Powder coating for wooden furniture as well as preparation method and application of powder coating

Through the sandwich structure of modified barrier agents and acetic anhydride intercalation technology, the problem of self-curing of wood furniture powder coatings in high temperature environments is solved, the stability and toughness of the coatings are improved, and tighter coating cross-linking and resistance are achieved. cracking performance.

CN118725699APending Publication Date: 2024-10-01JIANGXI LONGZHENG TECH DEV CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410950119.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing powder coatings for wooden furniture can easily lead to self-curing and cross-linking of the active groups of resin molecules in high-temperature environments, affecting the stability and toughness of the coating, especially during storage and transportation.

Method used

Modified barrier agents are used to construct a sandwich structure of modified sheets and hydroxide metal salt layers, and acetic anhydride intercalation is used to reduce the contact between resin molecules and active groups, and to promote the separation of modified sheets at the curing temperature. Exposing the groups allows cross-linking to form a tighter coating.

Benefits of technology

It effectively prevents the self-curing phenomenon of the coating during storage, improves the stability and toughness of the powder coating, enhances the tensile strength and tensile resistance of the coating, and avoids cracking and orange peel phenomena.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725699A_ABST
    Figure CN118725699A_ABST
Patent Text Reader

Abstract

The invention provides a powder coating for wood furniture and a preparation method and application thereof, and belongs to the technical field of powder paints.The powder coating is obtained by mixing polyester resin, epoxy resin, titanium dioxide, auxiliaries and a modified blocking agent and conducting melting and smashing; the modified blocking agent is prepared by the following steps: coupling a nano sheet with a modified group, mixing water, sodium alginate, metal salt, attapulgite and a surfactant, stirring to obtain an emulsion, adding the modified sheet into the emulsion according to a solid-to-liquid ratio of 1: (3-5), stirring, slowly dropwise adding a sodium hydroxide solution to adjust the emulsion to alkalescence, filtering and washing to obtain an intermediate, and drying to obtain the modified blocking agent. Mixing the intermediate, acetic anhydride and a polar solvent in a mass ratio of 1: (1-2): (12-16), performing soaking reaction for 30-60 minutes at the reaction temperature of 32-45 DEG C, and performing water washing, suction filtration and drying to obtain the modified blocking agent. The powder coating disclosed by the invention can be stably stored at a relatively high temperature and has relatively high toughness, cracking resistance and stretchability after being cured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder coatings, and in particular to a powder coating for wooden furniture and a preparation method and application thereof. Background Art

[0002] Powder coating is a fairly mature product in industrial coatings. It is mostly used on the surface of metal equipment and is rarely used on wooden furniture. This is mainly because the curing temperature of the coating is high, usually above 170°C. High temperature will quickly evaporate the moisture in the wood. Different parts of the wood will have different expansion degrees due to different thicknesses, causing wooden furniture to warp and shrink. The development direction of powder coatings applied to the surface of wood is low-temperature curing. As for the selection of low-temperature curing methods, the existing technology uses 2-butyl-2-ethyl-1,3-propanediol instead of neopentyl glycol to prepare synthetic polyester, and uses trimeric anhydride instead of isophthalic acid to prepare powder coatings that cure at 120°C. However, the glass transition temperature of low-temperature cured polyester resin is also low, and it is easily affected by high temperature weather, which increases the chemical reactivity of the active groups of the resin molecules, thereby causing undesirable cross-linking or degradation reactions to occur, affecting the stability of the coating during packaging, transportation and storage.

[0003] Another option is to use additives such as promoters and catalysts to reduce the crosslinking and curing temperature of the resin. As the main component of the coating, polyester / epoxy resin has strong chemical resistance and weather resistance, providing the coating with excellent protection, durability and good adhesion to the substrate; the curing agent used for polyester / epoxy resin mostly uses amino groups to attack the epoxy groups in the epoxy resin molecules to open the ring to form secondary hydroxyl and secondary amine groups, and then the secondary amine groups react with other epoxy groups to further form tertiary amine and secondary hydroxyl groups. The hydroxyl groups in the two-step reaction can open the epoxy groups under the catalysis of the tertiary amine, thereby forming bonds to complete the curing and crosslinking.

