum resin, 8-10 parts of modified plasticizer, 8-12 parts of wax, 15-35 parts of pigment, 550-850 parts of filler, 1-1.5 parts of water, 0.2-1.5 parts of antioxidant, and 3-7 parts of thermoplastic elastic material. The thermoplastic elastic material added to the coating component can enhance the toughness of the coating, thereby further improving the ability of the coating to adapt to extreme environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0018] Figure 1 A schematic structural diagram of a road marking machine provided in an embodiment of the present invention.

[0019] Figure 2 A schematic diagram of the road marking machine provided in an embodiment of the present invention with the frame omitted.

[0020] Figure 3 for Figure 2 A longitudinal section view of the road marking machine of the structure shown.

[0021] Figure 4 A front view of a scribing unit provided in an embodiment of the present invention.

[0022] Figure 5 An exploded view of a scribing unit provided in an embodiment of the present invention.

[0023] Figure 6 For along Figure 4 Cross-sectional view along the EE direction.

[0024] Figure 7 A cross-sectional view of a material cup provided in an embodiment of the present invention.

[0025] Figure 8 A cross-sectional view of a support ring provided in an embodiment of the present invention.

[0026] Among them, the reference numerals in the figure are:

[0027] 1. Frame; 11. Material barrel; 111. Material discharge port; 12. Travel wheel; 13. Connecting rod; 2. Marking unit; 21. Cavity 1; 211. Material feed port; 212. Spray port; 213. Support ring; 214. Connecting port; 22. Cavity 2; 221. Confluence chamber; 23. Heating element; 231. Shell; 24. Material discharge nozzle; 25. Material cup; 251. Storage chamber; 252. Connecting hole; 26. Chamber 1; 27. Chamber 2; 28. Protective tube; 29. ​​Chamber 3; 212. Suspension rod; 22. Gate 1; 3. Swing arm 1; 31. First arm body; 32. Second arm body; 4. Control lever; 5. Mounting frame; 51. Suspension rod; 52. Gate; 521. Marking port; 6. Hook. DETAILED DESCRIPTION

[0028] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0029] It should be noted that when an element is referred to as being "connected to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0030] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0031] It should be understood that the orientation or position relationship indicated by terms such as "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0032] Reference throughout the specification to "one embodiment" or "an embodiment" means that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present application. Thus, when the phrases "in one embodiment," "in some embodiments," or "in some of these embodiments" appear in various places throughout the specification, not all references are to the same embodiment. Furthermore, in one or more embodiments, the particular features, structures, or characteristics may be combined in any suitable manner.

[0033] Embodiment 1

[0034] Embodiment 1 of the present invention provides a hot-melt road marking paint prepared based on glass microbead grafting modification, which is prepared from the following raw materials in parts by weight: 115-135 parts of petroleum resin, 8-10 parts of modified plasticizer, 8-12 parts of wax, 15-35 parts of pigment, 550-850 parts of filler, 1-1.5 parts of water, 0.2-1.5 parts of antioxidant, and 3-7 parts of thermoplastic elastic material.

[0035] In some of the embodiments, the petroleum resin is one or more of modified C5 petroleum resin, modified piperyl petroleum resin and modified saturated C9 petroleum resin.

[0036] The modified petroleum resin is adopted in the present invention to reduce the cohesive force of the petroleum resin and improve the fluidity and dispersibility of the petroleum resin.

[0037] In some embodiments, the modified plasticizer raw material is composed of the following components by mass fraction:

[0038] 92% paraffin-based white oil and / or naphthenic white oil, 5% olefin anhydride, 2.5% emulsifier, 0.35% corrosion inhibitor and 0.25% preservative and fungicide;

[0039] The preparation method of the modified plasticizer comprises the following steps:

[0040] S1: 30% paraffin-based white oil and / or naphthenic white oil by mass fraction is injected into a reactor, mixed evenly, heated to 45°C, then 5% olefin anhydride, 2.5% emulsifier, 0.35% corrosion inhibitor and 0.25% preservative and fungicide are added by mass fraction, and stirred for 15 minutes to obtain liquid A;

[0041] S2: Take the remaining 62% of paraffin-based white oil and / or naphthenic white oil by mass fraction and add them to liquid A, stir for 30 minutes, mix evenly, filter, and obtain the modified plasticizer for standby use.

[0042] It should be noted that the use of modified plasticizers improves the compatibility between the components of the coating, increases the fluidity of the coating, and reduces the amount of petroleum resin, thereby effectively reducing VOC emissions generated by the decomposition of organic matter and reducing pollution to the air and surrounding environment. On the other hand, it can ensure that the coating does not change color during storage, transportation and construction, and improves the anti-discoloration performance of the marking line when it is in extreme environments for a long time after construction.

