Method for preparing high-sphericity and high-strength coated proppant by emulsion polymerization method
The petroleum fracturing proppant is processed by emulsion polymerization to form a film-coated proppant with high sphericity and high strength, which solves the problems of insufficient sphericity and strength of the proppant in the existing technology and achieves a lower crushing rate and density and has good market application prospects.
Patent Information
- Application Number
- CN202410831403.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
The sphericity and strength of existing petroleum fracturing proppant are poor, resulting in the proppant being easily broken, and the resin film layer prepared by traditional heating and curing is thin and cannot effectively improve the sphericity and apparent density of the proppant.
The emulsion polymerization method is used to treat the surface of the proppant raw material and prepare an epoxy resin-proppant mixed solution and a milky white mixed liquid to form a uniformly distributed resin coating and improve the sphericity and compression resistance of the proppant.
It significantly improves the sphericity and compression resistance of the proppant, reduces the crushing rate and density, and solves the problems of thin resin film and easy adhesion in traditional methods, and has good market application prospects.
Smart Images

Figure CN118725844A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of petroleum fracturing proppants, and in particular to a method for preparing a high-sphericity and high-strength coated proppant by an emulsion polymerization method. Background Art
[0002] Petroleum fracturing proppants are relatively regular spherical or rod-shaped materials used during the fracturing construction process to prevent the cracks formed after fracturing from closing. The fracturing proppants need to be pumped into the cracks during the process of opening the cracks. After the construction is completed, the cracks cannot close because they are filled with petroleum proppants. The cracks maintain a higher diversion channel, allowing oil and gas to flow smoothly and increase production.
[0003] Currently, most proppants used are quartz sand or ceramsite. In addition, there are walnut shells, glass microspheres and other types of proppants. Among them, except for artificial ceramsite, which has higher sphericity and strength, the sphericity and strength of other natural proppants are poor. In order to solve the shortcomings of the current proppants, such as easy breakage and sphericity, it is usually necessary to coat the surface of the proppants; please refer to Figure 1 The traditional coating method is to use a sand mixer to mix sand and organic resin, and then use a curing agent to heat and cure the resin to form a resin film on the surface of the proppant. However, the resin film layer formed by this method is relatively thin, and has limited effect on improving the sphericity of the proppant. It is similar to the morphology of the original proppant and is very easy to stick to each other after heating and curing, requiring further crushing and dispersion. In addition, the thin resin layer has little effect on reducing the apparent density of the proppant. Summary of the invention
[0004] In view of the shortcomings of the prior art described above, the purpose of the present invention is to provide a method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization, which is used to solve the problems in the prior art that the coated proppant prepared by heating and curing the sand-resin mixture has poor effect on improving the sphericity and apparent density and the finished products are very easy to stick to each other.
[0005] To achieve the above-mentioned object and other related objects, the present invention provides a method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization, comprising the following steps:
[0006] Step 1, pretreatment of proppant raw materials: select 5-15 parts of proppant raw materials with a particle size of 40-200 mesh, wash them in ethanol aqueous solution, and dry them for later use;
[0007] Step 2, treating the surface of the proppant raw material: weighing 0.05-0.3 parts of coupling agent and dissolving it in water, treating the surface of the proppant raw material for 4 hours to improve the surface interface effect between the proppant raw material particles;
[0008] Step 3, preparing an epoxy resin-proppant mixed solution: weighing 1-10 parts of epoxy resin and mixing it into the proppant raw material treated in step 2, the mixing time is 1 hour, and obtaining an epoxy resin-proppant mixed solution;
[0009] Step 4, preparing a milky white mixed solution: weighing 5-20 parts of a 10% polyvinyl alcohol solution and dropping it into the epoxy resin-proppant mixed solution, stirring to form a milky white mixed solution;
[0010] Step 5, obtaining the finished product of the coated proppant: weigh 1-3 parts of the curing agent and add it to the milky white mixed liquid. After curing for 2 hours, take out the coated proppant and place it in an oven at 120° C. to continue curing for 2 hours to obtain the finished product of the coated proppant.
