A fly ash-based dust suppressant and its application in coal dust suppression

Through the use of fly ash-based dust inhibitors, combined with the combination of organic binders and broad-spectrum antibacterial agents, the problems of bio-based dust inhibitors deterioration and viscosity reduction in summer are solved, and high viscosity and high strength are achieved. The cured layer meets the dust suppression needs of coal transportation and reduces costs.

CN118725827BActive Publication Date: 2024-11-19INNER MONGOLIA BORAN TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411214777.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing bio-based organic compound dust inhibitors have problems of deterioration and viscosity reduction during the storage and use of summer, resulting in poor storage and use stability, difficult to meet the viscosity requirements of summer spraying, and the strength of the cured layer and the anti-seismic cracking effect are not good.

Method used

Using fly ash-based dust inhibitor, the combination of fly ash silicon liquid with organic binder and broad-spectrum antibacterial agent is formed to form a cured layer with high viscosity and high strength, and combined with reinforced fibers to improve seismic and crack resistance. , and improve the viscosity characteristics of the inorganic binder through acid leaching and alkali extraction processes.

Benefits of technology

The viscosity stability during summer storage and use, the cured layer strength and earthquake resistance after spraying are achieved, which meets the high requirements for dust inhibitors during coal transportation, reduces costs and has the characteristics of circular economy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725827B_ABST
    Figure CN118725827B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of dust control in coal railway transportation, and specifically relates to a fly ash-based dust suppressant and its application in coal dust suppression. The fly ash-based dust suppressant provided by the present invention comprises: 800-6500 parts of fly ash-based inorganic binder, 5-50 parts of organic binder, 0.2-6 parts of bonding film-forming agent, 0.4-0.8 parts of broad-spectrum antibacterial agent, 10-40 parts of hygroscopic agent and 0.2-0.4 parts of reinforcing fiber; the fly ash-based inorganic binder is fly ash silicon-extracted liquid. The fly ash-based dust suppressant provided by the present invention has excellent summer storage and use stability, and can meet the actual spraying viscosity requirements (above 65mpa·s) about 10 days after stocking in summer; at the same time, the solidified layer formed has high strength and excellent anti-seismic and anti-cracking effects. The present invention realizes the preparation of dust suppressant products using fly ash as raw material, thereby controlling the generation of dust in the source coal transportation process, and has the characteristics of circular economy and green low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dust control in coal railway transportation, and particularly relates to a fly ash-based dust suppressant and application thereof in coal dust suppression. Background Art

[0002] With the widespread use of coal, the large amount of coal dust generated during its mining, transportation and utilization has become a serious environmental and health problem. For example, fine coal dust floats in the air, reducing air quality, and can also cause soil and water pollution through deposition; the dust generated during coal mining and transportation contains a large amount of fine particles, especially PM2.5, which can penetrate into the human respiratory system and pose a direct threat to the respiratory tract and lungs. Wet dust suppression is the most important and most commonly used means of coal dust prevention and control. Water or aqueous solution is used as a medium for wetting, bonding and condensing dust, and the medium is modified by physical or chemical methods, so it is often called a water-based medium. The physical modification method is a method to improve the dust-fixing capacity without adding solutes. The common method is water spray dust suppression. However, since coal dust has a hydrophobic surface, the wetting and penetration performance of medium water is poor, and the water evaporates quickly, which is easy to produce secondary dust. The chemical dust suppression method has the advantages of good dust suppression effect and long dust suppression cycle, and has gradually become the focus of future research and development of coal dust prevention and control technology. Chemical dust suppressants can be divided into wetting type, bonding type, cohesive type and composite type according to the dust suppression mechanism (wetting mechanism, bonding mechanism and coagulation film formation mechanism):

[0003] (1) Wet dust suppressants are made from some hygroscopic inorganic salts and halides as the main raw materials, and one or more surfactants (sodium hexanediyl sulfosuccinate, sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate, etc.) are added. The main mechanism of action is to reduce the surface tension of the solution, improve the wetting and penetration of the solution on dust particles, and accelerate dust sedimentation. However, this type of dust suppressant is easy to volatilize, has low adhesion, and is easy to cause secondary pollution;

[0004] (2) Adhesive dust suppressants are a type of dust suppressant that achieves dust suppression by bonding and solidifying with dust through physical or chemical adsorption. The raw materials mainly include inorganic components such as halides (such as CaCl2, MgCl2, NaCl, etc.), fly ash, water glass, and organic components such as crude oil and its derivatives, as well as bio-organic components such as cellulose, lignin, and starch. The main mechanism of action is to use the viscosity of the material itself to form a hard film of a certain strength on the surface of the dust, preventing the dust from diffusing into the air under air disturbance, thereby avoiding the dust from being entrained again (such as Figure 1 This type of dust suppressant is widely used in research and application ( Figure 2 However, it has the disadvantages of being difficult to decompose after spraying, having a strong odor, having a complicated process, and causing serious soil pollution.

[0005] (3) Coagulation-type dust suppressants absorb moisture through hygroscopic agents (such as halides, Na2SiO3, CaO and other hygroscopic inorganic salts and highly absorbent resins, etc.), capture dust in the air, increase the water content of the dust itself and eventually settle, thereby achieving the purpose of dust suppression. However, such inorganic salt solutions are usually corrosive and pose a great threat to the environment, and the preparation process of such resin-based dust suppressants is relatively complex and costly.

[0006] (4) Composite dust suppressants are formed by combining two or more dust suppressants under physical or chemical conditions. They are multifunctional dust suppressants with bonding, wetting and agglomeration properties. Composite dust suppressants have many components and a complex development process. Not only must various influencing factors be considered, but they must also be put into practical use, tested for dust suppression performance and examined for effectiveness. The research and development of composite dust suppressants is one of the key directions for future development in the field of dust suppressants in my country. However, composite dust suppressants with low preparation costs and good functions still need further research and development.