[0043] The purpose of adding paraffin-based white oil and / or cycloalkyl white oil twice in the preparation method of the modified plasticizer is: in step S1, the temperature is maintained at 45°C, which is higher than room temperature. In step S2, the material needs to be packaged, which will cause thermal expansion and contraction efficiency, resulting in poor packaging effect. If paraffin-based white oil and / or cycloalkyl white oil at room temperature are added in step S2, the product can be cooled to the actual ambient temperature at an accelerated rate, thereby alleviating the volume change caused by thermal expansion and contraction.

[0044] In some embodiments, the wax is one or a mixture of two or more of polyethylene wax, oxidized polyethylene wax, polypropylene wax, sasol wax, ethylene bis stearamide or octadecanoic acid.

[0045] In some embodiments, the antioxidant is a phenolic antioxidant or a phosphite antioxidant.

[0046] In some of the embodiments, the thermoplastic elastic material is one or more of thermoplastic rubber TPR, thermoplastic elastomer TPE, SEBS thermoplastic elastomer or SEPS thermoplastic elastomer.

[0047] In some embodiments, the pigment is one or more of titanium dioxide, chrome yellow, yellow iron oxide, black iron oxide, carbon black, phthalocyanine blue, organic yellow, fast yellow, permanent yellow or permanent red metal complex dyes.

[0048] In some embodiments, the filler is one or more of natural heavy calcium carbonate powder, quartz sand or talc.

[0049] In summary, the present invention provides a method for preparing a hot-melt road marking paint based on glass microbead grafting modification. By adding thermoplastic elastic materials TPR, TPE, SEBS or SEPS to the paint components, the toughness of the paint can be enhanced, thereby further improving the ability of the paint to adapt to extreme environments.

[0050] In addition, by adding a small amount of water to the components, an emulsified azeotrope is formed with the oily substance during the production process, thereby increasing the compatibility between the components and raising the boiling point of water in the emulsified azeotrope, making the mixing and reaction more complete. Higher compatibility can reduce the amount of petroleum resin added, thereby improving the anti-fouling ability of the coating. While saving energy, it can reduce the decomposition products of petroleum resin produced by ultraviolet radiation, thereby reducing VOC emissions and being more environmentally friendly.

[0051] Finally, during the construction process, as the temperature rises, the steam formed by water and the emulsified azeotrope runs in the paint to evenly heat the paint, avoiding the coking of the paint due to local high temperature. In addition, due to the increase in the boiling point of water in the emulsified azeotrope, the residence time of water in the high temperature stage can be extended to a certain extent, thereby accelerating the melting rate of the paint. At the same time, due to the increase in fluidity between the paint components, the stirring resistance is reduced, and the continuous volatilization of water will also take away some heat, making the paint less likely to coke. When the temperature increases to a certain level, the water will completely evaporate, and the oily substance with a higher boiling point will condense into oil droplets and return to the paint components, so the performance of the paint will not be negatively affected by water.

[0052] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass microbeads accounting for 60% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0053] The modified glass microspheres are obtained by the following treatment method:

[0054] Take glass beads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 4, heat and boil for 10 minutes, and filter out.

[0055] 500 mL of methanol was mixed with 500 mL of water, and 5 g of ammonium chloride and 10 g of 3-mercaptopropyltrimethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0056] The pH value of 1000 mL of water was adjusted to 8 with NaOH, and 5 g of 3-glycidyloxypropyltrimethoxysilane and 5 g of dodecyltrimethoxysilane were added dropwise under stirring. Stirring was continued for 5 min, and the pH value of the solution was adjusted to 4 with acetic acid.

[0057] Add the above-mentioned glass beads, stir at 500 rpm for 15 min, filter out the glass beads, and rinse with water twice.

[0058] The post-treatment solution is uniformly sprayed on the surface of the glass microspheres, the temperature is raised to 70° C., the solution is heated while being stirred, and the modified glass microspheres are obtained after drying.

[0059] Embodiment 2

[0060] The difference between the hot-melt road marking paint prepared based on glass microbead grafting modification provided in the second embodiment and the first embodiment is that the hot-melt road marking paint prepared based on glass microbead grafting modification provided in the second embodiment is prepared from the following raw materials in parts by weight: 115 parts of modified isoprene petroleum resin, 8 parts of modified plasticizer, 8 parts of wax, 15 parts of pigment, 850 parts of filler, 1 part of water, 0.3 parts of antioxidant, and 3 parts of thermoplastic elastic material.

