Polyurethane adhesive as well as preparation method and application thereof
By using isocyanate and other materials in polyurethane adhesives to react to form component A and component B, combined with curing accelerators and silane coupling agents, the problems of high viscosity, poor ink matching and insufficient cooking resistance of solvent-free adhesives are solved, achieving The effects of low viscosity, good ink adaptability, hydrolysis resistance and high adhesion improve the performance of soft bags.
Patent Information
- Application Number
- CN202410862114.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
The existing solvent-free adhesives used for retort-type aluminum-plastic packaging have high viscosity, require heating for coating, have poor ink matching, poor retort resistance and aluminum foil adhesion.
A solvent-free polyurethane adhesive is used to obtain component A and component B through the reaction of isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol, combined with a curing accelerator and Silane coupling agent forms an adhesive with low viscosity, good ink adaptability, strong adhesion resistance to 121℃, 40min cooking, and hydrolysis resistance.
It improves the sealing performance and high-temperature cooking resistance of the soft bag, enhances the adaptability and wetting performance of the ink, ensures the hydrolysis resistance and bonding strength of the adhesive, and meets the requirements of the flexible packaging industry.
Smart Images

Figure BDA0004919347990000141 
Figure BDA0004919347990000151
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite flexible packaging, and specifically relates to a polyurethane adhesive and a preparation method and application thereof. Background Art
[0002] High temperature resistant retort bags are one type of composite flexible packaging. They are made by compounding PET, PA, AL, CPP and other film materials with retort resistant adhesives to form bags for packaging food, medicine, medical equipment, etc., and can withstand high temperature steam heating and sterilization. They are also called retortable flexible packaging or soft cans. Solvent-free adhesives for retort aluminum-plastic packaging are divided into two types: outer layer and inner layer according to the different adhesive layers. The solvent-free adhesive of the outer layer of the retort aluminum-plastic packaging film is used for the compound of PET and AL (or PA and AL), which has the function of barrier and anti-puncture. At the same time, for the beautiful appearance of the product and the need for printing logos, the ink layer will be printed on the PET or PA layer; the solvent-free adhesive of the inner layer of the retort aluminum-plastic packaging film is used for the compound of AL and RCPP (or AL and NY), which has heat sealing properties.
[0003] However, the solvent-free adhesives currently used in retort-type aluminum-plastic packaging generally have the following problems: (1) high viscosity, requiring heating during coating; (2) poor compatibility with ink; and (3) poor retort resistance and poor adhesion to aluminum foil.
[0004] Therefore, the existing polyurethane adhesive for flexible packaging needs to be improved. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a polyurethane adhesive and a preparation method and application thereof. The polyurethane adhesive is solvent-free, low-viscosity, has good ink adaptability, good wetting performance, is resistant to 121°C, 40min boiling, has strong bonding strength, and has good hydrolysis resistance, so that it can be used in the field of soft packaging, which can not only improve the sealing performance of the soft packaging bag, but also improve its boiling resistance.
[0006] In one aspect of the present invention, the present invention provides a polyurethane adhesive. According to an embodiment of the present invention, it includes component A and component B; the component A includes an isocyanate-terminated polyurethane prepolymer; the isocyanate-terminated polyurethane prepolymer is obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol; the component B includes a hydroxyl-terminated polyurethane prepolymer; the hydroxyl-terminated polyurethane prepolymer is obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol.
[0007] Thus, the polyurethane adhesive is realized. The polyurethane adhesive is solvent-free, low-viscosity, has good ink adaptability, good wetting performance, resistance to 121°C, 40min boiling, strong bonding force, and good hydrolysis resistance, so that it can be used in the field of soft packaging, which can not only improve the sealing performance of the soft packaging bag, but also improve its high-temperature boiling resistance.
[0008] In addition, the polyurethane adhesive according to the present invention also has the following technical features:
[0009] In some embodiments of the present invention, the weight ratio of component A to component B is 1-1.5: 1. Thus, component A and component B react after being mixed in this ratio to form macromolecules and cross-link and solidify, and substantially no CO2 is released during the reaction, which is environmentally friendly, and makes the polyurethane adhesive solvent-free, low in viscosity, good in ink adaptability, good in wetting performance, resistant to 121°C, 40min cooking, strong in bonding strength, and good in hydrolysis resistance.
[0010] In some embodiments of the present invention, the viscosity of component A is 2000mPa·s-5000mPa·s, and the viscosity of component B is 1000mPa·s-3000mPa·s. Thus, the polyurethane adhesive has the characteristics of being solvent-free, low-viscosity, good ink adaptability, good wetting performance, resistance to 121°C, 40min cooking, strong bonding strength, and good hydrolysis resistance.
[0011] In some embodiments of the present invention, in the raw materials of component A, the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol is (50-70): (20-30): (10-20): (10-20): (5-10). Thus, the terminal group of component A is an isocyanate group, and the polyurethane adhesive has the characteristics of being solvent-free, low viscosity, good ink adaptability, good wetting performance, resistance to 121°C, 40min cooking, strong adhesion and good hydrolysis resistance.