[0007] In order to effectively reduce the negative impact of coal dust on the environment and human health, domestic and foreign researchers have achieved fruitful results in the field of coal dust suppressant research and developed many dust suppressant products with different performances. These products can be roughly divided into two categories according to the main raw materials: inorganic dust suppressants and organic dust suppressants. In terms of inorganic dust suppressants, chloride salts (NaCl, MgCl2, CaCl2, etc.) and surfactants are the main raw materials. However, since the main component of this dust suppressant is chloride salt, it has the disadvantage of easily polluting the environment and damaging the equipment. In terms of organic dust suppressants, researchers mainly use organic compounds extracted from plants, bacteria and fungi as raw materials to develop dust suppressants with biodegradable properties. Natural polymer materials such as cellulose, lignin sulfonate, chitosan, guar gum, xanthan gum and corn starch are widely used in the preparation of dust suppressants. These raw materials are not only widely available, but also have good biocompatibility and environmental friendliness.

[0008] However, due to the spraying cycle and stocking reasons, dust suppressant products generally need to be stocked for 4 to 7 days in summer, so they need to be produced in advance and placed in storage tanks. The above-mentioned organic compound dust suppressant products are mainly based on bio-based binders, such as hydroxypropyl methylcellulose, guar gum, building glue powder, emulsion or xanthan gum and other organic components as thickening binders, and the dosage is mostly around 20-50%. The large-scale use of biomass causes the dust suppressant storage tank to mold and deteriorate due to high temperature in summer, producing odor, and the viscosity of the solution, the main technical indicator, drops significantly during the deterioration process.

[0009] For example: Chinese patent CN117777952A discloses a mining dust suppressant for increasing the moisturizing and bonding capacity of water bodies, as well as its preparation method and application. It uses 0.02%~0.1% guar gum, 0.02%~0.1% sodium carboxymethyl cellulose, 0.01%~0.05% sodium alginate, 0.01%~0.05% sodium chloride, and the balance is water; the guar gum and sodium carboxymethyl cellulose used in the patent are both biomass binders, and the amount used is 5~10 times higher than that of sodium alginate and humectant sodium chloride. Therefore, the dust suppressant product disclosed in the patent is at risk of high-temperature deterioration during use in summer.

[0010] In summary, the current bio-based organic compound dust suppressant products have high biomass content and poor bio-antibacterial properties, resulting in poor storage performance at high temperatures in summer. During storage and use in summer, there is a serious deterioration phenomenon and a significant decrease in standard viscosity. Summary of the invention

[0011] The object of the present invention is to provide a fly ash-based dust suppressant and application thereof in coal dust suppression. The fly ash-based dust suppressant provided by the present invention has excellent summer storage and use stability, and can meet the actual spraying viscosity requirement (above 65 MPa·s) about 10 days after summer stocking; at the same time, the formed solidified layer has high strength and excellent anti-seismic and anti-cracking effects.

[0012] In order to achieve the above object, the present invention provides the following technical solutions:

[0013] The present invention provides a fly ash-based dust suppressant, comprising the following components in parts by mass: 800-6500 parts of a fly ash-based inorganic binder, 5-50 parts of an organic binder, 0.2-6 parts of a bonding film-forming agent, 0.4-0.8 parts of a broad-spectrum antibacterial agent, 10-40 parts of a moisture absorbent and 0.2-0.4 parts of a reinforcing fiber;

[0014] The fly ash-based inorganic binder is fly ash silicon-extracted liquid, which is obtained by acid leaching fly ash to obtain acid slag, and then alkali dissolving the acid slag to obtain the acid slag.

[0015] Preferably, the modulus of the fly ash silicon-extracting liquid is 2.35-2.75; the mass content of SiO2 in the fly ash silicon-extracting liquid is 20.5-25.2%.

[0016] Preferably, the method for preparing fly ash silicon-extracting liquid comprises the following steps:

[0017] The fly ash and the acid solution are mixed for acid leaching, and the solid phase obtained after solid-liquid separation is acid slag; the mass content of SiO2 in the fly ash is ≥60%;

[0018] The acid slag and alkaline solution are mixed for alkaline dissolution to obtain the fly ash silicon extraction liquid.

[0019] Preferably, the organic binder comprises a first organic binder and a second organic binder, the first organic binder is polyacrylamide, and the second organic binder comprises one or more of sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, xanthan gum and guar gum;

[0020] The polyacrylamide is anionic, and the number average molecular weight is 16-18 million; the number average molecular weight of the sodium carboxymethyl cellulose is 200,000-250,000, and the number average molecular weight of the hydroxypropyl methyl cellulose is 200,000-300,000.

[0021] Preferably, the reinforcing fibers include one or more of carbon fibers, cellulose fibers and polypropylene fibers; and the diameter of the reinforcing fibers is in the micron level.

[0022] Preferably, the reinforcing fibers have a length of 1 to 3 mm and a diameter of 5 to 30 μm.

[0023] Preferably, the bonding film-forming agent is polyvinyl alcohol;

[0024] The broad-spectrum antibacterial agent includes one or more of sodium benzoate, kasone and s-triazine;

[0025] The desiccant includes one or more of sodium sulfate, calcium chloride and magnesium sulfate.

[0026] The present invention provides the use of the fly ash-based dust suppressant described in the above technical solution in coal dust suppression.

[0027] Preferably, the application comprises the following steps:

[0028] Mixing the fly ash-based dust suppressant described in the above technical solution with water to obtain a dust suppressant solution;

[0029] The dust suppressant solution is applied to the surface of the coal.

[0030] Preferably, the mixing comprises the following steps:

[0031] first mixing a portion of water and reinforcing fibers to obtain a first solution;

[0032] The remaining water, the organic binder, the fly ash-based inorganic binder, the adhesive film-forming agent, the moisture absorbent and the broad-spectrum antibacterial agent are mixed for the second time to obtain a second solution;

[0033] The first solution and the second solution are thirdly mixed to obtain a dust suppressant solution.