[0061] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass microbeads accounting for 65% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0062] The modified glass microspheres are obtained by the following treatment method:

[0063] Take glass microbeads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 4, heat and boil for 20 minutes, and filter out.

[0064] 500 mL of methanol was mixed with 500 mL of water, and 5 g of ammonium chloride and 30 g of 3-mercaptopropyltrimethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0065] The pH value of 1000 mL of water was adjusted to 8 with NaOH, 10 g of 3-glycidyloxypropyltrimethoxysilane and 20 g of dodecyltrimethoxysilane were added dropwise under stirring, stirring was continued for 10 min, and the pH value of the solution was adjusted to 4 with acetic acid.

[0066] Add the above-mentioned glass microbeads, stir at 1000 rpm for 30 min, filter out the glass microbeads, and rinse with water twice.

[0067] The post-treatment solution is uniformly sprayed on the surface of the glass microspheres, the temperature is raised to 70° C., the solution is heated while being stirred, and the modified glass microspheres are obtained after drying.

[0068] Embodiment 3

[0069] The difference between the hot-melt road marking paint prepared based on glass microbead grafting modification in the third embodiment and the first embodiment is that the hot-melt road marking paint prepared based on glass microbead grafting modification provided in the third embodiment is prepared from the following raw materials in parts by weight: 120 parts of modified isopentylene petroleum resin, 9 parts of modified plasticizer, 10 parts of wax, 25 parts of pigment, 590 parts of filler, 1.25 parts of water, 0.9 parts of antioxidant, and 5 parts of thermoplastic elastomer.

[0070] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass beads accounting for 70% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0071] The modified glass microspheres are obtained by the following treatment method:

[0072] Take glass beads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 4, heat and boil for 30 minutes, and filter out.

[0073] 500 mL of methanol was mixed with 500 mL of water, and 5 g of ammonium chloride and 50 g of 3-mercaptopropyltrimethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0074] The pH value of 1000 mL of water was adjusted to 8 with NaOH, 12.5 g of 3-glycidyloxypropyltrimethoxysilane and 37.5 g of dodecyltrimethoxysilane were added dropwise under stirring, stirring was continued for 15 min, and the pH value of the solution was adjusted to 4 with acetic acid.

[0075] Add the above-mentioned glass microbeads, stir at 1500 rpm for 45 min, filter out the glass microbeads, and rinse with water twice.

[0076] The post-treatment solution is evenly sprayed on the surface of the glass microspheres, the temperature is raised to 70° C., and the solution is heated while being stirred. The modified glass microspheres are obtained after drying.

[0077] Embodiment 4

[0078] The difference between the hot-melt road marking paint prepared by glass microbead grafting modification in the fourth embodiment and the one in the first embodiment is that the hot-melt road marking paint prepared by glass microbead grafting modification provided in the fourth embodiment is prepared from the following raw materials in parts by weight: 135 parts of modified isopentylene petroleum resin, 10 parts of modified plasticizer, 12 parts of wax, 35 parts of pigment, 490 parts of filler, 1.5 parts of water, 1.5 parts of antioxidant, and 7 parts of thermoplastic elastomer.

[0079] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass microbeads accounting for 75% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0080] The modified glass microspheres are obtained by the following treatment method:

[0081] Take glass microbeads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 5, heat and boil for 10 minutes, and filter out.

[0082] 500 mL of ethanol was mixed with 500 mL of water, and 15 g of ammonium chloride and 10 g of 3-mercaptopropyltriethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0083] The pH value of 1000 mL of water was adjusted to 9 with NaOH, and 5 g of 3-(methacryloyloxy)propyltrimethoxysilane and 5 g of dodecyltrimethoxysilane were added dropwise under stirring. Stirring was continued for 10 min, and the pH value of the solution was adjusted to 5 with citric acid.

[0084] Add the above-mentioned glass beads, stir at 500 rpm for 30 min, filter out the glass beads, and rinse with water twice.

[0085] The post-treatment solution is evenly sprayed on the surface of the glass microspheres, the temperature is raised to 75° C., and the solution is heated while being stirred, and the modified glass microspheres are obtained after drying.

