Bio-based curved screen protective film and preparation method thereof

The multi-layer structure protective film of bio-based materials solves the problems of environmental pollution and poor fit of 3D curved screens of existing mobile phone protective films, achieves excellent anti-buffering and shaping effects, and reduces the use of petrochemical raw materials. Reduces the risk of environmental pollution.

CN118725757APending Publication Date: 2024-10-01XINLUN ELECTRONIC MATERIALS (CHANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410933749.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing mobile phone protective films use petrochemical derivatives as base materials, which cause environmental pollution and cannot be decomposed after use. They also have poor adhesion to 3D curved screens. Traditional flexible base materials are easy to scratch, and the risk of UV cured films becoming warped is high. Doesn't provide good cushioning.

Method used

It adopts a bio-based curved screen protective film, including a hardened layer, a bio-based film layer, a UV adhesive layer and an organic silicone pressure-sensitive adhesive layer, through polyamide and polyether copolymer elastomer, multi-functional bio-based polyurethane acrylate and organic silicone adhesive layer. A combination of different proportions to achieve excellent anti-cushioning and styling effects.

Benefits of technology

It realizes the use of bio-based materials to prepare protective films, reduces petrochemical refining of raw materials, provides good anti-nail marks and anti-impact effects, takes into account the shaping effect of curved screens, and reduces the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725757A_ABST
    Figure CN118725757A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of mobile phone protective films, and particularly relates to a bio-based curved screen protective film and a preparation method thereof. The bio-based curved screen protective film comprises a hardened layer, a bio-based film layer, a UV adhesive layer, an organic silicon pressure-sensitive adhesive layer and a release film layer which are sequentially arranged from top to bottom. According to the bio-based curved screen protection film, the protection film is prepared from bio-based raw materials, the same curved surface fitting effect is achieved, raw materials from petrochemical refining are greatly reduced, and meanwhile, the human body cannot be hurt even if the bio-based raw material protection film is frequently used; compared with an existing common UV curing film, the UV curing film has the advantages that the special polyamide and polyether copolymer elastomer is adopted as a base material, the excellent anti-buffering effect is achieved by adjusting different proportions of the soft section and the hard section, and meanwhile the good nail mark resisting effect is achieved; and a compact net-shaped cross-linked structure is formed by utilizing polyfunctional urethane acrylate, polyfunctional monomers and oligomers and UV illumination, so that an excellent shaping effect on the curved screen is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mobile phone protective films, and specifically relates to a bio-based curved screen protective film and a preparation method thereof. Background Art

[0002] The current mobile phone protective films on the market are basically made of PET film as the base material, coated with acrylic hardening layer and organic silicone layer on the surface. Among them, PET film is polyethylene terephthalate, the main cost of which is petroleum refining, and it is a petrochemical derivative. Similarly, acrylic acid monomers are also petrochemical refining products. The protective film is directly discarded after use and cannot be decomposed in a short time, causing pollution to the environment. With the development of 3C consumer electronics, the amount of protective film used is increasing, which greatly increases the environmental burden.

[0003] In addition, for 3D curved screen mobile phones, there are currently two ways on the market to solve the problem of curved screen bonding: one is the traditional flexible substrate protective film, which relies on the softness of the substrate to fit the curvature of the curved screen, such as TPU protective film; the other is the emerging UV curing protective film, which uses the protective film adhesive layer to instantly cure and shape under UV irradiation to maintain bonding to the curved screen. Curved screen mobile phones use 3D large-curved glass cover plates, and the corners are more easily scratched and broken than straight-screen phones. However, for the above two bonding methods for curved screens, the traditional flexible substrate protective film has the disadvantages of poor nail print effect, easy scratches on the surface, and poor user experience; UV light curing protective film has better nail print effect than the former, but because the UV adhesive layer is hard and brittle after curing, it cannot provide a good buffering effect for the curved screen. Since PET is the substrate, there is considerable anti-warping stress, and the risk of anti-warping is extremely high. Summary of the invention

[0004] The purpose of the present invention is to provide a bio-based curved screen protective film and a preparation method thereof to solve the above technical problems.

[0005] The first aspect of the present invention provides a bio-based curved screen protective film, comprising:

[0006] The hardening layer, the bio-based film layer, the UV adhesive layer, the silicone pressure-sensitive adhesive layer and the release film layer are arranged in sequence from top to bottom;

[0007] The raw materials of the bio-based membrane layer include polyamide and polyether copolymer elastomer;

[0008] The raw materials of the UV adhesive layer include, by weight: 50-70 parts of multifunctional bio-based polyurethane acrylate; 20-40 parts of multifunctional acrylic UV monomer or oligomer with a functionality ≥6; 5-10 parts of isocyanate curing agent; 1-3 parts of photoinitiator; 0.1-0.5 parts of catalyst; 30-50 parts of first solvent; and the bio-based content of the UV adhesive layer is ≥50%.