[0004] Therefore, when using the above-mentioned low-temperature curing powder coating and the corresponding amino-containing curing agent, the added curing agent should not be too much, otherwise the chemical reaction activity of the polyester resin will increase when approaching the Tg temperature, and it will easily react with the amino-containing components to form a "self-curing" effect in advance. Similarly, when using other amino-modified materials to improve powder coatings, "self-curing" reactions will often occur due to excessive amino active groups. Summary of the invention

[0005] In order to solve the problem that due to the addition of modified substrates, too many active groups in the coating cause the resin to be stored in a hot environment, and its active groups and the cross-linking sites of the resin are easily catalyzed and reacted, and pre-cross-linking is performed in advance, the present application provides a method for preparing a powder coating for wood furniture, and the specific steps are as follows:

[0006] A polyester resin, an epoxy resin, titanium dioxide, an additive, and a modified barrier agent are mixed to obtain a mixture, and the mixture is melt-pulverized to obtain a powder coating; wherein the modified barrier agent is obtained by a method comprising the following steps:

[0007] S1, preparing a sheet material into a single-layer nanosheet, coupling a modified group to the nanosheet to obtain a modified sheet;

[0008] S2, mixing water, sodium alginate, metal salt, attapulgite and surfactant, stirring to obtain an emulsion, adding the modified sheet to the emulsion at a solid-liquid ratio of 1:3-5, stirring, slowly adding sodium hydroxide solution to adjust the emulsion to slightly alkaline, filtering and washing, to obtain an intermediate;

[0009] S3. Mix the intermediate, acetic anhydride and polar solvent in a mass ratio of 1:1-2:12-16, soak and react for 30-60 minutes at a reaction temperature of 32-45°C, wash with water, filter and dry to obtain a modified barrier agent.

[0010] By adopting the technical solution of modified barrier agent, the modified sheet is prepared and used in combination with the emulsion, so as to construct a sandwich structure with the modified sheet inside and the metal hydroxide salt layer outside, and acetic anhydride is used to intercalate between the modified sheet layer and the isolation layer for the sandwich structure; after the intercalation, under the storage environment of room temperature, acetic anhydride will not increase the interlayer spacing of the sheet layer, and the presence of the external metal hydroxide salt layer reduces the contact between the active groups on the surface of the modified sheet layer and the active sites of the resin molecules, thereby protecting the coating from self-curing and improving the quality of the powder coating.

[0011] Furthermore, the acetic anhydride added by the applicant will produce a series of reactions or effects only at 120-140°C. The temperature during the curing process will promote the separation of the isolation layer and the modified sheet. The curing temperature can just increase the interlayer distance between the isolation layer and the modified sheet, and finally expose the active groups of the modified sheet, so that the modified groups can effectively undergo cross-linking and curing reactions with the resin molecules, and the resin molecules and the modified sheet are more closely combined. After the powder coating is cured and formed, the coating is tougher and less prone to cracking.

[0012] The powder coating of the present application not only effectively copes with the insufficient toughness of the coating caused by wood shrinkage, but also maintains the low-temperature curing conditions required for the powder coating to be applied to wooden furniture.

[0013] Furthermore, the epoxy resin is one of bisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, hexahydrophthalic acid diglycidyl ether, and acrylate diglycidyl ether.

[0014] The epoxy resin used in the present application can be effectively cross-linked and cured with amino groups, and the characteristics of the sheet material can be used to form a specific layered reinforcement effect, which directly improves the tensile strength of the coating. The glyoxylic acid used will spontaneously react at high temperature to "push away" the sheet material and the isolation layer, thereby increasing the interlayer spacing; the amino groups on the surface of the sheet material can not only serve as active sites for attacking the epoxy groups for cross-linking, but can also undergo nucleophilic addition reactions with glyoxylic acid to ultimately form new oxygen-nitrogen bonds, and the new oxygen-nitrogen structure can continue to react with the more active epoxy groups. The mica flakes can effectively increase the toughness of the resin coating and improve the tensile strength of the coating.

[0015] The sheet material in S1 is one of mica, bentonite, montmorillonite or flake graphite, the obtained nanosheet has a sheet diameter of 10 to 50 μm and a thickness of 1 to 50 nm, and the modified group is an amino group.

[0016] The polar solvent in S3 is one of tetrahydrofuran and dimethyl sulfoxide.

[0017] The sheet material is prepared into a single-layer nanosheet by peeling it off through any one of ultrasonic, grinding, nitric acid mixed heating or adhesive peeling.

[0018] The ratio of water, sodium alginate, metal salt, attapulgite and surfactant in the isolation layer of S2 is 5:1:1.5-2.5:0.5:0.05, wherein the metal salt is one of the alkaline earth metal salts.