[0011] In one embodiment of the present invention, the reaction environment temperature of step 2, step 3 and step 5 is 50-90°C.
[0012] In one embodiment of the present invention, the stirring speed in step 4 is 600-1000 rpm.
[0013] In one embodiment of the present invention, the total volume of the milky white mixed liquid system in step 4 is 70-90 ml.
[0014] In one embodiment of the present invention, the proppant raw material used in step 1 is quartz sand or ceramsite.
[0015] In one embodiment of the present invention, the coupling agent used in step 2 is a silane coupling agent, which is obtained by addition reaction of silyl chloroform (HSiCl3) and an unsaturated olefin with a reactive group under the catalysis of platinum chloroacid, followed by alcoholysis, including any of KH550, KH-560, KH-570, A151, A171, and A172.
[0016] In one embodiment of the present invention, the epoxy resin used in step 3 includes any type of E51, AG80, or Hyne.
[0017] In one embodiment of the present invention, the polyvinyl alcohol used in step 4 includes any one of type 0588, type 1788, type 1799, and type 2488.
[0018] In one embodiment of the present invention, the curing agent used in step 5 includes an aromatic curing agent and a modified aromatic amine curing agent, the aromatic curing agent includes any one of m-phenylenediamine, 4,4-diaminodiphenyl sulfone, and 4,4-diaminodiphenylmethane, and the modified aromatic amine curing agent includes any one of JH-0420-1 and JH-0422.
[0019] As described above, the method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization of the present invention has the following beneficial effects:
[0020] The present invention can effectively improve the surface interface effect between the proppant raw material particles by arranging the step of treating the surface of the proppant raw material, so as to achieve the purpose of improving the rheological properties and stability of the proppant raw material particles; by arranging the steps of preparing the epoxy resin-proppant mixed solution and preparing the milky white mixed solution, the proppant raw material and the epoxy resin are fully mixed by emulsion polymerization, the resin is evenly distributed on the proppant surface, and will not be affected by the surface morphology of the proppant. The sphericity of the coated proppant is extremely high, and the crushing rate after compression is extremely low, which is a revolutionary breakthrough compared with the traditional preparation method; and the coated proppant prepared by the present invention can reduce the thicker resin layer coated with ceramsite or quartz sand, and the apparent density of the obtained coated proppant is lower, which can effectively reduce the sedimentation problem caused by the excessive density of the proppant when it is injected into the formation, greatly reduce the density of the proppant, and has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Shown is a schematic diagram of the finished product of the coated proppant disclosed in the prior art.
[0022] Figure 2 Shown is a schematic diagram of a finished coated proppant obtained by the method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization disclosed in the present invention.
[0023] Figure 3 Plots showing sphericity and roundness for appearance evaluation.
[0024] Figure 4 The apparatus used to determine the bulk density Pbulk in Example 2 is shown.
[0025] Figure 5 Shown is a schematic diagram of the structure of the crushing chamber used in Real-time 2. DETAILED DESCRIPTION
[0026] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0027] See also Figure 2-4 It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings in this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the conditions under which the present invention can be implemented. Therefore, they have no substantial technical significance. Any structural modification, change in proportion or adjustment of size should still fall within the scope of the technical contents disclosed in the present invention without affecting the effects and purposes that can be achieved by the present invention.
[0028] Example 1, please refer to Figure 2 This embodiment provides a method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization, comprising the following steps:
[0029] Step 1, pretreatment of proppant raw materials: select 5-15 parts of proppant raw materials with a particle size of 40-200 mesh, clean them in ethanol aqueous solution, and dry them for use; the proppant raw materials are quartz sand or ceramsite.
[0030] Step 2, treating the surface of the proppant raw material: weigh 0.05-0.3 parts of a coupling agent and dissolve it in water, and treat the surface of the proppant raw material for 4 hours at an ambient temperature of 50-90°C to improve the surface interface effect between the proppant raw material particles; the coupling agent is a silane coupling agent, which is obtained by adding silicon chloroform (HSiCl3) and an unsaturated olefin with a reactive group under the catalysis of platinum chloroacid, and then undergoing alcoholysis, including any model of KH550, KH-560, KH-570, A151, A171, A172.