[0012] In some embodiments of the present invention, in the raw materials of component B, the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol is (1-10): (20-60): (5-20): (10-20): (1-10). Thus, the terminal group of component B is hydroxyl, and the polyurethane adhesive has the characteristics of being solvent-free, low viscosity, good ink adaptability, good wetting performance, resistance to 121°C, 40min cooking, strong adhesion and good hydrolysis resistance.
[0013] In some embodiments of the present invention, the B component also includes a curing accelerator and a silane coupling agent; preferably, the weight ratio of the terminal hydroxyl polyurethane prepolymer, the curing accelerator and the silane coupling agent is (90-100): (0.001-0.1): (0.1-3). The embodiment of the present invention adopts a synthetic method to prepare the terminal hydroxyl prepolymer and the curing accelerator and the silane coupling agent to obtain the B component, rather than a polyol compounding method, which will make the A component and the B component have more similarities in composition, thereby enhancing the similarity and compatibility of the A and B components, thereby improving the adaptability of the ink to a certain extent.
[0014] In some embodiments of the present invention, the weight average molecular weight of the branched polyester polyol is 500-2000. Thus, the polyurethane adhesive is solvent-free, low-viscosity, has good ink adaptability, good wetting performance, is resistant to 121°C, 40min cooking, has strong adhesion, and has good hydrolysis resistance.
[0015] In some embodiments of the present invention, the branched polyester polyol is obtained by reacting an aromatic polyacid or an aliphatic polyacid with a polyol having a side branch.
[0016] In some embodiments of the present invention, the aromatic polyacid includes at least one of aromatic dibasic acids.
[0017] In some embodiments of the present invention, the aliphatic polybasic acid includes at least one of an aliphatic dibasic acid.
[0018] In some embodiments of the present invention, the polyol with side branches includes at least one of a diol with side branches, a triol with side branches, and a tetraol with side branches.
[0019] In some embodiments of the present invention, the mass ratio of the diol with side branches, the triol with side branches and the tetraol with side branches is (90-100):(0-5):(0-5).
[0020] In some embodiments of the present invention, the side-branched polyol includes at least one of neopentyl glycol, 2-methyl-2-ethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, and 2,4-diethyl-1,5-pentanediol.
[0021] Polyurethanes made from polyester polyols synthesized from aromatic dibasic acids and diols have excellent hydrolysis resistance, heat resistance and adhesion due to the presence of a large number of benzene ring structures. Polyurethanes synthesized from polyester polyols generated by the reaction of long-chain aliphatic dibasic acids and diols have excellent toughness and softness due to the presence of long carbon chain structures. At the same time, they have more polar groups such as ester groups and urethane groups, and the cohesive strength and adhesion are guaranteed. Diols with side branches can make the synthesized polyurethane have lower viscosity and better adhesive fluidity, thereby achieving the purpose of reducing the viscosity of solvent-free adhesives. As a result, the hydrolysis resistance of branched polyester polyols can be greatly improved, the viscosity of the system can be reduced, and the advantages of polyurethane adhesives being solvent-free, low-viscosity, good ink adaptability, good wetting properties, resistance to 121°C, 40min boiling, strong adhesion, and good hydrolysis resistance can be achieved.
[0022] In some embodiments of the present invention, the bio-based polymer polyol is obtained by reacting vegetable oil, phthalic anhydride and polyol. Thus, the bio-based polymer polyol synthesized from phthalic anhydride and polyol can improve the hydrolysis resistance and heat resistance of the adhesive, achieve low viscosity of the polyurethane adhesive, good matching with ink, good wetting performance, and strong bonding effect.
[0023] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned adhesive. According to an embodiment of the present invention, the method comprises:
[0024] (1) mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol in a first ratio to obtain component A;
[0025] (2) mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol in a second ratio, and adding a curing accelerator and a silane coupling agent to obtain component B;
[0026] (3) Mixing the A component and the B component to obtain an adhesive.
[0027] By mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol in a first ratio, the NCO group of isocyanate reacts chemically with the OH group of polyol to obtain a carbamate bond (urethane), but the isocyanate is excessive, and an isocyanate-terminated polyurethane prepolymer is eventually formed to obtain component A with an isocyanate end group. By mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol in a second ratio, the NCO group of isocyanate reacts chemically with the OH group of polyol to obtain a carbamate bond (urethane), but the polyol is excessive, and a hydroxyl-terminated polyurethane prepolymer is eventually formed to obtain a hydroxyl-terminated polyurethane prepolymer, and the prepolymer is mixed with a curing accelerator and a silane coupling agent to obtain a component B, and then the component A is mixed with the component B. The terminal isocyanate prepolymer component A containing NCO groups reacts with the terminal hydroxyl prepolymer component B containing OH groups again to generate a urethane (urethane) structure with a larger molecular weight and a more compact structure. The urethane can also continue to react with isocyanate to form allophanate. These reactions are the main reactions that occur during the production and curing of two-component polyurethane coatings. Therefore, the method can be used to prepare a polyurethane adhesive that is solvent-free, low-viscosity, has good matching properties with inks, good wetting properties, is resistant to boiling at 121°C, has strong adhesion to aluminum foil after 40 minutes, and has good hydrolysis resistance.