[0086] Embodiment 5

[0087] The difference between the hot-melt road marking paint prepared by glass microbead grafting modification in the fifth embodiment and the first embodiment is that the hot-melt road marking paint prepared by glass microbead grafting modification provided in the fifth embodiment is prepared from the following raw materials in parts by weight: 125 parts of modified C5 petroleum resin, 9.5 parts of modified plasticizer, 9 parts of polyethylene wax, 3 parts of ethylene bis stearamide, 20 parts of pigment, 405 parts of calcium carbonate powder, 425 parts of 60-mesh heavy calcium carbonate sand, 1.5 parts of water, 0.5 parts of antioxidant, and 3 parts of TPR.

[0088] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass microbeads accounting for 60% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0089] The modified glass microspheres are obtained by the following treatment method:

[0090] Take glass microbeads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 5, heat and boil for 20 minutes, and filter out.

[0091] 500 mL of ethanol was mixed with 500 mL of water, and 15 g of ammonium chloride and 30 g of 3-mercaptopropyltriethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0092] The pH value of 1000 mL of water was adjusted to 9 with KOH, 20 g of 3-(methacryloyloxy)propyltrimethoxysilane and 10 g of dodecyltrimethoxysilane were added dropwise under stirring, stirring was continued for 15 min, and the pH value was adjusted to 4 with citric acid.

[0093] Add the above-mentioned glass microbeads, stir at 1000 rpm for 45 min, filter out the glass microbeads, and rinse with water twice.

[0094] The post-treatment solution is evenly sprayed on the surface of the glass microspheres, the temperature is raised to 75° C., and the solution is heated while being stirred, and the modified glass microspheres are obtained after drying.

[0095] Embodiment 6

[0096] The difference between the hot-melt road marking paint prepared by grafting modification of glass microspheres in the sixth embodiment and the first embodiment is that the hot-melt road marking paint prepared by grafting modification of glass microspheres provided in the sixth embodiment is prepared from the following raw materials in parts by weight: 115 parts of modified isopentylene petroleum resin, 9 parts of modified plasticizer, 10 parts of polypropylene wax, 2 parts of octadecanoic acid, 25 parts of pigment, 400 parts of calcium carbonate powder, 185 parts of 60 mesh quartz sand, 1.5 parts of water, 1 part of antioxidant, 2 parts of TPR, 1 part of TPE, and 1 part of SEBS thermoplastic elastomer.

[0097] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass microbeads accounting for 65% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0098] The modified glass microspheres are obtained by the following treatment method:

[0099] Take glass microbeads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 5, heat and boil for 30 minutes, and filter out.

[0100] 500 mL of ethanol was mixed with 500 mL of water, and 15 g of ammonium chloride and 50 g of 3-mercaptopropyltriethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0101] The pH value of 1000 mL of water was adjusted to 9 with KOH, and 37.5 g of 3-(methylpropyloxy)propyltrimethoxysilane and 12.5 g of dodecyltrimethoxysilane were added dropwise under stirring. Stirring was continued for 5 min, and the pH value of the solution was adjusted to 5 with citric acid.

[0102] Add the above-mentioned glass beads, stir at 1500 rpm for 15 min, filter out the glass beads, and rinse with water twice.

[0103] The post-treatment solution is evenly sprayed on the surface of the glass microspheres, the temperature is raised to 75° C., and the solution is heated while being stirred, and the modified glass microspheres are obtained after drying.

[0104] Embodiment 7

[0105] The difference between the hot-melt road marking paint prepared by grafting modification of glass microspheres in the seventh embodiment and the first embodiment is that the hot-melt road marking paint prepared by grafting modification of glass microspheres provided in the seventh embodiment is prepared from the following raw materials in parts by weight: 135 parts of modified isopentylene petroleum resin, 10 parts of modified plasticizer, 6 parts of polyethylene wax, 2 parts of octadecanoic acid, 35 parts of pigment, 390 parts of calcium carbonate powder, 85 parts of 60 mesh quartz sand, 1.5 parts of water, 1 part of antioxidant, 2 parts of TPE, 2 parts of SEBS thermoplastic elastomer, and 2 parts of SEPS thermoplastic elastomer.

[0106] The construction method of the road marking paint of the present invention is as follows: the road marking paint is put into a hot melt machine for melting and then poured into a material barrel 11 of the road marking machine, the road marking machine is used to draw road markings, and modified glass beads accounting for 70% of the mass of the paint matrix are sprinkled on the road markings, and the paint is waited for solidification to complete the construction.

[0107] The modified glass microspheres are obtained by the following treatment method:

[0108] Take glass beads with a particle size range of 30 to 100 mesh, add them to a hydrochloric acid aqueous solution with a pH value of 6, heat and boil for 30 minutes, and filter them out.