[0031] Step 3, preparing an epoxy resin-proppant mixed solution: weigh 1-10 parts of epoxy resin and mix it into the proppant raw material treated in step 2, mix at an ambient temperature of 50-90° C. for 1 hour to obtain an epoxy resin-proppant mixed solution; the epoxy resin includes any type of E51, AG80, or Hyne.
[0032] Step 4, prepare a milky white mixed solution: weigh 5-20 parts of a 10% polyvinyl alcohol solution and drop it into the epoxy resin-proppant mixed solution, stir at a speed of 600-1000rpm to form a milky white mixed solution, and keep the total volume of the milky white mixed solution system at 70-90ml. If there is a shortage, distilled water can be added; the polyvinyl alcohol includes any of the types 0588, 1788, 1799, and 2488.
[0033] Step 5, obtaining the finished product of the coated proppant: weigh 1-3 parts of the curing agent and add it to the milky white mixed liquid, and after curing for 2 hours at an ambient temperature of 50-90°C, take out the coated proppant, and place it in an oven at 120°C for further curing for 2 hours to obtain the finished product of the coated proppant; the curing agent includes an aromatic curing agent and a modified aromatic amine curing agent, the aromatic curing agent includes any one of m-phenylenediamine, 4,4-diaminodiphenyl sulfone, and 4,4-diaminodiphenylmethane, and the modified aromatic amine curing agent includes any one of JH-0420-1 and JH-0422. The curing agent is a special model provided by the manufacturer Hangmojiafa New Materials (Suzhou) Co., Ltd.
[0034] Example 2 This example provides an experimental method for visually evaluating the parameters of common proppant particle shape, sphericity and roundness. The greatest use of this measurement is in the characterization of new types of proppant deposits and new artificial proppants. See Figure 3 The most widely used method for determining roundness and sphericity is to use the Krumbien / Sloss plate. Sphericity is a measure of how close a proppant particle is to a spherical shape. Roundness is a measure of the sharpness of the corners of a proppant particle or the curvature of the particle. These parameters must be determined separately. These parameters are now determined using photographic or digital techniques, with X being roundness and Y being sphericity.
[0035] The experimental equipment should have the following capabilities:
[0036] a) A microscope with a magnification of 10 to 40 or an equivalent instrument.
[0037] b) Analytical balance with an accuracy of 0.001 g.
[0038] Experimental methods:
[0039] 1) Select the separation sample and use a sample separator to further reduce the sample mass to about 5g to 15g. If the sample separator is smaller, the sample mass can be further reduced to 1g or 2g.
[0040] 2) Spread the samples in a suitable place with a layer thickness of about one particle, and then observe the samples with a low-power magnifying glass (10x to 40x). If the proppant is light-colored, choose a dark background, and vice versa.
[0041] 3) Randomly select at least 20 proppant particles for evaluating the sphericity of the particles.
[0042] 4) Comparison Figure 3 Determine the sphericity of each selected particle using the graph shown in , and record the given sphericity number corresponding to each particle.
[0043] 5) Average the recorded sphericity numbers and report the nearest average particle sphericity with an accuracy of 0.1 graphic unit.
[0044] 6) Determine the roundness of each particle using the same particle selected by method 3). Record the given roundness number corresponding to each particle.
[0045] 7) Average the recorded roundness numbers and report the average particle roundness to the nearest 0.1 unit.
[0046] Alternative Methods for Determining Average Sphericity and Roundness: Photomicrographing of a representative proppant sample using a microscope Photomicrographing of a representative proppant sample can be used to provide the same, appropriately magnified reproduction of the average sphericity and roundness of the proppant particles. A scanning electron microscope, a reflected light microscope with a camera, a fixed camera with a bellows and wide angle lens, a digital camera, and / or other suitable photographic equipment can be successfully used to obtain photographs of known magnification. The choice of equipment is a matter of personal preference and practicality.