[0019] The additives include a leveling agent, a sand grain agent, a degassing agent, a charging agent, a hardening wax powder, and a tertiary amine accelerator. The specific weight percentage of each component in the mixture is as follows:

[0020] 40-50 parts of polyester resin, 25-35 parts of epoxy resin, 20-30 parts of titanium dioxide, 0.2-1 parts of leveling agent, 0.5-2 parts of sand grain agent, 1-3 parts of degassing agent, 0.2-0.8 parts of charging agent, 1-3 parts of hardening wax powder, 0.1-0.6 parts of tertiary amine accelerator, and 6-12 parts of modified barrier agent.

[0021] The coupling process of the nanosheets in S1 is as follows:

[0022] Ethanol, water and γ-glycidyloxypropyltrimethoxysilane were mixed in a weight ratio of 20:14:1 to obtain a coupling liquid, and the nanosheets were immersed in the coupling liquid for 15 minutes, with a solid-liquid mass ratio of 1-7:1. After filtering, the nanosheets were dried at 160°C for 1 hour.

[0023] According to a method for preparing a polyurethane composite material for high-speed rail according to an embodiment of the present application, there are at least the following beneficial effects:

[0024] The present application adopts a gel precipitation method to transform the sheet material, so as to block the contact between the surface of the sheet material and the resin, so that the resin will not produce the "self-curing" phenomenon due to excessive active groups at a higher temperature below the curing temperature. The reaction is carried out in three steps. Due to the use of a composite form of organic and inorganic materials, the metal salt is first evenly dispersed in a slightly alkaline environment, and then a hydroxide precipitate is formed in an alkaline environment and deposited on the surface of the modified sheet. The modified groups on the modified sheet are adapted to the slightly alkaline environment and will not disappear, thereby generating nano-scale hydroxide precipitation flakes on the outside of the modified sheet, which has an effective steric effect. Through a certain spatial steric hindrance, the contact between the modified groups on the modified sheet and the epoxy groups in the resin molecules is blocked, and the occurrence of cross-linking reactions is inhibited, thereby improving the stability of the powder coating particles, and eliminating the orange peel phenomenon, granulation and depression in the coating effect.

[0025] The present application further optimizes the modified barrier agent, and uses acetic anhydride in the barrier additive to be inserted between the sheets, so that the interlayer spacing changes at the curing temperature, ensuring that the coating surface can form a tighter effect during the subsequent curing process. Since the sheet material has the effect of enhancing the toughness of the coating, in order to achieve better cross-linking and crack resistance and stretch resistance, the cross-linking between the modified sheet and the resin needs to be closer. Therefore, the acetic anhydride used can not only react with a part of the modified group, but also separate the isolation layer outside the modified sheet at the curing temperature, so that the modified sheet can be more easily cross-linked with the resin molecules.

[0026] On the third aspect, the powder resin provided in the embodiment of the present application can be coated on the surface of furniture, so that the coating has a better curing temperature and better resistance to cracking, and can prevent the coating from cracking due to deformation and stretching of the wood. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a line graph of the impact resistance of the powder coatings of each embodiment and comparative example of the present application after temperature change;

[0028] Figure 2 It is a line graph of the flexibility of the powder coatings of various embodiments and comparative examples of the present application after temperature change. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the following will be combined with the appended drawings of the embodiments of the present application. Figure 1 -Attached Figure 2 , the technical scheme of the embodiment of the present application is clearly and completely described. Obviously, the described embodiment is a part of the embodiment of the present application, not all of the embodiments. Based on the described embodiment of the present application, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of this application.

[0030] Preparation Example 1

[0031] Preparation of modified barrier agent

[0032] S1. Remove the natural mica material of 200-1000 mesh by sticking it with an adhesive, and repeat the operation for multiple times to prepare a single-layer nanosheet to obtain a single-layer nanosheet, the nanosheet having a sheet diameter of 10-50 μm and a thickness of 1-50 nm. For coupling the modified group of the nanosheet, ethanol, water, and γ-glycidyloxypropyltrimethoxysilane are mixed in a weight ratio of 20:14:1 to obtain a coupling liquid, and then the nanosheet is immersed in the coupling liquid for 15 minutes, the solid-liquid mass ratio is 4:1, and then filtered and dried at 160°C for 1 hour to obtain a modified sheet;

[0033] S2. Mix water, sodium alginate, aluminum chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:2:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add the modified sheet to the emulsion in a solid-liquid ratio of 1:4 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate;

[0034] S3. The intermediate, acetic anhydride and tetrahydrofuran are mixed in a mass ratio of 1:1.5:14, and the mixture is immersed in water for reaction for 40 minutes at a reaction temperature of 40°C, and then washed, filtered and dried to obtain a modified barrier agent.