[0109] 500 mL of methanol was mixed with 500 mL of water, and 20 g of ammonium chloride and 50 g of 3-mercaptopropyltrimethoxysilane were added, and the mixture was stirred evenly to obtain a post-treatment solution.

[0110] The pH value of 1000 mL of water was adjusted to 10 with NaOH, 37.5 g of 3-(methacryloyloxy)propyltrimethoxysilane and 12.5 g of dodecyltrimethoxysilane were added dropwise under stirring, stirring was continued for 10 min, and the pH value of the solution was adjusted to 6 with citric acid.

[0111] Add the above-mentioned glass beads, stir at 1500 rpm for 30 min, filter out the glass beads, and rinse with water twice.

[0112] The post-treatment solution is evenly sprayed on the surface of the glass microspheres, the temperature is raised to 80° C., and the solution is heated while being stirred. The modified glass microspheres are obtained after drying.

[0113] Embodiment 8

[0114] Embodiment 8 of the present invention further provides a method for preparing a hot-melt road marking paint based on glass microsphere grafting modification provided in any of the above embodiments, and the method for preparing a hot-melt road marking paint based on glass microsphere grafting modification comprises:

[0115] Select fillers, pigments, waxes, modified plasticizers, antioxidants, thermoplastic elastic materials and water in order by weight, add them into a horizontal ribbon mixer and stir for 20 minutes to mix evenly, then add petroleum resin by weight, continue stirring for 3-5 minutes, mix evenly, and then pack the materials.

[0116] Embodiment 9

[0117] like Figure 1-8As shown, an embodiment of the present invention further provides a road marking machine, which is suitable for constructing a hot-melt road marking paint prepared based on glass microbead grafting modification provided in any of the above embodiments. The road marking machine includes a frame 1 and a marking unit 2 arranged on the frame 1, and a material barrel 11 for storing molten road marking paint is arranged on the frame 1. The marking unit 2 is arranged on one side of the frame 1, and a discharge port 111 is provided on the side of the material barrel 11 close to the marking unit 2. The marking unit 2 includes a cavity 1 21, a cavity 22, a heating element 23, a discharge nozzle 24 and a material cup 25. The cavity 1 21 is sleeved outside the cavity 22, so that a cavity 1 26 is formed between the inner cavity wall of the cavity 1 21 and the outer wall of the cavity 22. The cavity 1 21 A feed port 211 communicating with chamber 1 26 is arranged on the outer wall of cavity 1 21 and at an upper position, and the feed port 211 is used to inject modified glass microbeads into chamber 1 26. A spray port 212 communicating with chamber 1 26 is arranged on the outer wall of cavity 1 21 and at a lower position, and the spray port 212 is used to release the modified glass microbeads dropped from chamber 1 26. The heating element 23 is accommodated and installed in the inner cavity of cavity 22, and the outer wall of the heating element 23 and the inner cavity wall of cavity 22 are spaced to form chamber 27. The discharge nozzle 24 is arranged at the bottom end of cavity 1 21, and the discharge nozzle 24 is at least communicated with chamber 27. The material cup 25 is arranged at the upper end of chamber 27, and the inner cavity of the material cup 25 is communicated with chamber 27. The marking paint flowing out of the discharge port 111 then enters the inner cavity of the material cup 25, and then enters the chamber 27 through the material cup 25. Due to the heating element 23 in the chamber 27, the paint is heated in the process of falling through the chamber 27, ensuring that the paint is in a molten state, so that the paint will not solidify due to the temperature drop, and the paint flows out smoothly from the discharge nozzle 24 in an excellent fluid state, which is helpful to mark regular road markings; and the heat in the chamber 27 can be transferred to the chamber 1 26 through the cavity 22. In the marking unit 2 provided in the embodiment of the present invention, the high-temperature paint in the chamber 27 can increase the temperature of the chamber 1 26 through heat transfer, so that the modified glass microspheres When passing through chamber 1 26, the modified glass beads are heated and heated, so that when the high-temperature modified glass beads are sprinkled on the road marking, the part of the paint in contact with the modified glass beads will not lose temperature and solidify rapidly due to contact with cold modified glass beads. Since the modified glass beads are heated and have a high temperature, the solidification speed of the part of the paint in contact with the modified glass beads is slowed down. In this way, the modified glass beads have a longer time to penetrate into the paint under the action of gravity, so that the modified glass beads are more deeply and firmly combined with the road marking, the stability of the modified glass beads on the surface of the road marking is improved, and the modified glass beads on the road marking are not easily crushed and fallen off by wheels and anti-skid chains, so that the road marking after construction can have a long-term and effective reflective effect.