[0028] In a third aspect of the present invention, a flexible bag is provided. According to an embodiment of the present invention, the flexible bag comprises the above-mentioned polyurethane adhesive or the polyurethane adhesive prepared by the above-mentioned method. As a result, the flexible bag has excellent sealing and high temperature cooking resistance, good ink adaptability, good wetting performance, good hydrolysis resistance, and meets the requirements of the flexible packaging industry.
[0029] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0030] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.
[0031] In one aspect of the present invention, the present invention proposes a polyurethane adhesive. According to an embodiment of the present invention, it includes component A and component B; the component A includes an isocyanate-terminated polyurethane prepolymer; the isocyanate-terminated polyurethane prepolymer is obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol, wherein the NCO group of the isocyanate reacts chemically with the OH group of the polyol to obtain a carbamate bond (urethane), but the isocyanate is excessive, and an isocyanate-terminated polyurethane prepolymer is eventually formed; the component B includes a hydroxyl-terminated polyurethane prepolymer; the hydroxyl-terminated polyurethane prepolymer is obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol, wherein the NCO group of the isocyanate reacts chemically with the OH group of the polyol to obtain a carbamate bond (urethane), but the polyol is excessive, and a hydroxyl-terminated polyurethane prepolymer is eventually formed.
[0032] The polyurethane adhesive described in the present invention comprises component A and component B, and the terminal isocyanate prepolymer component A containing NCO group reacts with the terminal hydroxyl prepolymer component B containing OH group to generate a carbamate (urethane) structure with larger molecular weight and more compact structure, and the urethane can also continue to react with isocyanate to generate allophanate. These reactions are the main reactions occurring in the production and curing process of two-component polyurethane coating. Component A and component B are obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol, wherein the branched polyester polyol is due to the influence of the steric hindrance of the side chain, and the intermolecular entanglement is smaller, thereby having a larger activity space, which is equivalent to the increase of the molecular free volume, and the fluidity is enhanced, so that the system can present a lower viscosity, and the increase of the side chain can reduce the hydrophilic group in the polyurethane as much as possible, and the steric hindrance also protects the contact of the carbamate group with water, thereby realizing the hydrolysis resistance effect of the adhesive. The ether bonds in the molecular structure of polyether polyols have low cohesive energy and are easy to rotate. Therefore, the polyurethane materials prepared from them have good low-temperature flexibility and excellent hydrolysis resistance. The raw material system has low viscosity, is easily miscible with isocyanates, additives and other components, and has excellent processing performance. Bio-based polymer polyols have a multi-hydroxy and long-chain fatty structure, and have good water resistance and flexibility. The intermolecular cohesion of the polycarbonate bonds in the polycarbonate polyol molecular chain is strong, which can make the adhesive have a higher glass transition temperature, mechanical properties and good hydrolysis resistance.
[0033] Therefore, the polyurethane adhesive is solvent-free, low-viscosity, has good ink adaptability, good wetting performance, can withstand cooking at 121° C. for 40 minutes, has strong bonding strength, and has good hydrolysis resistance.
[0034] It should be noted that in the present invention, the isocyanate is a conventional material in the art, and those skilled in the art can select specific types according to actual needs. For example, the isocyanate includes at least one of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate. Among them, diphenylmethane diisocyanate and isophorone diisocyanate are preferred. Diphenylmethane diisocyanate generally has three isomers of 4,4'-MDI, 2,4'-MDI and 2,2'-MDI. There are commercially available MDI-100 and MDI-50 to choose from. It has high reactivity, low volatility, and relatively low toxicity to the human body. It is a better choice for food laminating glue. Generally, hexamethylene diisocyanate is reacted with water to make biuret diisocyanate, or catalyzed to form a trimer for reuse. Isophorone diisocyanate has a low vapor pressure, excellent light stability and chemical resistance, and is a better choice as a food laminating glue material.
[0035] It should be noted that, in the present invention, the polyether polyol is a conventional material in the art, and those skilled in the art can select specific types according to actual needs. For example, the polyether polyol can include at least one of polyethylene glycol, polypropylene glycol and polytetrahydrofuran diol.
[0036] It should be noted that, in the present invention, the polycarbonate polyol is a conventional material in the art, and those skilled in the art can select a specific type according to actual needs. For example, the polycarbonate polyol can be an aliphatic polycarbonate diol and / or an aromatic polycarbonate diol. The polyurethane prepared from the polycarbonate diol has excellent hydrolysis resistance.
[0037] It should be noted that in the present invention, the weight ratio of component A to component B is 1-1.5:1, for example, it can be 1:1, 1.05:1, 1.15:1, 1.25:1, 1.35:1, 1.45:1, 1.5:1 and any range between any two values, and those skilled in the art can adjust it according to actual needs. Thus, component A and component B react after mixing in this ratio to form macromolecules and cross-link and solidify, and there is basically no release of CO2 during the reaction process, which is environmentally friendly, so that the polyurethane adhesive has no solvent, low viscosity, good ink adaptability, good wetting performance, resistance to 121°C, 40min cooking, strong adhesion, and good hydrolysis resistance.