[0035] Preparation Example 2

[0036] Preparation of modified barrier agent

[0037] S1. The natural montmorillonite material is ultrasonically treated and ground to prepare a single-layer nanosheet to obtain a single-layer nanosheet, the nanosheet having a sheet diameter of 20-80 μm and a thickness of 1-100 nm. The nanosheet is coupled with a modified group by mixing ethanol, water, and γ-glycidyloxypropyltrimethoxysilane in a weight ratio of 20:14:1 to obtain a coupling liquid, and then the nanosheet is immersed in the coupling liquid for 15 minutes, the solid-liquid mass ratio is 1:1, and then filtered and dried at 160°C for 1 hour to obtain a modified sheet;

[0038] S2. Mix water, sodium alginate, magnesium chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:1.5:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add the modified sheet to the emulsion in a solid-liquid ratio of 1:3 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate;

[0039] S3. The intermediate, acetic anhydride and tetrahydrofuran are mixed in a mass ratio of 1:1:12, and the mixture is immersed in water for reaction for 30 minutes at a reaction temperature of 33°C, and then washed, filtered and dried to obtain a modified barrier agent.

[0040] Preparation Example 3

[0041] Preparation of modified barrier agent

[0042] S1. Prepare a single-layer nanosheet by pickling a natural flake graphite material with sulfuric acid and nitric acid and heating to obtain a single-layer nanosheet, wherein the nanosheet has a sheet diameter of 10-90 μm and a thickness of 1-100 nm. For coupling modification groups to the nanosheet, ethanol, water, and γ-glycidyloxypropyltrimethoxysilane are mixed in a weight ratio of 20:14:1 to obtain a coupling liquid, and then the nanosheet is immersed in the coupling liquid for 15 minutes, the solid-liquid mass ratio is 7:1, and then filtered and dried at 160°C for 1 hour to obtain a modified sheet;

[0043] S2. Mix water, sodium alginate, ferric chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:2.5:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add the modified sheet into the emulsion in a solid-liquid ratio of 1:5 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate.

[0044] S3. The intermediate, acetic anhydride and dimethyl sulfoxide are mixed in a mass ratio of 1:2:16, and the mixture is immersed in the reaction for 60 minutes at a reaction temperature of 45°C, and then washed with water, filtered and dried to obtain a modified barrier agent.

[0045] Preparation Comparative Example 1

[0046] The difference between this comparative example and Example 1 is that the modified sheet is not intercalated and mixed with acetic anhydride, but is directly immersed in a polar solvent to prepare a modified barrier agent. The specific operation is as follows:

[0047] S1. Prepare a single-layer nanosheet from natural mica material, the nanosheet has a sheet diameter of 10-50 μm and a thickness of 1-50 nm, mix ethanol, water, and γ-glycidyloxypropyltrimethoxysilane in a weight ratio of 20:14:1 to obtain a coupling liquid, and then soak the nanosheet in the coupling liquid for 15 minutes, the solid-liquid mass ratio is 4:1, filter and dry at 160°C for 1 hour to obtain a modified sheet;

[0048] S2. Mix water, sodium alginate, aluminum chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:2:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add the modified sheet to the emulsion in a solid-liquid ratio of 1:4 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate;

[0049] S3. The intermediate is mixed with tetrahydrofuran in a mass ratio of 1:10, and the mixture is immersed in the mixture for reaction for 30 minutes at a reaction temperature of 35°C, and then washed with water, filtered, and dried to obtain a modified barrier agent.

[0050] Preparation Comparative Example 2

[0051] The difference between this comparative example and Example 1 is that amino modification is not performed, but hydroxyl addition modification is performed. The specific preparation method is as follows:

[0052] S1. Remove the natural mica material of 200-1000 mesh by sticking it with an adhesive, and repeat the operation for many times to prepare a single-layer nanosheet to obtain a single-layer nanosheet, the diameter of the nanosheet is 10-50 μm, and the thickness is 1-50 nm. The nanosheet is coupled with a modified group, and the nanosheet is immersed in a mixed solution of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:2 for 10 hours, filtered and washed to neutrality, and then immersed in 10 mol / L hydrogen peroxide after drying, and slowly ground, washed with water and filtered to obtain a modified sheet;

[0053] S2. Mix water, sodium alginate, aluminum chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:2:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add the modified sheet to the emulsion in a solid-liquid ratio of 1:4 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate;

[0054] S3. The intermediate, acetic anhydride and tetrahydrofuran are mixed in a mass ratio of 1:1.5:14, and the mixture is immersed in water for reaction for 40 minutes at a reaction temperature of 40°C, and then washed, filtered and dried to obtain a modified barrier agent.