[0118] It is understood that the speed of inputting the modified glass microspheres from the feed port 211 into the chamber 26 is not less than the speed of outputting the modified glass microspheres from the spray port 212. In this way, on the one hand, sufficient modified glass microspheres can be maintained in the chamber 26 to ensure uninterrupted spraying; on the other hand, more importantly, the modified glass microspheres can stay in the chamber 26 for a long time, so that there is enough time to ensure that the modified glass microspheres in the chamber 26 can be heated.

[0119] like Figure 4 , Figure 5 and Figure 6 As shown, in some embodiments, the material cup 25 is a cylindrical structure, the cavity 1 21 is a cylindrical structure, the upper end opening of the cavity 1 21 is sleeved and fixed to the lower end of the material cup 25, the upper end of the cavity 22 is also fixedly connected to the lower end of the material cup 25, and the heating element 23 is arranged in the cavity 2 27 at the center of the cavity 2 22. Specifically, the outer shell 231 is sleeved on the outside of the heating element 23, and the heating element 23 is fixedly connected to the lower end of the material cup 25 through the shell 231, and the outer shell 231 plays a role in sealing and protecting the heating element 23. In this embodiment, the heating element 23 is an electric heating type.

[0120] like Figure 7 As shown, in some embodiments, a storage chamber 251 for accommodating the paint discharged from the material barrel 11 is provided inside the material cup 25, and a connecting hole 252 is provided on the material cup 25 and below the storage chamber 251, and the connecting hole 252 communicates between the storage chamber 251 and the chamber 2 27. In addition, the material cup 25 has an opening at the top of the storage chamber 251, so that the paint flowing out of the discharge port 111 can enter the storage chamber 251 through the top opening of the storage chamber 251, and the discharge port 111 and the top opening of the storage chamber 251 can be connected through a flexible guide pipe.

[0121] In some embodiments, the housing 231 is made of a material with high thermal conductivity.

[0122] In some of the embodiments, the second cavity 22 is made of a material with high thermal conductivity, thereby increasing the rate at which heat in the second cavity 27 is transferred to the first cavity 26 through the second cavity 22, and ensuring that the first cavity 26 can be heated up quickly.

[0123] like Figure 4 , Figure 5 and Figure 6 As shown, in some embodiments, the lower end of the second cavity 22 is supported on the inner wall of the first cavity 21 to stabilize the second cavity 22. Specifically, a support ring 213 is provided between the inner wall of the first cavity 21 and the outer wall of the second cavity 22. Figure 8As shown, a connecting port 214 is provided on the support ring 213, and the connecting port 214 is used for allowing the modified glass microbeads in the chamber 26 to pass through the supporting ring 213 through the connecting port 214, so as to prevent the support ring 212 from clogging the modified glass microbeads in the chamber 26.

[0124] like Figure 2 and Figure 3 As shown, in some embodiments, the end opening of the discharge nozzle 24 is flat, which is conducive to the linear outflow of the marking paint. It can be understood that the shape of the end opening of the discharge nozzle 24 can be selected according to the actual size of the marking line.

[0125] like Figure 6 As shown, in some embodiments, a protective tube 28 is provided at the upper end of the heating element 23, one end of the protective tube 28 is in communication with the heating element 23, and the other end of the protective tube 28 extends upward through the storage cavity 251, and a device for providing energy to the heating element 23 can be connected to the heating element 23 through the protective tube 28. Specifically, in this embodiment, one end of the protective tube 28 is butted against the upper end of the housing 231.

[0126] like Figure 6 As shown, in some embodiments, a confluence chamber 221 communicating with the second chamber 27 is provided in the inner cavity of the second cavity 22 and at a lower position, and the confluence chamber 221 is opposite to and communicated with the discharge nozzle 24 .

[0127] like Figure 6 As shown, in some embodiments, the lowermost end of chamber 1 26 is provided with chamber 3 29, chamber 3 29 is located below the spray port 212, and chamber 3 29 is connected between chamber 1 26 and discharge nozzle 24, so that at least part of the modified glass microbeads in chamber 1 26 can flow from chamber 3 29 to discharge nozzle 24, so that part of the modified glass microbeads are mixed with the marking paint, so that the road markings drawn will also be mixed with modified glass microbeads, and when the outer layer of the road marking is worn, the modified glass microbeads inside it will still make the road markings have a certain reflective effect. Specifically, the flow cross section of chamber 3 29 is smaller than the flow cross section of chamber 1 26.