[0009] In one embodiment of the present application, the hardened layer is an anti-fingerprint polyacrylic resin hardened layer, and the raw material of the anti-fingerprint polyacrylic resin hardened layer is a conventional anti-fingerprint polyacrylic resin hardening liquid.

[0010] In one embodiment of the present application, in the raw materials of the bio-based membrane layer, the mass ratio of polyamide to polyether copolymer elastomer is 3:1 to 1:3.

[0011] In one embodiment of the present application, the polyamide (hard segment) and polyether (soft segment) copolymer elastomer raw materials can be extracted from plant ends, preferably Arkema bio-based Series, which is made from renewable castor beans, with a bio-based content of up to 70% or more; by adjusting the ratio of hard and soft segments of polyamide and polyether, elastomers of different hardness and softness can be obtained, and the grades are ranked in order of hardness and softness using the Shore hardness meter.

[0012]

[0013] In one embodiment of the present application, the multifunctional bio-based polyurethane acrylate includes at least one of castor oil-based polyurethane acrylate and polyethylene glycol-based polyurethane acrylate; it can be prepared by polymerizing bio-based monomer raw materials castor oil and ethylene glycol;

[0014] The multifunctional acrylic UV monomer or oligomer includes at least one of dipentaerythritol hexaacrylate (DPHA) and hexafunctional acrylic oligomer (Sartomer CN9006NS, CN9110NS),

[0015] The isocyanate curing agent includes at least one of toluene diisocyanate (TDI) and hexamethylene diisocyanate (HDI);

[0016] The photoinitiator includes at least one of 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycyclohexyl phenyl ketone;

[0017] The catalyst includes dibutyltin dilaurate;

[0018] The first solvent includes at least one of toluene, ethyl acetate and butanone.

[0019] In one embodiment of the present application, the raw materials of the organic silica gel layer include, by mass percentage:

[0020] The second solvent is 30%-60%, the silicone gum is 5%-20%, the silicone resin is 25%-50%, the cross-linking agent is 0.5%-1%, the adhesion promoter is 0.5%-1% and the catalyst is 0.5%-1.5%, and the total is 100%.

[0021] In one embodiment of the present application, the second solvent is at least one of ethyl acetate, toluene, and butanone;

[0022] The silicone rubber is one or both of vinyl-terminated polydimethylsiloxane and vinyl-terminated polydimethylphenylsiloxane;

[0023] The silicone resin is MQ methyl silicone resin or MQ methyl phenyl silicone resin;

[0024] The cross-linking agent is hydrogen-containing silicone oil;

[0025] The adhesion promoter is a composite carboxyl-terminated organosiloxane;

[0026] The catalyst is a platinum catalyst.

[0027] In one embodiment of the present application, the hardened layer is an anti-fingerprint polyacrylic resin hardened layer;

[0028] The release film layer is a fluorine release film or a non-silicon release film, and the release force is less than 10g / 25mm; preferably, the release film substrate is made of recycled PET.

[0029] In one embodiment of the present application, the thickness of the hardened layer is 1-5 um; the thickness of the bio-based film layer is 30-100 um; the thickness of the UV adhesive layer is 50-100 um; and the thickness of the silicone pressure-sensitive adhesive layer is 10-20 um.

[0030] Accordingly, the second aspect of the present invention provides a method for preparing the bio-based curved screen protective film as described above, comprising:

[0031] Through the hot melt coating process, polyamide and polyether copolymer elastomer are extruded into a film in a molten state at 200-300°C to obtain a special optical grade bio-based film layer;

[0032] The anti-fingerprint polyacrylic acid resin hard liquid is coated on one surface of the bio-based film layer through micro-concave, and a hardened layer is obtained by UV curing;

[0033] The raw materials of the UV adhesive layer are mixed in proportion and then coated on the other side of the bio-based film layer through a slot-die, and then heated and cured in an oven to obtain a surface-dried UV adhesive layer;

[0034] The raw materials of the organic silicone layer are mixed in proportion and then coated on the surface of the UV adhesive layer through a slot-die, and then heated and cured in an oven to obtain an organic silicone layer;

[0035] Finally, the prepared organic silicone layer is laminated to a release film to form a finished bio-based curved screen protective film;

[0036] The above gluing processes are all completed under yellow light conditions.