[0055] Preparation Comparative Example 3

[0056] The difference between this comparative example and Preparation Example 1 is that the modified sheet is directly soaked with acetic anhydride for reaction. The specific preparation method is as follows:

[0057] S1. Remove the natural mica material of 200-1000 mesh by sticking it with an adhesive, and repeat the operation for multiple times to prepare a single-layer nanosheet to obtain a single-layer nanosheet, the nanosheet having a sheet diameter of 10-50 μm and a thickness of 1-50 nm. For coupling the modified group of the nanosheet, ethanol, water, and γ-glycidyloxypropyltrimethoxysilane are mixed in a weight ratio of 20:14:1 to obtain a coupling liquid, and then the nanosheet is immersed in the coupling liquid for 15 minutes, the solid-liquid mass ratio is 4:1, and then filtered and dried at 160°C for 1 hour to obtain a modified sheet;

[0058] S2. The modified sheet, acetic anhydride and tetrahydrofuran are mixed in a mass ratio of 1:1.5:14, and the mixture is immersed in the mixture for reaction for 40 minutes at a reaction temperature of 40°C, and then washed with water, filtered and dried to obtain a modified barrier agent.

[0059] Preparation Comparative Example 4

[0060] The difference between this comparative preparation example and Preparation Example 1 is that the solid-liquid ratio of the intermediate is changed so that the emulsion reacts in excess. The specific changes are as follows:

[0061] S2. Mix water, sodium alginate, aluminum chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:2:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add the modified sheet to the emulsion in a solid-liquid ratio of 1:8 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate;

[0062] Preparation Comparative Example 5

[0063] The difference between this comparative example and Example 1 is that the modified barrier agent is prepared using granular materials instead of sheet materials. The specific preparation is as follows:

[0064] S1. Couple the modified groups of nano-scale quartz sand, mix ethanol, water and γ-glycidyloxypropyltrimethoxysilane in a weight ratio of 20:14:1 to obtain a coupling liquid, and then soak the quartz sand in the coupling liquid for 15 minutes, with a solid-liquid mass ratio of 4:1, filter and dry at 160°C for 1 hour to obtain modified quartz sand;

[0065] S2. Mix water, sodium alginate, aluminum chloride, attapulgite and surfactant sodium lauryl sulfate in a weight ratio of 5:1:2:0.5:0.05, and prepare an emulsion after high-speed shear stirring. Add modified quartz sand to the emulsion in a solid-liquid ratio of 1:4 and stir. Use a drip hose to slowly add 0.1 mol / L sodium hydroxide solution to adjust the emulsion to slightly alkaline. Use a pH meter to monitor the pH value. The pH value does not exceed 7.8. Filter and wash to obtain an intermediate;

[0066] S3. The intermediate, acetic anhydride and tetrahydrofuran are mixed in a mass ratio of 1:1.5:14, and the mixture is immersed in water for reaction for 40 minutes at a reaction temperature of 40°C, and then washed, filtered and dried to obtain a modified barrier agent.

[0067] Example 1

[0068] This embodiment provides a powder coating for wooden furniture, wherein the modified barrier agent of the wooden furniture powder coating adopts the modified barrier agent of Preparation Example 1, and the specific operation is as follows:

[0069] Step 1: Weigh 45 parts of polyester resin, 30 parts of epoxy resin, 25 parts of titanium dioxide, 0.6 parts of leveling agent, 1 part of sand grain agent, 2 parts of deaerator, 0.5 parts of charging agent, 2 parts of hardening wax powder, 0.3 parts of tertiary amine accelerator, and 10 parts of modified barrier agent by weight, wherein the epoxy resin type is bisphenol A diglycidyl ether.

[0070] The synthesis of the above polyester resin is as follows:

[0071] The polyester resin raw materials include 1,6-hexanediol, 2-methyl-1,3-propanediol, cyclohexanedimethanol, terephthalic acid, isophthalic acid, trimellitic anhydride, trans-butyl diacid, triphenyl phosphite, and F4100 catalyst; the amount of each component by weight is 15 parts, 3 parts, 0.5 parts, 20 parts, 4 parts, 0.5 parts, 5 parts, 0.1 parts, and 0.3 parts, respectively.