[0128] like Figure 2 , Figure 3 and Figure 6 As shown, in some embodiments, the spray port 212 is located on the side of the discharge nozzle 24 facing away from the travel direction of the road marking machine, so that when the paint is released from the discharge nozzle 24 to the ground to draw the road markings, the modified glass beads released from the spray port 212 will be sprinkled on the surface of the road markings to form a reflective layer on the surface of the road markings.

[0129] like Figure 2 and Figure 3As shown, in some embodiments, the marking unit 2 is installed on the mounting frame 5. Specifically, the cavity 21 is fixedly connected to the mounting frame 5. A gate 52 is provided at the outlet of the discharge nozzle 24. The gate 52 is slidably fitted on the mounting frame 5. A marking opening 521 is provided on the gate 52 corresponding to the discharge nozzle 24. When the gate 52 is moved to stagger the marking opening 521 with the discharge nozzle 24, the gate 52 covers the discharge nozzle 24. Or when the gate 52 is moved to make the marking opening 521 on the gate 52 relative to the discharge nozzle 24, the connection between the discharge nozzle 24 and the marking opening 521 is opened, so that the marking paint can flow out through the discharge nozzle 24 and the marking opening 521 in sequence to implement the marking work.

[0130] like Figure 1 , Figure 2 and Figure 3 As shown, in some embodiments, the first end of the mounting frame 5 is movably connected to the frame 1, so that the mounting frame 5 can at least swing up and down around the first end of the mounting frame 5 on the frame 1, so as to control the mounting frame 5 to drive the marking unit 2 to move the marking opening 521 close to the ground when it is descending, and the mounting frame 5 can drive the marking unit 2 to be lifted up to be away from the ground when it is not working or needed. The road marking machine also includes a control rod 4, one end of the control rod 4 is hinged on the mounting frame 5, and the side of the mounting frame 5 is hinged with a swing arm 3, and the swing arm 3 includes The first arm body 31 and the second arm body 32 are connected in sequence, the first arm body 31 is connected to the control rod 4, and the second arm body 32 is connected to the gate 52. When the control rod 4 swings upward on the mounting frame 5, the second arm body 32 of the swing arm 3 swings downward toward the gate 52, thereby pushing the gate 52 to move and close the discharge nozzle 24. Conversely, when the control rod 4 swings downward on the mounting frame 5, the second arm body 32 of the swing arm 3 swings upward away from the gate 52, thereby driving the gate 52 to move and open the discharge nozzle 24. Specifically, when the control rod 4 is lifted, the mounting frame 5 drops due to gravity, and at the same time, the control rod 4 swings upward on the mounting frame 5 and leaves the ground, driving the gate 52 to move to close the discharge nozzle 24. At this time, the mounting frame 5 is hung on the frame 1, so that the marked opening 521 of the mounting frame 5 can be kept in a closed state at all times. Figure 2 As shown, specifically, a hook 6 is provided on the swing arm 31 of the first arm body 23, and the hook 6 can be hung on the frame 1, so that the mounting frame 5 sinks under the action of gravity, and the first arm body 31 of the swing arm 3 swings upward relative to the mounting frame 5, keeping the gate 52 closing the discharge spout 24; when the mounting frame 5 is placed on the ground, the control lever 4 is released at this time, and the control lever 4 will swing downward under the action of gravity, driving the first arm body 31 of the arm body 231 to swing downward, driving the gate 52 to move to open the discharge spout 24. In order to facilitate the hook 6 to be hung on the frame 1 or detached from the frame 1, the mounting frame 5 is hinged on the frame 1 and can swing left and right relative to the frame 1, so that the mounting frame 5 and / or the control lever 4 can swing left and right to make the hook 6 close to or away from the frame 1.

[0131] like Figure 1 and Figure 2 As shown, in some embodiments, a suspension rod 51 is provided on one side of the mounting frame 5, and a connecting rod 13 is provided on the frame 1 corresponding to the suspension rod 51, and the suspension rod 51 is movably connected to the connecting rod 13, so that the mounting frame 5 can swing on the connecting rod 13 of the frame 1 in various directions, such as up and down, left and right, etc. Thus, the control lever 4 can at least drive the mounting frame 5 to swing up and down around the connecting rod 13, so that the mounting frame 5 can be lifted up to leave the ground when not in use, and the mounting frame 5 can be lowered to close to the ground when marking is required.