[0037] The beneficial effects of the present invention are that the bio-based curved screen protective film of the present invention is prepared by using bio-based raw materials to prepare the protective film, and the same curved surface fitting effect is achieved, but the raw materials from petrochemical extraction are greatly reduced. At the same time, the frequent use of the bio-based raw material protective film will not cause harm to the human body; compared with the existing ordinary UV curing film, the present invention adopts a special polyamide and polyether copolymer elastomer as the base material, and achieves excellent anti-buffering effect by adjusting different proportions of soft / hard segments, while taking into account a good anti-nail mark effect; using multi-functional polyurethane acrylate, multi-functional monomers and oligomers, UV light forms a tight network cross-linking structure, which has an excellent shaping effect on the curved screen.

[0038] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and the drawings.

[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 is a schematic structural diagram of the bio-based curved screen protective film of the present invention;

[0042] Figure 2 This is a table showing the physical properties of the protective films of the respective examples.

[0043] In the figure:

[0044] Hardening layer 1, bio-based film layer 2, UV adhesive layer 3, silicone pressure-sensitive adhesive layer 4 and release film layer 5. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Example 1

[0047] like Figure 1 As shown, a bio-based curved screen protective film of this embodiment has a multi-layer structure, including a hardening layer 1, a bio-based film layer 2, a UV adhesive layer 3, an organic silicone layer 4, and a release film layer 5; wherein

[0048] The hardened layer is an anti-fingerprint polyacrylic resin hardened layer with a thickness of 3um;

[0049] The bio-based membrane layer is 30um thick and uses a copolymer elastomer of polyamide (hard segment) and polyether (soft segment), with a hard segment / soft segment mass ratio of 25:75. Arkema bio-based Heat to 200℃ to melt, and cool to form a film by extrusion;

[0050] The thickness of the UV adhesive layer is 50um, and the raw materials include: 50 parts of castor oil-based polyurethane acrylate, 30 parts of dipentaerythritol hexaacrylate (DPHA), 5 parts of hexamethylene diisocyanate (HDI), 2 parts of 1-hydroxycyclohexyl phenyl ketone, 0.1 parts of dibutyltin dilaurate, and 30 parts of solvent ethyl ester;

[0051] The thickness of the organic silica gel layer is 15 μm. In terms of mass percentage, the raw materials include 50% of solvent ethyl ester, 8% of vinyl-terminated polydimethylsiloxane, 40% of MQ methyl silicone resin, 0.5% of hydrogenated silicone oil, 0.5% of composite carboxyl-terminated organic siloxane and 1% of platinum catalyst, the total of which is 100%;

[0052] The release film layer is a 50um thick fluorine release film with a release force of 5gf / 25mm;

[0053] Preparation process:

[0054] The hardening layer is coated on the surface of the bio-based membrane layer through micro-concaves, the UV adhesive layer is coated on the other side of the bio-based membrane layer through slit extrusion, and then the organic silicone layer is also coated on the UV adhesive layer through slit extrusion, and finally the fluoroplastic release film is coated to form a protective film.

[0055] Example 2

[0056] like Figure 1 As shown, a bio-based curved screen protective film of this embodiment has a multi-layer structure, including a hardening layer 1, a bio-based film layer 2, a UV adhesive layer 3, an organic silicone layer 4, and a release film layer 5; wherein

[0057] The hardened layer is anti-fingerprint polyacrylic resin with a hardened layer thickness of 3um;

[0058] The bio-based membrane layer is 50um thick and uses a copolymer elastomer of polyamide (hard segment) and polyether (soft segment), with a hard segment / soft segment mass ratio of 50:50, preferably Arkema bio-based Heat to 230℃ to melt, and cool to form a film by extrusion;

[0059] The thickness of the UV adhesive layer is 50um, and the above substances are mixed with 70 parts of castor oil-based polyurethane acrylate, 40 parts of dipentaerythritol hexaacrylate (DPHA), 6 parts of hexamethylene diisocyanate (HDI), 2 parts of 1-hydroxycyclohexyl phenyl ketone, 0.2 parts of dibutyltin dilaurate, and 30 parts of solvent ethyl ester;

[0060] The thickness of the organic silica gel layer is 15 μm, and by mass percentage, it includes 50% of solvent ethyl ester, 8% of vinyl-terminated polydimethylsiloxane, 40% of MQ methyl silicone resin, 0.5% of hydrogenated silicone oil, 0.5% of composite carboxyl-terminated organic siloxane and 1% of platinum catalyst, the total of which is 100%;

[0061] The release film layer is 50um fluorine release film with a release force of 5gf / 25mm;

[0062] The preparation process is the same as that of Example 1.