[0038] According to an embodiment of the present invention, the viscosity of component A is 2000mPa·s-5000mPa·s, for example, it may be 2500mPa·s, 3000mPa·s, 3500mPa·s, 4000mPa·s, 4500mPa·s, 5000mPa·s, etc., and the viscosity of component B is 1000mPa·s-3000mPa·s, for example, it may be 1000mPa·s, 1500mPa·s, 2000mPa·s, 2500mPa·s, 3000mPa·s, etc. The inventors found that if the viscosity of component A is less than 2000mPa·s, the NCO content of component A is too high and the weight-average molecular weight is too small, thereby affecting the construction viscosity after the two components are mixed, and affecting the bonding effect and appearance. If the viscosity of component A is greater than 5000mPa·s, the NCO content of component A is too low, and the hydroxyl group OH of component B cannot be completely reacted, affecting the bonding effect and appearance, and affecting the construction viscosity after the two components are mixed; if the viscosity of component B is less than 1000mPa·s, the weight-average molecular weight of component B is too small, affecting the construction viscosity after the two components are mixed, and affecting the bonding effect and appearance. If the viscosity of component B is greater than 3000mPa·s, the weight-average molecular weight of component B is too large, affecting the construction viscosity after the two components are mixed. Therefore, the present application adopts a polyurethane adhesive obtained by mixing component A with a viscosity of 2000mPa·s-5000mPa·s and component B with a viscosity of 1000mPa·s-3000mPa·s, which can achieve the polyurethane adhesive being solvent-free, low-viscosity, having good ink adaptability, good wetting properties, resistance to 121°C, 40min cooking, strong adhesion, and good hydrolysis resistance.
[0039] According to an embodiment of the present invention, in the raw materials of component A, the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol is (50-70): (20-30): (10-20): (10-20): (5-10). Therefore, by adopting the above-mentioned ratio range for each raw material of component A in the present application, it can not only ensure that the terminal group of component A is an isocyanate group, but also take into account the heat and moisture resistance, strong adhesion, low viscosity, hydrolysis resistance and good ink adaptability of the adhesive.
[0040] According to an embodiment of the present invention, in the raw materials of component B, the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol is (1-10): (20-60): (5-20): (10-20): (1-10). Therefore, by controlling the raw materials of component B in the present application within the above-mentioned ratio range, it can not only ensure that the terminal group of component B is hydroxyl, but also take into account the heat and moisture resistance, strong adhesion, low viscosity, hydrolysis resistance and good ink adaptability of the adhesive.
[0041] According to an embodiment of the present invention, the B component further includes a curing accelerator and a silane coupling agent. In some embodiments of the present invention, the hydroxyl-terminated prepolymer, the curing accelerator and the silane coupling agent are mixed to obtain the B component. Since the hydroxyl group OH in the B component is excessive, it is closer to the nature of alcohol as a whole. Therefore, compared with the A component, the compatibility of the B component with the silane coupling agent is better. The curing accelerator is a type of substance that helps the NCO group to react with the OH group. If added to the A component, it will promote the side reaction of the NCO group with the moisture in the air, which is not conducive to the stable storage of the A component. Therefore, it is more appropriate to add the curing accelerator to the B component. .
[0042] According to an embodiment of the present invention, the weight ratio of the terminal hydroxyl polyurethane prepolymer, the curing accelerator and the silane coupling agent is (90-100): (0.001-0.1): (0.1-3). The inventors found that if the weight ratio of the terminal hydroxyl polyurethane prepolymer, the curing accelerator and the silane coupling agent in the B component does not meet the above ratio range, it will lead to excessive small molecule additives in the B component, resulting in a decrease in the overall bonding strength of the adhesive. Therefore, the B component in the present application adopts the above ratio range, which can not only ensure that the B component maintains a suitable molecular weight and performance, but also take into account the moisture and heat resistance, strong adhesion, low viscosity, hydrolysis resistance and good ink adaptability of the adhesive.
[0043] It should be noted that, in the present invention, the curing accelerator is a conventional material in the art, and those skilled in the art can select specific types according to actual needs. For example, the curing accelerator can be at least one of stannous octoate, dibutyltin dilaurate, dibutyltin, tetrabutyl titanate, tetraisopropyl titanate, bismorpholinyl diethyl ether and dimorpholine triethyl ether. In the present invention, the silane coupling agent is a conventional material in the art, and those skilled in the art can select specific types according to actual needs. For example, the silane coupling agent can be at least one of KH560, KH570 and KH580.
[0044] According to an embodiment of the present invention, the weight average molecular weight of the branched polyester polyol is 500-2000. Thus, the branched polyester polyol can be ensured to have better hydrolysis resistance, and the polyurethane adhesive can be solvent-free, low-viscosity, good ink adaptability, good wetting performance, resistance to 121°C, 40min cooking, strong adhesion, and good hydrolysis resistance.
[0045] In some embodiments of the present invention, the branched polyester polyol is obtained by reacting an aromatic polyacid or an aliphatic polyacid with a polyol having a side branch.
[0046] In some embodiments of the present invention, the aromatic polyacid includes at least one of the aromatic dibasic acids. For example, the aromatic dibasic acid may include terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalene dicarboxylic acid, 2,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, etc.
[0047] In some embodiments of the present invention, the aliphatic polyacid includes at least one of aliphatic dibasic acids. For example, the long-chain aliphatic dibasic acid may be succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, maleic anhydride, 1,3-cyclopentanedicarboxylic acid, and the like.