[0132] like Figure 1 As shown, in some of the embodiments, a running wheel 12 is mounted on the frame 1, and the running wheel 12 is used for contacting the ground and rolling.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing hot melt road marking paint based on glass microbead grafting modification, characterized in that: The hot-melt road marking paint based on glass microbead grafting modification is prepared from the following raw materials in parts by weight: 115-135 parts of petroleum resin, 8-10 parts of modified plasticizer, 8-12 parts of wax, 15-35 parts of pigment, 550-850 parts of filler, 1-1.5 parts of water, 0.2-1.5 parts of antioxidant, and 3-7 parts of thermoplastic elastic material.

2. The method for preparing hot melt road marking paint based on glass microsphere grafting modification according to claim 1, characterized in that: The petroleum resin is one or more of modified C5 petroleum resin, modified piperyl petroleum resin and modified saturated C9 petroleum resin.

3. The method for preparing hot-melt road marking paint based on glass microbead grafting modification according to claim 1, characterized in that: The modified plasticizer raw material consists of the following components by mass fraction: 92% paraffin-based white oil and / or cycloalkyl white oil, 5% olefin anhydride, 2.5% emulsifier, 0.35% corrosion inhibitor and 0.25% antiseptic and bactericide.

4. The method for preparing hot-melt road marking paint based on glass microsphere grafting modification according to claim 1, characterized in that: The thermoplastic elastic material is one or more of thermoplastic rubber TPR, thermoplastic elastomer TPE, SEBS thermoplastic elastomer or SEPS thermoplastic elastomer.

5. A road marking machine, suitable for applying the hot melt road marking paint prepared by grafting and modifying glass beads as described in any one of claims 1 to 4, characterized in that: The road marking machine includes a frame and a marking unit arranged on the frame, the frame is provided with a material barrel, the material barrel is provided with a discharge port, the marking unit includes a cavity one, a cavity two, a heating element, a discharge nozzle and a material cup, the cavity set is arranged outside the cavity two, so that a cavity one is formed between the inner cavity wall of the cavity one and the outer wall of the cavity two, a feed port communicating with the cavity one is arranged on the outer wall of the cavity one and at an upper position, a spray port communicating with the cavity one is arranged on the outer wall of the cavity one and at a lower position, the heating element is accommodated and installed in the inner cavity of the cavity two, and a cavity two is formed between the outer wall of the heating element and the inner cavity wall of the cavity two The discharge nozzle is arranged at the bottom end of the cavity one, and the discharge nozzle is communicated with at least the cavity two, the material cup is arranged at the upper end of the cavity two, the inner cavity of the material cup is communicated with the cavity two, when the discharge port is opened, the marking paint flowing out from the discharge port then enters the inner cavity of the material cup, and then enters the cavity two through the material cup, due to the heating element in the cavity two, the paint is heated in the process of falling through the cavity two, and the heat in the cavity two can be transferred to the cavity one through the cavity two, so that the high-temperature paint in the cavity two can increase the temperature of the cavity one through the heat transfer, so that the modified glass microbeads are heated when passing through the cavity one.

6. The road marking machine according to claim 5, characterized in that: The material cup is of cylindrical structure, and cavity one is of cylindrical structure. The upper end opening of cavity one is sleeved and fixed on the lower end of the material cup, and the upper end of cavity two is also fixedly connected to the lower end of the material cup. The heating element is disposed in cavity two at the center of cavity two.

7. The road marking machine according to claim 5, characterized in that: The second cavity is made of a material with high thermal conductivity.

8. The road marking machine according to claim 5, characterized in that: The material cup is provided with a storage cavity for accommodating the paint discharged from the material barrel, and a connecting hole is provided on the material cup and below the storage cavity, and the connecting hole is connected between the storage cavity and the second chamber.

9. The road marking machine according to claim 5, characterized in that: The speed of inputting the modified glass microspheres from the feed port into the chamber 1 is not less than the speed of outputting the modified glass microspheres from the spray port.

10. The road marking machine according to claim 5, characterized in that: The spraying port is located at a side of the discharge nozzle facing away from the traveling direction of the road marking machine.

Citation Information

Patent Citations

  • Hot melting scribing machine with heating device with uncoated surface scattered with glass beads

    CN103147383A

  • Quick-melting environment-friendly high-toughness hot-melt marking paint and preparation method thereof

    CN108467653A

  • Device and preparation method for preparing leather surfactant

    CN112426997A

  • Quick-setting hot-melt marking coating, preparation method thereof and marking machine

    CN116855137A

  • Spraying raw material heating device for road marking improvement

    CN214992973U

Cited By

  • High-durability reflective hot-melt road marking coating and preparation method thereof

    CN121203543A