[0034] The invention provides a fly ash-based dust suppressant, comprising the following components in parts by mass: 800-6500 parts of a fly ash-based inorganic binder, 5-50 parts of an organic binder, 0.2-6 parts of a bonding film-forming agent, 0.4-0.8 parts of a broad-spectrum antibacterial agent, 10-40 parts of a hygroscopic agent and 0.2-0.4 parts of a reinforcing fiber; the fly ash-based inorganic binder is fly ash silicon-extracted liquid, and the fly ash silicon-extracted liquid is obtained by acid leaching fly ash to obtain acid slag, and then alkali dissolving the acid slag. The dust suppressant product provided by the present invention adopts an "inorganic + organic" binder compounding method, which on the one hand reduces the amount of organic binder used, reduces the cost and the amount of organic raw materials that can be corroded by fungi; on the other hand, the use of the inorganic binder (silicon-extracted liquid from fly ash) changes the liquid environment after the dust suppressant product of the present invention is configured into a dust suppressant solution, and the pH value of the dust suppressant solution system obtained by the present invention is increased. The increase in the pH value of the dust suppressant solution system will produce two beneficial parts: first: as the pH value increases, the system changes to a direction that is not conducive to the survival of fungi, thereby creating beneficial conditions for the in situ bacteriostasis of the dust suppressant solution (the in situ bacteriostasis in the present invention is relative to the dust suppressant formula in the prior art that does not change the pH value of the system, and can play an in situ bacteriostasis role. The dust suppressant product provided by the present invention also contains a broad-spectrum antibacterial agent, which is an enhanced supplement to the existing in situ antibacterial effect of the present invention, and the two do not conflict). Second: As the temperature rises, the organic binder that plays a major thickening role in the dust suppressant will break its molecular chain due to hydrolysis, and the molecular weight will decrease, which will cause the viscosity of the dust suppressant solution system to decrease. The increase in the pH value of the dust suppressant in the present invention can delay the trend of hydrolysis of the organic binder to a certain extent, thereby enhancing the stability of the viscosity of the dust suppressant solution in summer. At the same time, compared with existing products, the dust suppressant provided by the present invention forms a coal solidification layer after spraying on coal with a short time, high thickness, strong strength, and is not easy to crack. The thickness of the solidified layer formed by the existing dust suppressant products on the market after spraying basically meets the thickness requirement of 10mm in the national standard requirements, but the national standard has no requirements for the strength of the solidified layer, and only makes requirements for the wind erosion rate of the solidified layer, which is not enough in the actual application process. For example, taking the coal mining and transportation in Ordos City, Inner Mongolia Autonomous Region as an example, the coal is loaded and sprayed with dust suppressant to form a solidified layer, and then it is transported. During the coal transportation process in the Ordos area, the transport trains need to pass through a large number of tunnels. When the train passes through the tunnel at high speed, the pressure waves and shock waves generated by the tunnel effect will impact the solidified layer on the train during the propagation process, causing cracks in the solidified layer or directly shattering. In the subsequent high-speed transportation process, under the action of wind, the cracks in the solidified layer develop rapidly, causing the solidified layer to fail, and then causing the coal to escape. Or there is another situation, after the dust suppressant is sprayed, fine cracks are generated due to curing shrinkage during the film formation and drying process. The dust suppressant product provided by the present invention uses reinforcing fibers to enhance the strength of the coal solidified layer, thereby giving the solidified layer enhanced anti-seismic and anti-cracking effects.Finally, the inorganic binder in the dust suppressant product provided by the present invention is derived from fly ash, a product of coal combustion. With fly ash as the raw material, acid leaching and alkali extraction are performed to obtain fly ash silicon-extracted liquid with viscosity characteristics, so that it is used as an inorganic binder in the present invention. Therefore, the present invention realizes the preparation of dust suppressant products with fly ash as raw material, thereby controlling the generation of dust in the source coal transportation process, and has the characteristics of circular economy and green and low cost.

[0035] At the same time, the method for preparing the fly ash-based dust suppressant solution applied to coal for dust suppression is simple, has few steps, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is the dust suppression mechanism of bonding dust suppressant;

[0037] Figure 2 This is a statistical chart of dust suppressant research results from 1985 to 2021;

[0038] Figure 3 The present invention is a schematic diagram of the preparation process of a low-cost coal transportation dust suppressant prepared from fly ash in an embodiment of the present invention;

[0039] Figure 4 The static viscosity stability test results of the dust suppressant solution prepared in the embodiment of the present invention;

[0040] Figure 5 The test result of the thickness of the solidified layer formed by spraying the dust suppressant solution prepared in the embodiment of the present invention on the surface of coal;

[0041] Figure 6 The following are comparative results of static viscosity stability test of dust suppressant solutions prepared in Example 1 of the present invention and the comparative example. DETAILED DESCRIPTION

[0042] The present invention provides a fly ash-based dust suppressant, comprising the following components in parts by mass: 800-6500 parts of a fly ash-based inorganic binder, 5-50 parts of an organic binder, 0.2-6 parts of a bonding film-forming agent, 0.4-0.8 parts of a broad-spectrum antibacterial agent, 10-40 parts of a moisture absorbent and 0.2-0.4 parts of a reinforcing fiber;

[0043] The fly ash-based inorganic binder is fly ash silicon-extracted liquid, which is obtained by acid leaching fly ash to obtain acid slag, and then alkali dissolving the acid slag to obtain the acid slag.

[0044] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0045] In parts by mass, the fly ash-based dust suppressant provided by the present invention includes 800 to 6500 parts of fly ash-based inorganic binder, preferably 850 to 4800 parts, and specifically preferably 2180 parts, 880 parts, 1774 parts, 2510 parts, 3792 parts or 3632 parts.

[0046] In the present invention, the fly ash-based inorganic binder is fly ash silicon-extracted liquid, which is obtained by acid leaching fly ash to obtain acid slag, and then alkali dissolving the acid slag. The modulus of the fly ash silicon-extracted liquid is preferably 2.35-2.75; the mass content of SiO2 in the fly ash silicon-extracted liquid is preferably 20.5-25.2%.

[0047] In the present invention, the method for preparing fly ash silicon-extracting liquid preferably comprises the following steps:

[0048] The fly ash and the acid solution are mixed for acid leaching, and the solid phase obtained after solid-liquid separation is acid slag; the mass content of SiO2 in the fly ash is ≥60%;

[0049] The acid slag and alkaline solution are mixed for alkaline dissolution to obtain the fly ash silicon extraction liquid.