[0048] In some embodiments of the present invention, the polyol with side branches includes at least one of a diol with side branches, a triol with side branches, and a tetraol with side branches.
[0049] In some embodiments of the present invention, the mass ratio of the diol with side branches, the triol with side branches and the tetraol with side branches is (90-100):(0-5):(0-5).
[0050] In some embodiments of the present invention, the side-branched polyol includes at least one of neopentyl glycol, 2-methyl-2-ethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, and 2,4-diethyl-1,5-pentanediol.
[0051] Polyurethanes made from polyester polyols synthesized from aromatic dibasic acids and diols have excellent hydrolysis resistance, heat resistance and adhesion due to the presence of a large number of benzene ring structures. Polyurethanes synthesized from polyester polyols generated by the reaction of long-chain aliphatic dibasic acids and diols have excellent toughness and softness due to the presence of long carbon chain structures. At the same time, they have more polar groups such as ester groups and urethane groups, and the cohesive strength and adhesion are guaranteed. Diols with side branches can make the synthesized polyurethane have lower viscosity and better adhesive fluidity, thereby achieving the purpose of reducing the viscosity of solvent-free adhesives. As a result, the hydrolysis resistance of branched polyester polyols can be greatly improved, the viscosity of the system can be reduced, and the polyurethane adhesive can be made solvent-free, low-viscosity, good ink adaptability, good wetting performance, resistance to 121°C, 40min boiling, strong adhesion, and good hydrolysis resistance.
[0052] In some embodiments of the present invention, the method for synthesizing the branched polyester polyol comprises: first adding polycarboxylic acid and polyol (and a trace amount of catalyst) into a reactor, performing esterification and polycondensation reactions at 140°C-220°C, controlling the top temperature of the tower, distilling off the by-product water, keeping the temperature at 200°C-230°C for 1h-2h, and then vacuuming and dealcoholizing to obtain the final branched polyester polyol.
[0053] According to an embodiment of the present invention, the bio-based polymer polyol can be obtained by reacting vegetable oil, phthalic anhydride, and polyol. Wherein, the vegetable oil includes at least one of soybean oil, palm oil, and castor oil. The polyol may include at least one of ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, methyl pentanediol, dimethyl butanediol, butyl ethyl propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, dihydroxyethoxybenzene, 1,4-cyclohexanediol, glycerol, trimethylolpropane, bisphenol A, bisphenol F, etc. The phthalic anhydride is phthalic anhydride.
[0054] Therefore, the bio-based polymer polyol synthesized by the present invention using vegetable oil, phthalic anhydride and polyol can improve the hydrolysis resistance and heat resistance of the adhesive, thereby achieving better boiling resistance, strong adhesion, hydrolysis resistance and good ink adaptability of the polyurethane adhesive.
[0055] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned polyurethane adhesive. According to an embodiment of the present invention, the method comprises:
[0056] S100: mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol according to a first ratio for reaction
[0057] In this step, isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol are mixed and reacted in a first ratio, wherein the NCO group of the isocyanate reacts chemically with the OH group of the polyol to obtain a carbamate bond (urethane), but the isocyanate is excessive, and an isocyanate-terminated polyurethane prepolymer is eventually formed to obtain component A.
[0058] Among them, the first ratio in S100 refers to the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol satisfying (50-70): (20-30): (10-20): (10-20): (5-10).
[0059] It should be noted that the container for the mixing reaction in S100 is not particularly limited, and can be, for example, a reactor or a round-bottom flask conventionally used in the art, and those skilled in the art can select one according to actual needs. Specifically, heating is required during the mixing reaction in S100, and the heating temperature is 60° C.-90° C., and the reaction time is 2 h-6 h to obtain an isocyanate-terminated polyurethane prepolymer.
[0060] S200: mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol according to a second ratio for reaction
[0061] In this step, isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol are mixed and reacted in a second ratio, wherein the NCO group of the isocyanate reacts chemically with the OH group of the polyol to obtain a carbamate bond (urethane), but the polyol is in excess and a hydroxyl-terminated polyurethane prepolymer is eventually formed to obtain component B.
[0062] The second ratio in S200 refers to the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol satisfying (1-10): (20-60): (5-20): (10-20): (1-10).
[0063] It should be noted that the container for the mixing reaction in S200 is not particularly limited, and can be, for example, a reactor or a round-bottom flask conventionally used in the art, and those skilled in the art can select one according to actual needs. Specifically, heating is required during the mixing reaction in S200, and the heating temperature is 60° C.-90° C., and the reaction time is 2 h-6 h to obtain a hydroxyl-terminated polyurethane prepolymer, which is mixed with a curing accelerator and a silane coupling agent to obtain component B.
[0064] S300: Mixing the A component with the B component
[0065] In this step, the component A is mixed with the component B, and the component A containing the terminal isocyanate prepolymer of the NCO group reacts with the component B containing the terminal hydroxyl prepolymer of the OH group to generate a carbamate (urethane) structure with a larger molecular weight and a more compact structure. The urethane can also continue to react with the isocyanate to generate allophanate. These reactions are the main reactions that occur during the production and curing of two-component polyurethane coatings. Thus, an adhesive is obtained. Specifically, the component A with an isocyanate end group and the component B with a hydroxyl end group are mixed in a weight ratio of 1-1.5:1 to react to form a macromolecule and cross-link and cure to obtain an adhesive.