[0047] In addition to using selected camera equipment, numbering each selected particle imaged according to method 4) can avoid confusion and ensure that it is the same particle when determining sphericity and roundness.
[0048] Recommended Micrograph Magnifications For the specified proppant particle size ranges, the magnifications are given in the table below.
[0049]
[0050] Proppant bulk density, apparent density and absolute density test. The purpose of this test is to determine the bulk density P of the proppant. ralk , apparent density p p and the absolute density P abs .
[0051] Bulk density, apparent density and absolute density are important properties of proppants. Bulk density describes the mass of proppant that fills a unit volume, including proppant and pore volume. Bulk density can be used to determine the mass of proppant required to fill a crack or fill a tank; Apparent density is a density that does not include the pore volume between proppant. It is usually measured with a low-viscosity liquid that wets the particle surface, including the pore volume that the liquid cannot reach; Absolute density does not include the pores in the proppant and the pore volume between the proppant.
[0052] SY / T 5108-2014
[0053] 10.3 Bulk density
[0054] 10.3.1 Equipment and Materials
[0055] For equipment to determine bulk density Pbulk see Figure 4 , Figure 4 The following is described:
[0056] 1--spring, diameter p9.525mm;
[0057] 2--Rubber ball valve, diameter p30.48mm;
[0058] 3--Bracket diameter, p4.8mm, welded to the base;
[0059] 4--cylinder, inner diameter 38.1mm;
[0060] 5--3 hole positioning, diameter p139.7mm;
[0061] 10.3.1.1 Funnel stand: It consists of a 304.8mm x 304.8mm metal base and a 304.8mm high tripod. The upper part of the tripod is a horizontal circular platform with a diameter of φ203.2mm, which forms the support part of the funnel and can be replaced, adjusted or fixed in place with screws.
[0062] 10.3.1.2 There is a shut-off valve at the outlet of the funnel, which is a φ34.9mm rubber ball connected to the funnel by two spiral springs. The strength of the springs can form a strong seal. The dimensions of the funnel are as follows:
[0063] a) Top diameter (inside): 114.3mm±0.4mm.
[0064] b) Bottom diameter (inside): 12.7mm+0.4mm.
[0065] c) Height of slope section: 76.2mm±0.4mm.
[0066] d) Height of parallel section: 12.7mm+0.4mm.
[0067] 10.3.1.3 Brass cylinder: The capacity is approximately 100 cm'. The cylinder capacity shall be calibrated with water as described in 10.3.2. The cylinder shall be made of brass seamless pipe No. 17. Its dimensions are as follows:
[0068] a) Internal diameter: gp38.9mm.
[0069] b) Height: 88.9mm+0.4mm.
[0070] c) Base thickness: 12.7mm+0.4mm.
[0071] d) The bottom surface of the base should be recessed and the cylinder should be centered with a peg on the main plate, just below the outflow of the funnel.
[0072] NOTE 1: The inside diameter of brass cylinders should be within the tolerances specified for standard high-grade commercial tubing.
[0073] Note 2: Other unimportant dimensions of the equipment may be adjusted according to the user's convenience.
[0074] 10.3.2 Calibration of brass cylinder
[0075] 10.3.2.1 Cover the dry empty brass cylinder with a flat glass plate and weigh its mass and record it as
[0076] 10.3.2.2 Add water into the cylinder and slide the glass plate so that it contacts the upper edge of the cylinder and the water surface stops at the flat surface of the brass cylinder edge.
[0077] 10.3.2.3 Fix the glass plate firmly in place, wipe off the excess water, and then weigh the total mass.
[0078] 10.3.2.4 Calculate the volume of the cylinder according to formula (3)
[0079] V cly =m w / 0.9971……………………………………(3)
[0080]
[0081] Where:
[0082] --The volume of the cylinder in cubic centimeters (cm);
[0083] m w --Net mass of water, in grams (g);
[0084] 0.9971-density of water, the temperature of the test liquid shall not be lower than 18℃ nor higher than 28℃.