[0072] Synthesis process: Place the materials in a reactor, heat to above 200°C, manipulate and adjust the materials for esterification, detect that the acid value is reduced to 7.5 mgKON / g, reduce the temperature to 170°C, introduce nitrogen for protection, heat to 220°C, take samples to detect the acid value, and when the acid value reaches 30 mgKON / g, cool and stir for 30 minutes to obtain a polyester resin material.

[0073] Step 2: Place the above-mentioned various mixed materials in a high-speed mixer and stir them at a speed of 1200 rpm / min to obtain a mixed material after mixing evenly. Melt and extrude the mixed material through an extruder at an extrusion temperature of 80°C. After cooling, crush and sieve to obtain a polyester / epoxy powder coating.

[0074] Example 2

[0075] This embodiment provides a powder coating for wooden furniture, wherein the modified barrier agent of the wooden furniture powder coating adopts the modified barrier agent of Preparation Example 2, and the specific operation is as follows:

[0076] Step 1: Weigh 40 parts of polyester resin, 25 parts of epoxy resin, 20 parts of titanium dioxide, 0.2 parts of leveling agent, 0.5 parts of sand grain agent, 1 part of degassing agent, 0.2 parts of charging agent, 1 part of hardening wax powder, 0.1 parts of tertiary amine accelerator, and 6 parts of modified barrier agent by weight, wherein the epoxy resin type is hydrogenated bisphenol A diglycidyl ether, and the polyester resin is the same as that in Example 1.

[0077] Step 2: Place the above-mentioned various mixed materials in a high-speed mixer and stir them at a speed of 1200 rpm / min to obtain a mixed material after mixing evenly. Melt and extrude the mixed material through an extruder at an extrusion temperature of 80°C. After cooling, crush and sieve to obtain a polyester / epoxy powder coating.

[0078] Example 3

[0079] This embodiment provides a powder coating for wooden furniture, wherein the modified barrier agent of the wooden furniture powder coating adopts the modified barrier agent of Preparation Example 3, and the specific operation is as follows:

[0080] Step 1: Weigh 50 parts of polyester resin, 35 parts of epoxy resin, 30 parts of titanium dioxide, 1 part of leveling agent, 2 parts of sand grain agent, 3 parts of degassing agent, 0.8 parts of charging agent, 3 parts of hardening wax powder, 0.6 parts of tertiary amine accelerator, and 12 parts of modified barrier agent by weight, wherein the epoxy resin type is hexahydrophthalic acid diglycidyl ether, and the polyester resin is the same as that in Example 1.

[0081] Step 2: Place the above-mentioned various mixed materials in a high-speed mixer and stir them at a speed of 1200 rpm / min to obtain a mixed material after mixing evenly. Melt and extrude the mixed material through an extruder at an extrusion temperature of 80°C. After cooling, crush and sieve to obtain a polyester / epoxy powder coating.

[0082] Comparative Example 1

[0083] This comparative example provides a powder coating, wherein the modified barrier of the powder coating is prepared by using the modified barrier in the comparative example 1 to prepare the furniture powder coating, and the remaining steps are the same as those in Example 1.

[0084] Comparative Example 2

[0085] This comparative example provides a powder coating, wherein the modified barrier of the powder coating is prepared by using the modified barrier in the comparative example 2 to prepare the furniture powder coating, and the remaining steps are the same as those in Example 1.

[0086] Comparative Example 3

[0087] This comparative example provides a powder coating, wherein the modified barrier of the powder coating is prepared by using the modified barrier in comparative example 3 to prepare the furniture powder coating, and the remaining steps are the same as those in example 1.

[0088] Comparative Example 4

[0089] This comparative example provides a powder coating, wherein the modified barrier of the powder coating is prepared by using the modified barrier in the comparative example 4 to prepare the furniture powder coating, and the remaining steps are the same as those in Example 1.

[0090] Comparative Example 5

[0091] This comparative example provides a powder coating, wherein the modified barrier of the powder coating is prepared by using the modified barrier in comparative example 5 to prepare the furniture powder coating, and the remaining steps are the same as those in example 1.

[0092] experiment

[0093] First, a variable temperature storage experiment was carried out on the above-mentioned coating, in which the above-mentioned powder coating was maintained at 45 degrees Celsius and 55 degrees Celsius for 8 hours a day, and the rest of the time was at room temperature. The variable temperature storage was carried out continuously for 15 days, and then the powder coating was sprayed on the surface of the wooden material test board using an electrostatic spray gun, and cured in an infrared heating furnace at 130 degrees Celsius for 3 minutes.