[0066] Therefore, the polyurethane adhesive prepared by the method has low viscosity, good matching with ink, good wetting performance, resistance to cooking at 121°C for 40 minutes, strong adhesion and good hydrolysis resistance.
[0067] It should be noted that the characteristics and advantages described above for the polyurethane adhesive are also applicable to this method and will not be described in detail here.
[0068] In a third aspect of the present invention, a flexible bag is provided. According to an embodiment of the present invention, the flexible bag comprises the above-mentioned polyurethane adhesive or the polyurethane adhesive prepared by the above-mentioned method. As a result, the flexible bag has better high temperature cooking resistance, good ink adaptability, good wetting performance, good hydrolysis resistance, and meets the requirements of the flexible packaging industry.
[0069] It should be noted that the features and advantages described above for the polyurethane adhesive and its preparation method are also applicable to the soft bag and will not be described in detail here.
[0070] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0071] Example 1
[0072] Preparation of component A:
[0073] According to the total weight of the raw materials, 25% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1500), 10% of polyether polyol (polypropylene glycol, Mw=600), 10% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 5% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 60% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2 h, cooled to 40° C. to obtain component A;
[0074] Component A is a clear, transparent, viscous liquid at room temperature, with a viscosity of 2500 mPa·s at 25°C.
[0075] Preparation of component B:
[0076] According to the total weight of the raw materials, 30% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1000), 20% of polyether polyol (polypropylene glycol, Mw=600), 20% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 3% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 7% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2.5 h, cooled to 40° C., added 0.005% of dibutyltin dilaurate and 0.3% of KH560, and stirred evenly, and the material was discharged to obtain component B;
[0077] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 1500 mPa·s at 25°C.
[0078] Component A and component B were mixed in a mass ratio of 1.15:1, and PET (with ink) / AL / CPP were compounded on a solvent-free laminating machine. The coating and laminating temperature was 35°C, and the machine speed was 300m / min. The composite film was cured in a 60°C curing room for 48h and then taken out. The appearance was good and the performance test was carried out.
[0079] Example 2
[0080] Preparation of component A:
[0081] Calculated according to the total weight of the raw materials, 30% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1000), 10% of polyether polyol (polypropylene glycol, Mw=600), 10% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 5% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 70% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2 h, cooled to 40° C. to obtain component A;
[0082] Component A is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 2400 mPa·s at 25°C.
[0083] Preparation of component B:
[0084] According to the total weight of the raw materials, 30% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1500), 20% of polyether polyol (polypropylene glycol, Mw=600), 20% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 3% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 5% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2.5 h, cooled to 40° C., added 0.005% of dibutyltin dilaurate and 0.3% of KH570, and stirred evenly, and the material was discharged to obtain component B;
[0085] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 1300 mPa·s at 25°C.
[0086] Component A and component B were mixed in a mass ratio of 1.25:1, and PET (with ink) / AL / CPP were compounded on a solvent-free compounding machine. The coating compounding temperature was 35°C and the machine speed was 300m / min. The compounded film was cured in a 60°C curing room for 48h and then taken out. The appearance was good and the performance test was carried out.
[0087] Example 3
[0088] Preparation of component A:
[0089] According to the total weight of the raw materials, 25% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1500), 13% of polyether polyol (polypropylene glycol, Mw=600), 12% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 5% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 50% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2 h, cooled to 40° C. to obtain component A;
[0090] Component A is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 3500 mPa·s at 25°C.
[0091] Preparation of component B:
[0092] According to the total weight of the raw materials, 60% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1500), 5% of polyether polyol (polypropylene glycol, Mw=600), 12% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 10% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 10% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2.5 h, cooled to 40° C., added 0.005% of dibutyltin dilaurate and 0.3% of KH580, and stirred evenly, and the material was discharged to obtain component B;
[0093] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 1800 mPa·s at 25°C.
[0094] Component A and component B were mixed in a mass ratio of 1.35:1, and PET (with ink) / AL / CPP were compounded on a solvent-free laminating machine. The coating and laminating temperature was 35°C, and the machine speed was 300m / min. The composite film was cured in a 60°C curing room for 48h and then taken out. The appearance was good and the performance test was carried out.
[0095] Example 4
[0096] Preparation of component A:
[0097] Calculated according to the total weight of the raw materials, 30% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1000), 10% of polyether polyol (polypropylene glycol, Mw=600), 10% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 8% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 60% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2 h, cooled to 40° C. to obtain component A;
[0098] Component A is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 2700 mPa·s at 25°C.
[0099] Preparation of component B:
[0100] According to the total weight of the raw materials, 40% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1000), 5% of polyether polyol (polypropylene glycol, Mw=600), 10% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 5% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 10% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2.5 h, cooled to 40° C., added 0.005% of bismorpholinyl diethyl ether and 0.3% of KH560, and stirred evenly, and the material was discharged to obtain component B;
[0101] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 2500 mPa·s at 25°C.
[0102] Component A and component B were mixed in a mass ratio of 1.45:1, and PET (with ink) / AL / CPP were compounded on a solvent-free laminating machine. The coating and laminating temperature was 35°C, and the machine speed was 300m / min. The composite film was cured in a 60°C curing room for 48h and then taken out. The appearance was good and the performance test was carried out.