[0050] In the present invention, the fly ash and the acid solution are mixed for acid leaching, and the solid phase obtained after solid-liquid separation is acid slag; the mass content of SiO2 in the fly ash is ≥60%. In the present invention, the acid solution used for the acid leaching is preferably an aqueous solution of an inorganic acid, and the mass percentage of the acid solution is preferably 3-21%, and more preferably 13-17%. The acid solution is specifically preferably a hydrochloric acid solution. The liquid-solid mass ratio during the acid leaching is preferably (5-18):1, and more preferably (7-11):1. In the present invention, the temperature of the acid leaching is preferably 35-98°C, and more preferably 60-80°C; the time of the acid leaching is preferably 10-100min, and more preferably 30-60min. In the present invention, the acid leaching process can form an acid leaching filtrate from aluminum oxide, iron oxide, calcium oxide and sodium oxide soluble in the acid solution in the fly ash, and form an acid slag from silicon oxide insoluble in the acid solution, so that the silicon element and the aluminum element in the fly ash can be better separated, thereby increasing the mass content of silicon oxide in the fly ash acid slag, and thus facilitating the alkali dissolution process. The present invention has no special requirements on the specific implementation of the solid-liquid separation.

[0051] After obtaining the acid slag, the present invention mixes the acid slag and an alkaline solution for alkaline dissolution to obtain the fly ash silicon extraction liquid. In the present invention, the alkaline solution is preferably an aqueous solution of an inorganic strong alkali, and the mass percentage of the alkaline solution is preferably 5-45%, and more preferably 15-30%. In a specific embodiment of the present invention, the alkaline solution is specifically preferably a sodium hydroxide solution. The liquid-to-solid mass ratio during the alkaline dissolution is preferably (5-30):1, and more preferably (18-22):1. In the present invention, the temperature of the alkaline dissolution is preferably 50-165°C, and more preferably 80-130°C; the time of the alkaline dissolution is preferably 0.4-8h, and more preferably 3-5h. In the present invention, the alkaline dissolution enables the silicon oxide in the acid slag to fully react with the alkaline solution at the alkaline dissolution temperature, which is more conducive to the formation of fly ash silicon extraction liquid with high viscosity and good bonding effect.

[0052] The present invention uses high-silicon fly ash (mass content of SiO2 in fly ash ≥ 60%) as raw material, and does not require a high-energy ball milling process. It can directly carry out acid leaching and alkali dissolution processes to obtain fly ash silicon extraction liquid with higher SiO2 content and higher modulus. Since it is relatively difficult to extract silicon oxide from fly ash, because silicon generally exists in the form of insoluble sodium aluminosilicate phase, the present invention can increase the silicon oxide content and modulus in the fly ash silicon extraction liquid by controlling the silicon dioxide content in the fly ash raw material, the operating parameters of acid leaching and the operating parameters of alkali dissolution, thereby increasing the viscosity (bonding ability) of the fly ash silicon extraction liquid, and finally obtaining a fly ash-based inorganic binder with high solidified layer strength.

[0053] Based on the mass fraction of the fly ash-based inorganic binder, the fly ash-based dust suppressant provided by the present invention includes 5 to 50 parts of organic binder, preferably 10 to 50 parts, further preferably 20 to 50 parts, more preferably 30 to 50 parts, and specifically preferably 50 parts or 45 parts.

[0054] In the present invention, the organic binder preferably includes a first organic binder and a second organic binder, and the first organic binder is preferably polyacrylamide. The second organic binder preferably includes one or more of sodium carboxymethylcellulose, hydroxypropyl methylcellulose, xanthan gum and guar gum, and more preferably includes one or two of sodium carboxymethylcellulose, hydroxypropyl methylcellulose, xanthan gum and guar gum, and is preferably xanthan gum, or guar gum, or hydroxypropyl methylcellulose and guar gum, or sodium carboxymethylcellulose and xanthan gum. When the second organic binder is preferably any two of the above substances, the mass ratio of any two second organic binders is preferably 1:1.

[0055] In the present invention, the polyacrylamide is preferably anionic, and the number average molecular weight is preferably 16 to 18 million. The number average molecular weight of the sodium carboxymethyl cellulose is preferably 200,000 to 250,000. The number average molecular weight of the hydroxypropyl methylcellulose is preferably 200,000 to 300,000. The mass ratio of the first organic binder to the second organic binder is preferably (3 to 9): 1, more preferably (3.5 to 9): 1, and specifically preferably 9: 1, 4: 1, 8: 1 or 3.5: 1.

[0056] As one or more embodiments of the present invention, the organic binder is preferably polyacrylamide and xanthan gum. The mass ratio of the polyacrylamide to the xanthan gum is preferably 45:5, 40:10, 35:10 or 40:5.

[0057] As one or more embodiments of the present invention, the organic binder is preferably polyacrylamide, hydroxypropyl methylcellulose and guar gum. The mass ratio of the polyacrylamide, hydroxypropyl methylcellulose and guar gum is preferably 40:5:5.

[0058] As one or more embodiments of the present invention, the organic binder is preferably polyacrylamide and guar gum. The mass ratio of the polyacrylamide to the guar gum is preferably 40:5.

[0059] As one or more embodiments of the present invention, the organic binder is preferably polyacrylamide, sodium carboxymethyl cellulose and xanthan gum. The mass ratio of polyacrylamide, sodium carboxymethyl cellulose and xanthan gum is preferably 40:5:5.

[0060] Based on the mass fraction of the fly ash-based inorganic binder, the fly ash-based dust suppressant provided by the present invention includes 0.2 to 6 parts of a bonding film-forming agent, preferably 1 to 5 parts, and specifically preferably 5 parts, 2 parts, 3 parts or 4 parts.

[0061] In the present invention, the adhesive film-forming agent is preferably polyvinyl alcohol.

[0062] Based on the mass fraction of the fly ash-based inorganic binder, the fly ash-based dust suppressant provided by the present invention includes 0.4 to 0.8 parts of a broad-spectrum antibacterial agent, preferably 0.4 to 0.6 parts, and particularly preferably 0.5 parts or 0.4 parts.