[0063] Example 3

[0064] like Figure 1 As shown, a bio-based curved screen protective film of this embodiment has a multi-layer structure, including a hardening layer 1, a bio-based film layer 2, a UV adhesive layer 3, an organic silicone layer 4, and a release film layer 5; wherein

[0065] The hardened layer is an anti-fingerprint polyacrylic resin hardened layer with a thickness of 3um;

[0066] The bio-based membrane layer is 50um thick and uses a copolymer of polyamide (hard segment) and polyether (soft segment) with a hard segment / soft segment mass ratio of 75:25. Arkema bio-based Heat to 250℃ to melt, and cool to form a film by extrusion;

[0067] The thickness of the UV adhesive layer is 50um, and the above substances are mixed with 70 parts of polyethylene glycol-based polyurethane acrylate, 40 parts of dipentaerythritol hexaacrylate (DPHA), 6 parts of hexamethylene diisocyanate (HDI), 1 part of 1-hydroxycyclohexyl phenyl ketone, 1 part of 2-hydroxy-2-methyl-1-phenyl acetone, 0.1 part of dibutyltin dilaurate, and 30 parts of solvent ethyl ester;

[0068] The thickness of the organic silica gel layer is 20 μm, and the mass percentage includes 40% of a mixed solvent of ethyl ester and toluene, 8% of vinyl-terminated polydimethylsiloxane, 50% of MQ methyl silicone resin, 0.5% of hydrogenated silicone oil, 0.5% of a composite carboxyl-terminated organic siloxane, and 1% of a platinum catalyst, the total of which is 100%;

[0069] The release film layer is a 50um thick fluorine release film with a release force of 5gf / 25mm;

[0070] The preparation process is the same as that of Example 1.

[0071] Example 4

[0072] like Figure 1 As shown, a bio-based curved screen protective film of this embodiment has a multi-layer structure, including a hardening layer 1, a bio-based film layer 2, a UV adhesive layer 3, an organic silicone layer 4, and a release film layer 5; wherein

[0073] The hardened layer is an anti-fingerprint polyacrylic resin hardened layer with a thickness of 3um;

[0074] The bio-based membrane layer is 70um thick and uses a copolymer elastomer of polyamide (hard segment) and polyether (soft segment), with a hard segment / soft segment mass ratio of 50:50, preferably Arkema bio-based Heat to 230℃ to melt, and cool to form a film by extrusion;

[0075] The thickness of the UV adhesive layer is 50um, and the above substances are mixed with 60 parts of castor oil-based polyurethane acrylate, 20 parts of dipentaerythritol hexaacrylate (DPHA), 20 parts of hexafunctional acrylic oligomer, 6 parts of hexamethylene diisocyanate (HDI), 2 parts of 1-hydroxycyclohexyl phenyl ketone, 0.2 parts of dibutyltin dilaurate, and 30 parts of solvent ethyl ester;

[0076] The thickness of the organic silica gel layer is 15 μm, and in terms of mass percentage, it includes 50% of solvent ethyl ester, 8% of vinyl-terminated polydimethylsiloxane, 40% of MQ methyl silicone resin, 0.5% of hydrogenated silicone oil, 0.5% of composite carboxyl-terminated organic siloxane and 1% of platinum catalyst, the total of which is 100%;

[0077] The release film layer is 50um fluorine release film with a release force of 5gf / 25mm;

[0078] The preparation process is the same as that of Example 1.

[0079] See also Figure 2 , are the physical properties of the protective films of each example.

[0080] From the data in the table:

[0081] 1) By adjusting the ratio of bio-based soft / hard segments, protective film samples with different softness can be obtained. When the soft segment accounts for a larger proportion, the energy absorption effect of falling ball impact is better, but the surface hardness is poor; conversely, when the hard segment ratio increases, the energy absorption of falling ball impact of the protective film decreases, but the surface hardness effect is better;

[0082] 2) In horizontal comparison, the protective film of the present invention has better surface hardness and impact resistance than TPU protective film; compared with ordinary UV curing protective film, it has better impact resistance and excellent curved surface shaping effect; in addition, since the mobile phone has an under-screen fingerprint unlocking function, the ordinary UV protective film PET substrate (biaxially stretched) requires die-cutting at a specific angle and has a low utilization rate, while the substrate of the present invention is made by a bio-based casting method and can be conventionally cut, which greatly improves the utilization rate.