[0103] Comparative Example 1
[0104] Preparation of component A:
[0105] According to the total weight of the raw materials, 30% of polyester polyol (synthesized from adipic acid and hexanediol, Mw=3000), 15% of polyether polyol (polypropylene glycol, Mw=600), 10% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 3% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 60% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2 h, cooled to 40° C. to obtain component A;
[0106] Component A is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 6300 mPa·s at 25°C.
[0107] Preparation of component B:
[0108] According to the total weight of the raw materials, 37% of polyester polyol (synthesized from adipic acid and hexanediol, Mw=3000), 20% of polyether polyol (polypropylene glycol, Mw=600), 15% of bio-based polymer polyol (model CF-177, Qingdao Ruinuo Chemical Co., Ltd.), and 3% of polycarbonate polyol (model SYPH1000, Shanghai Shuyu Chemical Co., Ltd.) were put into a reaction device, and vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%. After cooling to 50° C., 5% of isocyanate (diphenylmethane diisocyanate) was added, the stirring speed was increased to make it fully mixed, and nitrogen protection was introduced at the same time. The temperature was raised to 80° C., the reaction was carried out for 2.5 h, and after cooling to 40° C., 0.005% of dibutyltin dilaurate and 0.3% of KH560 were added and stirred evenly, and the material was discharged to obtain component B;
[0109] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 4900 mPa·s at 25°C.
[0110] Component A and component B were mixed in a mass ratio of 1.15:1, and PET (with ink) / AL / CPP were compounded on a solvent-free laminating machine. The coating and laminating temperature was 50°C, and the machine speed was 300m / min. The composite film was cured in a 60°C curing room for 48h and then taken out. The appearance was good and the performance test was carried out.
[0111] Comparative Example 2
[0112] Preparation of component A:
[0113] Calculated according to the total weight of the raw materials, 30% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1000) and 40% of polyether polyol (polypropylene glycol, Mw=600) were put into a reaction device, vacuum dehydrated at 110°C for 1h to make the water content ≤0.05%, cooled to 50°C, 60% of isocyanate (diphenylmethane diisocyanate) was added, the stirring speed was increased to make it fully mixed, nitrogen protection was introduced at the same time, the temperature was raised to 80°C, the reaction was carried out for 2h, and the temperature was lowered to 40°C to obtain component A;
[0114] Component A is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 1900 mPa·s at 25°C.
[0115] Preparation of component B:
[0116] Calculated according to the total weight of the raw materials, 33% of branched polyester polyol (synthesized from isophthalic acid, adipic acid and neopentyl glycol, Mw=1000) and 50% of polyether polyol (polypropylene glycol, Mw=600) were put into a reaction device, vacuum dehydrated at 110° C. for 1 h to make the water content ≤0.05%, cooled to 50° C., added 7% of isocyanate (diphenylmethane diisocyanate), increased the stirring speed to make it fully mixed, and introduced nitrogen protection at the same time, heated to 80° C., reacted for 2.5 h, cooled to 40° C., added 0.005% of dibutyltin dilaurate and 0.3% of KH560, and stirred evenly, and the material was discharged to obtain component B;
[0117] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 1700 mPa·s at 25°C.
[0118] Component A and component B were mixed in a mass ratio of 1.25:1, and PET (with ink) / AL / CPP were compounded on a solvent-free compounding machine. The coating compounding temperature was 35°C and the machine speed was 300m / min. The compounded film was cured in a curing room at 60°C for 48h and then taken out for performance testing.
[0119] Comparative Example 3
[0120] Component A was prepared according to the method of Example 4.
[0121] Component A is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 2700 mPa·s at 25°C.
[0122] Component A was compounded into PET (with ink) / AL / CPP on a solvent-free compounding machine, with a coating compounding temperature of 35°C and a machine speed of 300m / min. The compounded film was cured in a 60°C curing room for 48h and then taken out for performance testing.
[0123] Comparative Example 4
[0124] Component B was prepared according to the method of Example 4.
[0125] Component B is a clear, transparent, viscous liquid at room temperature, and has a viscosity of 2500 mPa·s at 25°C.
[0126] Component B was compounded into PET (with ink) / AL / CPP on a solvent-free compounding machine, with a coating compounding temperature of 35°C and a machine speed of 300m / min. The compounded film was cured in a curing chamber at 60°C for 48h and then taken out for performance testing.
[0127] Performance Testing
[0128] The T-peel strength in the embodiment of the present invention is tested according to GB / T2791-1995 standard. The T-peel test of the flexible material to the flexible material bonding is to apply a peeling force to the unbonded end of the sample to cause the sample to peel along the glue line, and the angle between the applied force and the glue line does not need to be controlled.
[0129] The PET / AL / CPP films compounded and aged by the polyurethane adhesives of Examples 1-4 and Comparative Examples 1-4 were tested respectively, and the T-peel strengths between PET (with ink) / AL and AL / CPP were recorded as follows. The results are shown in Table 1 below:
[0130] Table 1 Performance test statistics
[0131]
[0132]
[0133] It can be seen from Table 1 that, compared with Comparative Examples 1-2, the polyurethane adhesive of Examples 1-4 is solvent-free, and after being steamed at 121°C for 40 minutes, the peel strength is still high, the bonding force is strong, the appearance performance is good, the adaptability to ink is good, the wetting performance is good, and the hydrolysis resistance is excellent. At the same time, the polyurethane adhesive of Examples 1-4 has a low viscosity at 25°C and can be coated at 30-40°C, which is more energy-saving and environmentally friendly.