[0063] In the present invention, the broad-spectrum antibacterial agent preferably includes one or more of sodium benzoate, kasone and s-triazine, and more preferably sodium benzoate, kasone or s-triazine.

[0064] Based on the mass fraction of the fly ash-based inorganic binder, the fly ash-based dust suppressant provided by the present invention includes 10 to 40 parts of a hygroscopic agent, preferably 20 to 40 parts, more preferably 30 to 40 parts, and specifically preferably 35 parts or 40 parts.

[0065] In the present invention, the moisture absorbent preferably includes one or more of sodium sulfate, calcium chloride and magnesium sulfate.

[0066] Based on the mass fraction of the fly ash-based inorganic binder, the fly ash-based dust suppressant provided by the present invention includes 0.2 to 0.4 parts of reinforcing fiber, preferably 0.25 to 0.4 parts, and particularly preferably 0.3 parts or 0.4 parts.

[0067] In the present invention, the reinforcing fibers preferably include one or more of carbon fibers, cellulose fibers and polypropylene fibers. The diameter of the reinforcing fibers is preferably in the micrometer range. The length of the reinforcing fibers is preferably 1 to 3 mm, and the diameter is preferably 5 to 30 μm, more preferably 10 to 25 μm.

[0068] The present invention provides the use of the fly ash-based dust suppressant described in the above technical solution in coal dust suppression.

[0069] In the present invention, the coal dust suppression preferably includes dust suppression during coal transportation or dust suppression during coal storage. The coal dust suppression during coal transportation is specifically preferably dust suppression during railway coal transportation.

[0070] In the present invention, the application preferably comprises the following steps:

[0071] Mixing the fly ash-based dust suppressant described in the above technical solution with water to obtain a dust suppressant solution;

[0072] The dust suppressant solution is applied to the surface of the coal.

[0073] The present invention mixes the fly ash-based dust suppressant described in the above technical solution with water to obtain a dust suppressant solution. In the present invention, the ratio of the mass of the water to the total mass of the components in the fly ash-based dust suppressant is preferably (150-200):1. The components of the fly ash-based dust suppressant include an organic binder, a bonding film-forming agent, a broad-spectrum antibacterial agent, a hygroscopic agent and reinforcing fibers.

[0074] In the present invention, the mixing preferably comprises the following steps:

[0075] first mixing a portion of water and reinforcing fibers to obtain a first solution;

[0076] The remaining water, the organic binder, the fly ash-based inorganic binder, the adhesive film-forming agent, the moisture absorbent and the broad-spectrum antibacterial agent are mixed for the second time to obtain a second solution;

[0077] The first solution and the second solution are thirdly mixed to obtain a dust suppressant solution.

[0078] The present invention first mixes part of the water and the reinforcing fiber to obtain a first solution. In the present invention, the mass ratio of the part of the water to the remaining water is preferably 1:9. The first mixing preferably includes the following steps: soaking the reinforcing fiber in part of the water, and then stirring and mixing. The soaking is preferably static soaking, the soaking temperature is preferably room temperature, and the time is preferably 20 to 30 minutes. The temperature of the stirring and mixing is preferably 25 to 30°C, the time is preferably 40 to 60 minutes, and the speed of the stirring and mixing is preferably 30 to 40 r / min. The first mixing is preferably carried out in a stirred tank.

[0079] The present invention performs a second mixing of the remaining water, the organic binder, the fly ash-based inorganic binder, the bonding film-forming agent, the hygroscopic agent and the broad-spectrum antibacterial agent to obtain a second solution. In the present invention, the second mixing preferably includes the following steps: pre-mixing the remaining water and the organic binder, and then adding the fly ash-based inorganic binder, the bonding film-forming agent, the hygroscopic agent and the broad-spectrum antibacterial agent for mixing. When the organic binder is preferably the first organic binder and the second organic binder, the pre-mixing preferably includes: pre-mixing the remaining water and the second organic binder, and then adding the first organic binder for the second pre-mixing. The temperature of the first pre-mixing is preferably 25-30°C, the time is preferably 10-20min, and the speed of the first pre-mixing is preferably 50-60r / min. The temperature of the second pre-mixing is preferably 25-30°C, the time is preferably 25-35min, and the speed of the second pre-mixing is preferably 50-60r / min. The stirring and mixing temperature is preferably 25-30° C., the time is preferably 20-30 min, and the speed of the pre-stirring and mixing is preferably 50-60 r / min.

[0080] After obtaining the first solution and the second solution, the present invention performs a third mixing of the first solution and the second solution to obtain a dust suppressant solution. In the present invention, the third mixing is preferably: injecting the first solution into the second solution for stirring and mixing. The specific implementation of the injection is preferably pumping. The temperature of the stirring and mixing is preferably room temperature, and the time is preferably 20 to 30 minutes.

[0081] After obtaining the dust suppressant solution, the present invention applies the dust suppressant solution to the surface of the coal. In the present invention, the application is preferably spraying.

[0082] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0083] In the following examples and comparative examples: the length of the reinforcing fiber is 1-3 mm, the diameter is 20-30 μm, the number average molecular weight of sodium carboxymethyl cellulose is 200,000, and the number average molecular weight of hydroxypropyl methyl cellulose is 300,000.

[0084] The preparation method of fly ash silicon extraction liquid used in the following examples and comparative examples specifically includes:

[0085] First, high silicon fly ash (SiO2 mass content of 60%) was acid leached. The acid solution used for acid leaching was hydrochloric acid solution, and the mass content of HCl in the hydrochloric acid solution was 17%; the liquid-solid mass ratio during acid leaching was 11:1. The acid leaching temperature was 60°C; the acid leaching time was 30 minutes. The solid phase product obtained after separation was acid slag.

[0086] The above acid slag is subjected to alkali dissolution to prepare fly ash silicon extraction liquid. The alkaline solution used for alkali dissolution is a sodium hydroxide aqueous solution, the mass content of NaOH in the sodium hydroxide aqueous solution is 15%, and the liquid-solid mass ratio during alkali dissolution is 18:1. The temperature of alkali dissolution is preferably 80°C; the time of alkali dissolution is 3h. After alkali dissolution, fly ash silicon extraction liquid is obtained. The modulus of fly ash silicon extraction liquid is 2.56, and the mass content of SiO2 in fly ash silicon extraction liquid is 23.5%.