[0083] The various devices selected in this application (components whose specific structures are not described) are all universal standard parts or components known to technical personnel in this field, and their structures and principles can be known to technical personnel through technical manuals or through conventional experimental methods.

[0084] In the description of the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0085] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0086] In the several embodiments provided in the present application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. The device embodiments described above are merely schematic. For example, the division of the units is only a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some communication interfaces, and the indirect coupling or communication connection of devices or units can be electrical, mechanical or other forms.

[0087] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.

[0088] In addition, each functional unit in each embodiment of the present invention may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit.

[0089] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A bio-based curved screen protective film, characterized in that: It includes a hardening layer, a bio-based film layer, a UV adhesive layer, a silicone pressure-sensitive adhesive layer and a release film layer which are arranged in sequence from top to bottom; in The raw materials of the bio-based membrane layer include polyamide and polyether copolymer elastomer; The raw materials of the UV adhesive layer include, by weight: 50-70 parts of multifunctional bio-based polyurethane acrylate; 20-40 parts of multifunctional acrylic UV monomer or oligomer with a functionality ≥6; 5-10 parts of isocyanate curing agent; 1-3 parts of photoinitiator; 0.1-0.5 parts of catalyst; 30-50 parts of first solvent; and the bio-based content of the UV adhesive layer is ≥50%.

2. The bio-based curved screen protective film according to claim 1, characterized in that: In the raw materials of the bio-based membrane layer, the mass ratio of polyamide to polyether copolymer elastomer is 3:1 to 1:

3.

3. The bio-based curved screen protective film according to claim 1, characterized in that: The multifunctional bio-based polyurethane acrylate includes at least one of castor oil-based polyurethane acrylate and polyethylene glycol-based polyurethane acrylate; The multifunctional acrylic UV monomer or oligomer includes at least one of dipentaerythritol hexaacrylate and hexafunctional acrylic oligomer. The isocyanate curing agent includes at least one of toluene diisocyanate and hexamethylene diisocyanate; The photoinitiator includes at least one of 2-hydroxy-2-methyl-1-phenylpropanone and 1-hydroxycyclohexyl phenyl ketone; The catalyst includes dibutyltin dilaurate; The first solvent includes at least one of toluene, ethyl acetate and butanone.

4. The bio-based curved screen protective film according to claim 1, characterized in that: The raw materials of the organic silica gel layer include, by mass percentage: The second solvent is 30%-60%, the silicone gum is 5%-20%, the silicone resin is 25%-50%, the cross-linking agent is 0.5%-1%, the adhesion promoter is 0.5%-1% and the catalyst is 0.5%-1.5%, and the total is 100%.

5. The bio-based curved screen protective film according to claim 1, characterized in that: The second solvent is at least one of ethyl acetate, toluene and butanone; The silicone rubber is one or both of vinyl-terminated polydimethylsiloxane and vinyl-terminated polydimethylphenylsiloxane; The silicone resin is MQ methyl silicone resin or MQ methyl phenyl silicone resin; The cross-linking agent is hydrogen-containing silicone oil; The adhesion promoter is a composite carboxyl-terminated organosiloxane; The catalyst is a platinum catalyst.

6. The bio-based curved screen protective film according to claim 1, characterized in that: The hardened layer is an anti-fingerprint polyacrylic resin hardened layer; The release film layer is a fluorine release film or a non-silicone release film, and the release force is less than 10g / 25mm.

7. The bio-based curved screen protective film according to claim 1, characterized in that: The thickness of the hardened layer is 1-5um; Bio-based membrane layer 30-100um; UV adhesive layer 50-100um; Silicone pressure-sensitive adhesive layer 10-20um.

8. A method for preparing a bio-based curved screen protective film according to any one of claims 1 to 7, characterized in that: include: Through the hot melt coating process, polyamide and polyether copolymer elastomer are extruded into a film in a molten state at 200-300°C to obtain a special optical grade bio-based film layer; The anti-fingerprint polyacrylic acid resin hard liquid is coated on one surface of the bio-based film layer through micro-concave, and a hardened layer is obtained by UV curing; The raw materials of the UV adhesive layer are mixed in proportion and then coated on the other side of the bio-based film layer through a slot-die, and then heated and cured in an oven to obtain a surface-dried UV adhesive layer; The raw materials of the organic silicone layer are mixed in proportion and then coated on the surface of the UV adhesive layer through a slot-die, and then heated and cured in an oven to obtain an organic silicone layer; Finally, the prepared organic silicone layer is laminated to a release film to form a finished bio-based curved screen protective film; The above gluing processes are all completed under yellow light conditions.