[0094] The following performance tests were conducted on the above-mentioned coating films, and the test standards are as follows:

[0095] The paint film flexibility test method is carried out in accordance with the standard GB / T 1731-93.

[0096] Testing standard, no mesh, cracks, peeling

[0097] The paint film adhesion test is carried out according to the white standard of GB 1720-79.

[0098] Testing standards, level one is the best, level seven is the worst

[0099] Impact resistance test method is in accordance with GB / T 1732-93

[0100] Testing standard: impact resistance > 50kg·cm is better

[0101] Paint film bending test (conical shaft) GB 11185-89

[0102] The test standard is that after the test plate rotates 180 degrees around the cylindrical axis within 2-3 seconds, the distance from the crack of the paint film to the small end of the axis is expressed in mm.

[0103] Test data table see table 1 below

[0104] Table 1

[0105]

[0106] A blank test comparison was performed on the powder coatings of each embodiment and comparative example, that is, no temperature change experiment was performed, and the above-mentioned related tests were directly performed on the newly produced powder coatings.

[0107] Test data table see table 2 below

[0108] Table 2

[0109]

[0110]

[0111] In order to more intuitively show that the powder coating of the present application has a more excellent performance, the impact resistance and flexibility in Table 1 are plotted, and the results are as follows: Figure 1 and Figure 2 shown.

[0112] Data and conclusions

[0113] According to Table 1, Table 2, Figure 1 and Figure 2 The data show that the coating effects of Examples 1, 2 and 3 of the present application have no cracking or orange peel particles, the adhesion is level one, the adhesion performance is good, the impact resistance is strong, and the flexibility is also proved to be strong in the paint film bending test.

[0114] The modified sheet in Comparative Example 1 did not undergo acetic anhydride mixing reaction. The coating formed by coating Comparative Example 1 did not crack or show orange peel phenomenon before and after the temperature change test, proving that self-crosslinking did not occur in the temperature change test. However, its adhesion, impact resistance and flexibility were poor after the temperature change test, indicating that the insertion of acetic anhydride during the curing process made the powder coating crosslink more tightly and finely. Combined with the beneficial effects, it can be explained that the presence of acetic anhydride exposes the groups on the surface of the modified sheet during the curing process, thereby greatly enhancing the coating's anti-bending performance.

[0115] The nanosheets of Comparative Example 2 were not amino-modified, but hydroxyl-added. The coating formed by coating Comparative Example 2 performed poorly in the tests before and after the temperature change. Therefore, the hydroxyl addition was not achieved for the subsequent emulsion precipitation and the insertion of acetic anhydride. It can be concluded that the amino addition modification can not only effectively enhance the cross-linking effect during curing, but also can cooperate with the outer layer material to produce a barrier effect during the preparation process, and has a strong resistance to temperature-changing storage.

[0116] The modified sheet of comparative example 3 did not react with the emulsion in step 2 of the present application, but was directly mixed with a solution of acetic anhydride to prepare a modified barrier. The performance of comparative example 3 before the temperature change test was similar to that of the embodiments of the present application, but after the temperature change test, various data indicators were very poor. Not only did the apparent cracks have orange peel particles, but its impact resistance, adhesion and toughness were all unqualified, indicating that the immersion and precipitation of the emulsion on the outside of the modified sheet had a strong protective effect on the modified group, and the difference compared with the embodiments may be due to the consumption of amino groups and acetic anhydride, but it still has a certain enhancement effect.

[0117] In Comparative Example 4, an excess amount of emulsion is used to precipitate and adsorb the outside of the modified sheet. The coating of Comparative Example 4 has very good apparent effects before and after the temperature change test, proving that self-crosslinking does not occur. It has strong resistance to hotter environments and can be stored well. However, the adhesion, impact resistance and toughness of Comparative Example 4 are not good, proving that its crosslinking degree is not good. It can be explained that the emulsion can not only effectively protect the modified sheet in the limited amount of this application, but also does not affect the crosslinking between the modified sheet and the external resin molecules during the curing process. Excessive emulsion precipitation will cause the modified sheet to be unable to crosslink.