[0085] 10.3.3 Bulk density test method
[0086] 10.3.3.1 Weigh the mass of the dry empty cylinder in grams (g), recorded as mf.
[0087] 10.3.3.2 The temperature of the test sample is between 18℃ and 28℃. Place the proppant sample in a 150mL beaker.
[0088] 10.3.3.3 Close the outlet of the funnel, center the brass cylinder just below the outlet of the funnel, and pour the sample from the beaker into the funnel.
[0089] 10.3.3.4 Open the rubber ball valve at the bottom of the funnel to allow the proppant to flow into the brass cylinder.
[0090] 10.3.3.5 After all the proppant in the funnel has flowed out, use a ruler to push smoothly on the edge of the cylinder to make the proppant flush with the surface of the brass cylinder mouth.
[0091] 10.3.3.6 Weigh the mass of the cylinder filled with proppant in grams (g), recorded as mf + p.
[0092] 10.3.3.7 Calculate the bulk density P according to formula (4) balk .
[0093]
[0094] m p =m i-p -m i
[0095] Where:
[0096] P balk -- Bulk density, in grams per cubic centimeter (g / cm);
[0097] M p --Net mass of proppant, in grams (g). 10.4
[0099] Apparent Density
[0100] 10.4.1 Equipment and Materials
[0101] 10.4.1.1 Analytical balance, accuracy 0.01g.
[0102] 10.4.1.2 Weighing dish.
[0103] 10.4.1.3 Density bottle, calibrated, 25mL or 50mL.
[0104] 10.4.1.4 Test liquid: low-density paraffin oil, kerosene, diesel or similar oils, with a maximum viscosity of less than 5 mPa.s at the operating temperature.
[0105] 10.4.1.5 Funnel, the stem of which should be suitable for the inner diameter of the density bottle.
[0106] 10.4.2 Apparent density test method
[0107] 10.4.2.1 Calibrate the volume of the density bottle according to the method in 10.3.2.
[0108] SY / T 5108-2014
[0109] 10.4.2.2 Weigh the mass of the dry empty density bottle in grams (g) and record its mass m.
[0110] 10.4.2.3 At ambient temperature, fill the density bottle with the test liquid to the fill mark. Make sure there are no bubbles in the liquid and wipe off the liquid on the outer surface of the density bottle.
[0111] 10.4.2.4 Weigh the mass of the density bottle containing the test liquid with an accuracy of 0.01 g and record its mass m++1.
[0112] 10.4.2.5 Weigh the mass of the weighing dish, then add about 10g of proppant sample, and weigh the mass of the weighing dish and sample to the nearest 0.01g. Calculate the mass of the proppant in grams (g) and record its mass mp.
[0113] 10.4.2.6 Pour out about half of the liquid in the density bottle and transfer the weighed proppant sample from the weighing dish to the density bottle. Use a funnel that fits the neck of the density bottle.
[0114] 10.4.2.7 At ambient temperature, add enough test liquid to the fill mark on the density bottle. Rotate the bottle along its vertical axis until all bubbles in the proppant are expelled. If necessary, add test liquid again to the fill mark and wipe off the test liquid on the surface of the density bottle.
[0115] 10.4.2.8 Weigh the density bottle containing the proppant and the test liquid to an accuracy of 0.01 g and record its mass m(+).p. Calculate the density p1 of the test liquid using formula (5).
[0116]
[0117] Where:
[0118] ρ l - Density of the test liquid in grams per cubic centimeter (g / cm 3 );
[0119] m f+1 ——The mass of the density bottle filled with the test liquid at room temperature, in grams (g);
[0120] m f ——The mass of the dry empty density bottle, in grams (g);
[0121] V pyc The volume of the density bottle is in cubic centimeters (cm 3 ).