[0134] Compared with Examples 1-4, the polyester polyol used in the raw materials for synthesizing components A and B of the polyurethane adhesive of Comparative Example 1 does not meet the branched polyester polyol described in the present invention. The branched polyester polyol is not obtained by reacting an aromatic polyacid with a polyol with side branches. The polyester polyol obtained by reacting adipic acid with hexanediol has strong crystallinity and high viscosity, resulting in a viscosity of component A of 6300 mPa·s at 25°C and a viscosity of component B of 4900 mPa·s at 25°C. As a result, the viscosity of the obtained polyurethane adhesive is relatively high, which is not conducive to coating at a relatively low temperature, and has poor hydrolysis resistance. In addition, the peel strength of PET (with ink) / AL is significantly reduced from 3.5 before cooking to 1.5 after cooking at 121°C for 40 minutes.
[0135] Compared with Examples 1-4, the polyether polyol used in the synthesis of components A and B of the polyurethane adhesive of Comparative Example 2 is excessive and does not meet the weight ratio of the raw materials specified in the present invention. The viscosity of component A at 25°C is 1900 mPa·s, and the viscosity of component B at 25°C is 1700 mPa·s. Although the polyurethane adhesive exhibits a lower viscosity, the hard segments in the adhesive molecules are relatively small, the polarity is poor, the mechanical properties are poor, and the bonding performance with aluminum foil is poor, so the boiling resistance cannot be achieved.
[0136] Compared with Example 4, only component A was synthesized in Comparative Example 3, and glue overflow occurred after coating. The excess NCO groups were not completely reacted, and an effective and dense glue layer could not be formed, resulting in extremely low peeling force and poor substrate adhesion. A part of the NCO groups reacted with moisture in the air to generate bubbles and make the entire sample white, with a very poor appearance. After cooking, the sample delaminated and the peeling force could not be tested.
[0137] Compared with Example 4, only component B was synthesized in Comparative Example 4, and glue overflow occurred after coating. The OH in the glue solution could not form an effective chemical reaction. It was in a liquid and uncross-linked state before and after aging, and the substrate was not bonded. It delaminated after cooking and the peeling force could not be tested.
[0138] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0139] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A polyurethane adhesive, characterized in that: The invention comprises component A and component B, wherein component A comprises an isocyanate-terminated polyurethane prepolymer obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol; and component B comprises a hydroxyl-terminated polyurethane prepolymer obtained by reacting isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol.
2. The adhesive according to claim 1, characterized in that The weight ratio of component A to component B is 1-1.5:
1.
3. The adhesive according to claim 1, characterized in that The viscosity of the component A is 2000mPa·s-5000mPa·s; And / or, the viscosity of the B component is 1000 mPa·s-3000 mPa·s.
4. The adhesive according to claim 1, characterized in that In the raw materials of component A, the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol is (50-70): (20-30): (10-20): (10-20): (5-10).
5. The adhesive according to claim 1, characterized in that In the raw materials of the B component, the weight ratio of the isocyanate, the branched polyester polyol, the polyether polyol, the bio-based polymer polyol and the polycarbonate polyol is (1-10): (20-60): (5-20): (10-20): (1-10).
6. The adhesive according to claim 1, characterized in that: The B component also includes a curing accelerator and a silane coupling agent; Optionally, the weight ratio of the hydroxyl-terminated polyurethane prepolymer, the curing accelerator and the silane coupling agent is (90-100): (0.001-0.1): (0.1-3).
7. The adhesive according to claim 1, characterized in that: The weight average molecular weight of the branched polyester polyol is 500-2000.
8. The adhesive according to claim 1 or 7, characterized in that: The branched polyester polyol is obtained by reacting an aromatic polyacid or an aliphatic polyacid with a polyol with a side branch; Preferably, the aromatic polyacid includes at least one of aromatic dibasic acids; Preferably, the aliphatic polybasic acid comprises at least one of an aliphatic dibasic acid; Preferably, the side-branched polyol comprises at least one of a side-branched diol, a side-branched triol and a side-branched tetraol; preferably, the mass ratio of the side-branched diol, the side-branched triol and the side-branched tetraol is (90-100): (0-5): (0-5); More preferably, the side-branched polyol includes at least one of neopentyl glycol, 2-methyl-2-ethyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-1,3-hexanediol, and 2,4-diethyl-1,5-pentanediol.
9. A method for preparing the adhesive according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol in a first ratio to obtain component A; (2) mixing isocyanate, branched polyester polyol, polyether polyol, bio-based polymer polyol and polycarbonate polyol in a second ratio, and adding a curing accelerator and a silane coupling agent to obtain component B; (3) Mixing the A component and the B component to obtain an adhesive.
10. A soft bag, characterized in that: The invention comprises the adhesive described in any one of claims 1 to 8 or the adhesive prepared by the method described in claim 9.