[0118] In Comparative Example 5, sheet materials were not used to prepare the modified materials. Instead, particles with smaller volume and surface area were used to prepare the modified materials. The data of Comparative Example 5 showed that its surface had slight cracks after the temperature change test, indicating the occurrence of self-crosslinking. This may be due to too few surface amino groups or too few attachment sites for external precipitation substances, resulting in loose bonding and inability to form effective protection. The adhesion, impact resistance and toughness of Comparative Example 5 did not change much before and after the temperature change test. The crosslinking ability of the granular material modified substance is not as strong as that of the sheet material. The sheet material has obvious effects on the enhancement of powder coatings and the protection means of the present invention.

[0119] The above is a preferred embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles described in the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.

Claims

1. A method for preparing a powder coating for wooden furniture, It is characterized in that A polyester resin, an epoxy resin, titanium dioxide, an additive, and a modified barrier agent are mixed to obtain a mixture, and the mixture is melt-pulverized to obtain a powder coating; wherein the modified barrier agent is obtained by a method comprising the following steps: S1, preparing a sheet material into a single-layer nanosheet, coupling a modified group to the nanosheet to obtain a modified sheet; S2, mixing water, sodium alginate, metal salt, attapulgite and surfactant, stirring to obtain an emulsion, adding the modified sheet to the emulsion at a solid-liquid ratio of 1:3-5, stirring, slowly adding sodium hydroxide solution to adjust the emulsion to slightly alkaline, filtering and washing, to obtain an intermediate; S3. Mix the intermediate, acetic anhydride and polar solvent in a mass ratio of 1:1-2:12-16, soak and react for 30-60 minutes at a reaction temperature of 32-45°C, wash with water, filter and dry to obtain a modified barrier agent.

2. A method for preparing a powder coating for wooden furniture according to claim 1, It is characterized in that The epoxy resin is one of bisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, hexahydrophthalic acid diglycidyl ether and acrylate diglycidyl ether.

3. The method for preparing a powder coating for wooden furniture according to claim 1, It is characterized in that The sheet material in S1 is one of mica, bentonite, montmorillonite or flake graphite, the obtained nanosheet has a sheet diameter of 10 to 50 μm and a thickness of 1 to 50 nm, and the modified group is an amino group.

4. The method for preparing a powder coating for wooden furniture according to claim 3, It is characterized in that The polar solvent in S3 is one of tetrahydrofuran and dimethyl sulfoxide.

5. The method for preparing a powder coating for wooden furniture according to claim 1, It is characterized in that The sheet material is prepared into a single-layer nanosheet by peeling it off through any one of ultrasonic, grinding, nitric acid mixed heating or adhesive peeling.

6. The method for preparing a powder coating for wooden furniture according to claim 1, It is characterized in that The weight ratio of water, sodium alginate, metal salt, attapulgite and surfactant in S2 is 5:1:1.5-2.5:0.5:0.05, wherein the metal salt is one of the alkaline earth metal salts.

7. A method for preparing a powder coating for wooden furniture according to claim 6, It is characterized in that The additives include a leveling agent, a sand grain agent, a degassing agent, a charging agent, a hardening wax powder, and a tertiary amine accelerator. The specific weight percentage of each component in the mixture is as follows: 40-50 parts of polyester resin, 25-35 parts of epoxy resin, 20-30 parts of titanium dioxide, 0.2-1 parts of leveling agent, 0.5-2 parts of sand grain agent, 1-3 parts of degassing agent, 0.2-0.8 parts of charging agent, 1-3 parts of hardening wax powder, 0.1-0.6 parts of tertiary amine accelerator, and 6-12 parts of modified barrier agent.

8. The method for preparing a powder coating for wooden furniture according to claim 7, It is characterized in that The coupling process of the nanosheets in S1 is as follows: Ethanol, water and γ-glycidyloxypropyltrimethoxysilane are mixed in a weight ratio of 20:14:1 to obtain a coupling liquid, and then the nanosheet is immersed in the coupling liquid for 15 minutes, with a solid-liquid mass ratio of 1-7:

1. After filtering, it is dried at 160°C for 1 hour.

9. A powder coating for wooden furniture, It is characterized in that The powder coating for wooden furniture is prepared by the preparation method of the powder coating for wooden furniture according to any one of claims 1 to 8.

10. Application of powder coating for wooden furniture, Features: The powder coating according to claim 9 is used for surface coating of wooden furniture.

Citation Information

Patent Citations

  • Special low-temperature curing powder coating for electrostatic spraying and preparation method thereof

    CN106752759A

  • Heat-stable powder coating for metal surface

    CN111793415A

  • Weather-resistant powder coating as well as preparation method and application thereof

    CN117683440A