[0087] In the following embodiments, Figure 3 The experimental results show the operating process of preparing low-cost coal transportation dust suppressant using fly ash as raw material.

[0088] Example 1

[0089] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by weight: 2180 parts of fly ash silicon-extracted liquid, 5 parts of xanthan gum, 45 parts of 18 million number average molecular weight polyacrylamide, 5 parts of polyvinyl alcohol, 0.5 parts of kasonite, 35 parts of sodium sulfate, and 0.3 parts of cellulose fiber.

[0090] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0091] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add cellulose fiber, soak for 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0092] In a 15-ton stirring kettle, add water according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the dust suppressant, then add hydroxypropyl methylcellulose and xanthan gum, and stir them thoroughly at a speed of 60r / min for 10-20min at 25-30℃; then add polyacrylamide, keep the stirring conditions unchanged, and stir for 25-35min; then, add fly ash silicon-extracted liquid, polyvinyl alcohol, sodium sulfate (sodium sulfate) and kasonite in turn, and continue stirring for 20-30min to obtain pre-product solution II.

[0093] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0094] Example 2

[0095] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by weight: 880 parts of fly ash silicon-extracted liquid, 10 parts of xanthan gum, 40 parts of 18 million number average molecular weight polyacrylamide, 2 parts of polyvinyl alcohol, 0.5 parts of sodium benzoate, 35 parts of sodium sulfate, and 0.3 parts of cellulose fiber.

[0096] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0097] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add cellulose fiber, soak for about 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0098] In a 15-ton stirring kettle, water is added according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, and then xanthan gum is added. At 25-30°C, the mixture is stirred at a speed of 60r / min for 10-20min. Then, polyacrylamide is added, and the stirring conditions are kept unchanged for 25-35min. Then, fly ash silicon-extracted liquid, polyvinyl alcohol, sodium sulfate and sodium benzoate are added in sequence, and stirring is continued for 20-30min to obtain pre-product solution II.

[0099] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0100] Example 3

[0101] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by mass: 1774 parts of fly ash silicon-extracted liquid, 5 parts of hydroxypropyl methylcellulose, 5 parts of guar gum, 40 parts of 18 million number average molecular weight polyacrylamide, 3 parts of polyvinyl alcohol, 0.4 parts of kason, 35 parts of calcium chloride, and 0.3 parts of carbon fiber.

[0102] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0103] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add carbon fiber, soak for about 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0104] In a 15-ton stirring kettle, add water according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the dust suppressant, then add hydroxypropyl methylcellulose and guar gum, and stir them thoroughly at a speed of 60r / min for 10-20min at 25-30℃; then add polyacrylamide, keep the stirring conditions unchanged, and stir for 25-35min; then, add fly ash silicon-extracting liquid, polyvinyl alcohol, calcium chloride and kasonite in turn, and continue stirring for 20-30min to obtain pre-product solution II.

[0105] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0106] Example 4

[0107] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by weight: 2510 parts of fly ash silicon-extracted liquid, 10 parts of xanthan gum, 35 parts of 16 million number average molecular weight polyacrylamide, 3 parts of polyvinyl alcohol, 0.4 parts of sodium benzoate, 35 parts of sodium sulfate, and 0.4 parts of cellulose fiber.

[0108] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0109] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add cellulose fiber, soak for about 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0110] In a 15-ton stirring kettle, water is added according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, and then xanthan gum is added. At 25-30°C, the mixture is stirred at a speed of 60r / min for 10-20min. Then, polyacrylamide is added, and the stirring conditions are kept unchanged for 25-35min. Then, fly ash silicon-extracted liquid, polyvinyl alcohol, sodium sulfate and sodium benzoate are added in sequence, and stirring is continued for 20-30min to obtain pre-product solution II.

[0111] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0112] Example 5

[0113] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by weight: 3792 parts of fly ash silicon-extracted liquid, 10 parts of guar gum, 40 parts of 18 million number average molecular weight polyacrylamide, 4 parts of polyvinyl alcohol, 0.5 parts of s-triazine, 40 parts of magnesium sulfate, and 0.3 parts of polypropylene fiber.

[0114] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0115] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add cellulose fiber, soak for about 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0116] In a 15-ton stirring kettle, water is added according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, and then guar gum is added. At 25-30°C, the mixture is stirred at a speed of 60r / min for 10-20min. Then, polyacrylamide is added, and the stirring conditions are kept unchanged for 25-35min. Then, fly ash silicon-extracted liquid, polyvinyl alcohol, magnesium sulfate and s-triazine are added in sequence, and stirring is continued for 20-30min to obtain pre-product solution II.

[0117] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0118] Example 6

[0119] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by weight: 3632 parts of fly ash silicon-extracted liquid, 5 parts of guar gum, 40 parts of 18 million number average molecular weight polyacrylamide, 5 parts of polyvinyl alcohol, 0.4 parts of s-triazine, 40 parts of magnesium sulfate, and 0.4 parts of polypropylene fiber.

[0120] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0121] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add polypropylene fiber, soak for about 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0122] In a 15-ton stirring kettle, water is added according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, and then guar gum is added. At 25-30°C, the mixture is stirred at a speed of 60 r / min for 10-20 min. Then, polyacrylamide is added, and the stirring conditions are kept unchanged for 25-5 min. Then, fly ash silicon-extracted liquid, polyvinyl alcohol, magnesium sulfate and s-triazine are added in sequence, and stirring is continued for 20-30 min to obtain pre-product solution II.

[0123] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0124] Example 7

[0125] The fly ash-based dust suppressant provided in this embodiment includes the following raw materials in parts by weight: 4790 parts of fly ash silicon-extracted liquid, 5 parts of sodium carboxymethyl cellulose, 5 parts of xanthan gum, 40 parts of 16 million number average molecular weight polyacrylamide, 5 parts of polyvinyl alcohol, 0.4 parts of kason, 40 parts of calcium chloride, and 0.4 parts of carbon fiber.

[0126] The fly ash-based dust suppressant solution provided in this embodiment is prepared from a fly ash-based dust suppressant and water, wherein the mass of water is 200 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the fly ash-based dust suppressant.

[0127] Weigh the raw materials and proportions mentioned above. Add water 20 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kason, sodium sulfate and cellulose fiber in the dust suppressant, add carbon fiber, soak for about 30 minutes, then start the pre-mixing kettle at 25-30°C and 40r / min for pre-dispersion stirring, the stirring time is 40-60 minutes, and obtain dispersion 1.

[0128] In a 15-ton stirring kettle, add water according to 180 times the total mass of xanthan gum, polyacrylamide, polyvinyl alcohol, kasonite, sodium sulfate and cellulose fiber in the dust suppressant, then add sodium carboxymethyl cellulose and xanthan gum, and stir them thoroughly at a speed of 60r / min for 10-20min at 25-30℃; then add polyacrylamide, keep the stirring conditions unchanged, and stir for 25-35min; then, add fly ash silicon-extracting liquid, polyvinyl alcohol, calcium chloride and kasonite in turn, and continue stirring for 20-30min to obtain pre-product solution II.

[0129] The dispersion 1 is pumped into the pre-product solution 2 by pipeline delivery, and stirring is continued for 30 minutes to obtain the final dust suppressant product solution for standby use.

[0130] The dust suppressant product prepared in the embodiment of the present invention is a Type II product. The effect parameters of the dust suppressant product solution prepared in Examples 1 to 7 sprayed on the coal sample are shown in Table 1. The data in Table 1 complete the Type II spraying task according to the spraying amount of Type I. According to the requirements of the national standard TB-T3210.1-2020, the spraying amount is 2.2L / m 2 .

[0131] Table 1 Technical effect parameters of dust suppressant solution and coal sample spraying

[0132]

[0133] The dust suppressant product solutions prepared in Examples 1 to 7 were left to stand (temperature was 32.5±2.5°C) and the viscosity stability test results were as follows: Figure 4 The actual photos of the dust suppressant product solution prepared in Examples 1 to 6 after spraying the coal sample product are shown in FIG. Figure 5 As shown in the left figure, Figure 5 In the left figure: the three samples in the first row are from left to right the actual photos of the coal samples after the dust suppressant product solutions of Examples 1 to 3 were sprayed, and the three samples in the second row are from left to right the actual photos of the coal samples after the dust suppressant product solutions of Examples 4 to 6 were sprayed. The measurement results of the thickness of the solidified layer obtained after the dust suppressant product solution in Example 5 was sprayed on the coal sample product are shown in Figure 5 As shown in the right figure.

[0134] It can be seen from the data in Table 1 that the wind erosion rate of the solidified layer obtained after the dust suppressant product solution prepared in Examples 1 to 7 of the present invention was sprayed on the coal sample was less than 0.35%.

[0135] Depend on Figure 4 It can be seen that the viscosity of the dust suppressant product solutions prepared in Examples 1 to 7 of the present invention is stable and changes little over time.

[0136] Comparative Example 1

[0137] The preparation method is basically the same as that of Example 1, except that 0.5 parts of kason is omitted from the raw materials of the dust suppressant provided in this comparative example. Figure 6 The control group 1 in this paper is used to compare the in-situ antibacterial effect of fly ash silicon-extracted liquid.

[0138] Comparative Example 2

[0139] The preparation method is basically the same as that of Example 1, except that: the raw material of the dust suppressant provided in this comparative example omits 0.5 parts of kason, and the amount of fly ash silicon extraction liquid is 1090 parts. The product of this comparative example is Figure 6 The control group 2 is used to compare the effect of the addition of fly ash silicon-extracted liquid on the stability of the dust suppressant solution.

[0140] Comparative Example 3

[0141] The preparation method is basically the same as that of Example 1, except that the raw materials of the dust suppressant provided in this comparative example omit 2180 parts of fly ash silicon extract and 0.5 parts of kason. The product of this comparative example is Figure 6 The control group 3 in this paper reflects the effect of fly ash silicon-extracted liquid on the stability of dust suppressant solution.

[0142] The relationship between the viscosity of the solution of Example 1, Comparative Examples 1 to 3 and a commercially available dust suppressant product (Inner Mongolia Bo Ran Technology Co., Ltd.) and the time of standing is as follows: Figure 6The temperature during the standing time is 32.5±2.5℃.

[0143] Depend on Figure 6 It can be seen that comparative examples 1 to 3 and the products of Bo Ran Company in the same period showed poor stability during the static experiment of the dust suppressant solution. However, it can be seen from the comparison that the viscosity of the dust suppressant solution of the current comparative formula (the comparative formula is calculated by mass, including: 18 parts of hydroxypropyl methylcellulose with a number average molecular weight of 300,000, 26 parts of high viscosity guar gum, and 56 parts of magnesium sulfate) shows a sudden drop in solution viscosity on the 4th day under room temperature; the dust suppressant solution viscosity of Bo Ran Company's products in the same period began to show a large drop in solution viscosity at 6 days under room temperature. The above reason is mainly that the composition of the current formula (Bo Ran Company's products in the same period) is mainly based on biomass binders. Under summer temperature conditions, bacteria and fungi breed, deteriorate, and break macromolecular chains, causing the solution viscosity to begin to drop sharply in a very short time. After the formula is adjusted, Example 1 has the effects of antibacterial effect and high stability. The solution viscosity can maintain viscosity for about 10 days after a short period of decline, which can give enterprises great freedom in production and stocking, and is of great significance to improving the production efficiency and competitiveness of enterprises.

[0144] Depend on Figure 6 It can be seen that compared with the comparative formula and the products of Inner Mongolia Bo Ran Technology Co., Ltd. in the same period, the viscosity of the dust suppressant solution prepared in Comparative Example 1 drops sharply at about 10 days, showing the enhanced antibacterial and high viscosity stability effects. Compared with Example 1, although the initial viscosity of Comparative Example 1 is higher and has a relatively high viscosity performance when standing for 2 to 5 days, its long-term stability is not as high as the viscosity stability of adding kason in Example 1, so it is suitable to add kason components in Example 1 to enhance the long-term stability of the dust suppressant product.

[0145] In order to compare the effect of the amount of sodium silicate solution added on the stability of the dust suppressant solution, on the basis of Control Group 1, the amount of sodium silicate solution added was reduced (reduced to 1090 parts) to form Comparative Example 2 (Control Group 2).

[0146] Depend on Figure 6 It can be seen that compared with the control group 1, the reduction in the amount of sodium silicate used increased the viscosity of the dust suppressant solution, and a more obvious viscosity decrease began to appear around 8 days, and in comparison, the percentage of viscosity decrease on the corresponding days after 8 days was higher. This shows that although the reduction in the amount of sodium silicate solution can increase the short-term use viscosity of the dust suppressant, it makes the dust suppressant solution have lower antibacterial and solution stability.

[0147] Finally, based on control group 2, the sodium silicate solution was removed from the formula to reflect the effect of the sodium silicate solution on the stability of the dust suppressant solution. Figure 6It can be seen that although the control group 3 can obtain a higher viscosity (more than 80 MPa·s) when no sodium silicate solution is added, the viscosity of its dust suppressant solution can only be stable for about 4 days. Then the viscosity of the solution shows a gradual downward trend, and the viscosity decrease trend is stronger after standing for 8 days. This is mainly due to the mold and deterioration of the biomass in the xanthan gum, and the accumulation of microorganisms has a qualitative change that affects the stability of the polyacrylamide solution, causing the viscosity of the dust suppressant solution to drop sharply. This also illustrates the necessity of using sodium silicate solution as a pH regulator, that is, an in situ antibacterial solution.

[0148] It can be seen from the above embodiments that: the present invention establishes a complete method for preparing low-cost coal transportation dust suppressants using fly ash as raw material; the present invention develops a high-stability solution for mildew and antibacterial in-situ dust suppressants; the present invention conducts a scaled-up study on the preparation process of 100-kilogram-level coal transportation dust suppressants; the present invention conducts on-site research in application scenarios such as coal yards and spraying stations to investigate and evaluate the actual application effects of new dust suppressant products on coal transportation and coal piles at stations. The fly ash-based dust suppressant provided by this method breaks through the traditional drawbacks of bio-based dust suppressants, such as high cost, easy deterioration during summer use, and poor stability, and forms a new formula and production process technology package for the production of dust suppressants using fly ash with high added value, providing scientific theory and key technical support for the cultivation of characteristic and advantageous industries.

[0149] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A fly ash-based dust suppressant, characterized in that: The invention comprises the following components in parts by weight: 1774-6500 parts of fly ash-based inorganic binder, 5-50 parts of organic binder, 0.2-6 parts of bonding film-forming agent, 0.4-0.8 parts of broad-spectrum antibacterial agent, 10-40 parts of moisture absorbent and 0.2-0.4 parts of reinforcing fiber; The fly ash-based inorganic binder is fly ash silicon-extracted liquid, and the preparation method of the fly ash silicon-extracted liquid comprises the following steps: The fly ash and the acid solution are mixed for acid leaching, and the solid phase obtained after solid-liquid separation is acid slag; the mass content of SiO2 in the fly ash is ≥60%, the acid solution used for the acid leaching is an aqueous solution of an inorganic acid, the mass percentage of the acid solution is 3-21%, the liquid-solid mass ratio during the acid leaching is (5-18):1, and the temperature of the acid leaching is 35-98°C; The acid residue and the alkaline solution are mixed for alkaline dissolution to obtain the fly ash silicon extraction liquid; the alkaline solution is an aqueous solution of an inorganic strong alkali, the mass percentage of the alkaline solution is 5-45%, the liquid-solid mass ratio during the alkaline dissolution is (5-30):1, and the temperature of the alkaline dissolution is 50-165°C; The organic binder includes a first organic binder and a second organic binder, the first organic binder is polyacrylamide, and the second organic binder includes one or more of sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, xanthan gum and guar gum.

2. The fly ash-based dust suppressant according to claim 1, characterized in that: The modulus of the fly ash silicon-extracting liquid is 2.35-2.75; the mass content of SiO2 in the fly ash silicon-extracting liquid is 20.5-25.2%.

3. The fly ash-based dust suppressant according to claim 1, characterized in that: The polyacrylamide is anionic, and the number average molecular weight is 16-18 million; the number average molecular weight of the sodium carboxymethyl cellulose is 200,000-250,000, and the number average molecular weight of the hydroxypropyl methyl cellulose is 200,000-300,000.

4. The fly ash-based dust suppressant according to claim 1, characterized in that: The reinforcing fibers include one or more of carbon fibers, cellulose fibers and polypropylene fibers; and the diameter of the reinforcing fibers is in the micron level.

5. The fly ash-based dust suppressant according to claim 1 or 4, characterized in that: The reinforcing fibers have a length of 1 to 3 mm and a diameter of 5 to 30 μm.

6. The fly ash-based dust suppressant according to claim 1, characterized in that: The bonding film-forming agent is polyvinyl alcohol; The broad-spectrum antibacterial agent includes one or more of sodium benzoate, kasone and s-triazine; The desiccant includes one or more of sodium sulfate, calcium chloride and magnesium sulfate.

7. Use of the fly ash-based dust suppressant according to any one of claims 1 to 6 in coal dust suppression.

8. The use according to claim 7, characterized in that: The application comprises the following steps: Mixing the fly ash-based dust suppressant according to any one of claims 1 to 6 with water to obtain a dust suppressant solution; The dust suppressant solution is applied to the surface of the coal.

9. The use according to claim 8, characterized in that: The mixing comprises the following steps: first mixing a portion of water and reinforcing fibers to obtain a first solution; The remaining water, the organic binder, the fly ash-based inorganic binder, the adhesive film-forming agent, the moisture absorbent and the broad-spectrum antibacterial agent are mixed for the second time to obtain a second solution; The first solution and the second solution are thirdly mixed to obtain a dust suppressant solution.

Citation Information

Cited By

  • Fly ash dust suppressant and preparation method thereof

    CN120230514A