[0122] According to formula (6), the apparent density ρ is calculated p :
[0123]
[0124] Where:
[0125] ρ p - apparent density, in grams per cubic centimeter (g / cm 3 );
[0126] m P ——Mass of proppant, in grams (g);
[0127] m f+1 ——The mass of the density bottle and the test liquid at room temperature, in grams (g);
[0128] m t+1+p ——The mass of the density bottle, liquid and proppant at room temperature, in grams (g).
[0129] Submit apparent density data in grams per cubic centimeter (g / cm 3 ) and indicate the name of the liquid used in the experiment.
[0130] 11. Proppant breakage rate
[0131] 11.1 Purpose
[0132] The breakage rate test determines the amount of proppant that breaks under given stress conditions.
[0133] 11.2 Description
[0134] This test is used to determine and compare the resistance of proppants to breakage. The test is conducted on samples that have been screened so that all particles are within a specified size range. The amount of proppant material that breaks at various pressures is measured. The test results should indicate the pressure level at which a significant amount of proppant breaks, i.e., the maximum pressure that the proppant material can withstand.
[0135] 11.3 Equipment and Materials
[0136] 11.3.1 Hydraulic press, which can provide a pressure of 103MPa, should be equipped with a pressure plate that can remain parallel when pressurizing the crushing chamber. The hydraulic press should be calibrated at least once a year and after each overhaul to ensure that the accuracy of the pressure measurement is within 5%; or when pressurizing the crushing chamber, use an independent, calibrated load measuring device. The test pressure must not exceed 5% of the established value. Please refer to Figure 5 . An automatic loading press is highly recommended.
[0137] 11.3.2 Crushing chamber, see Figure 5 , or corresponding equipment. The piston is 88.9mm long, φ50.8mm in diameter, and has a Rockwell hardness of 43HRC or higher (60HRC is preferred). Regularly check the wear of the inner diameter to indicate when the piston should be replaced. When the inner diameter of the lower part of the crushing chamber exceeds 3.25% of the design size (cross-sectional area increases by -10%), the crushing chamber must be replaced.
[0138] 11.3.3 Test sieves (GB / T 6003.1-2012 series), pans and covers.
[0139] 11.3.4 Balance, used to weigh the proppant sample and the proppant retained on each sieve, with an accuracy of 0.1 g or better.
[0140] 11.3.5 Vibrating screen.
[0141] 11.3.6 Timer.
[0142] 11.3.7 Sample divider.
[0143] 11.3.8 Metal beakers or weighing dishes. Plastic, glass, or paper containers are prone to generate static electricity and should be avoided.
[0144] 11.4 Sample preparation
[0145] 11.4.1 Use a sample divider to reduce the sample to 80 g to 120 g.
[0146] 11.4.2 Select the mesh size of the top and bottom sieves that is appropriate for the proppant sample size. Prepare the sieve assembly and place the sieve assembly in the sieve shaker.
[0147] 11.4.3 Pour the sample obtained after splitting into the top sieve and cover it with the lid.
[0148] 11.4.4 Place the sieve assembly in a vibrating sieve machine and vibrate for 10 minutes.
[0149] 11.4.5 Take the group sieve out of the sieve vibrator and discard all the samples left in the top sieve and bottom plate. Only the samples in the bottom sieve are left for the crushing rate test.
[0150] 11.5 Proppant breakage rate test method
[0151] 11.5.1 Determine the exact mass m of the proppant for the breakage rate experiment as follows: p .
[0152] 11.5.1.1 Determine the uncompacted bulk density of the proppant sample used in the experiment of 10.3.
[0153] 11.5.1.2 The mass of the 850 / 425 (μm) proppant sample used in the experiment was spread on the surface of the piston at a laying concentration equivalent to 19.6 g / cm. The average non-compacted bulk density of 850 / 425 (μm) quartz sand is 1.60 g / cm. Therefore, the volume of 850 / 425 (μum) quartz sand required per square meter of the crushing chamber unit piston area is 1.22 cm' (1.96 / 1.60). In a crushing chamber with an inner diameter of φ50.8 mm, 24.7 cm is required. The required amount of proppant with different bulk density is also different. The sample mass of other proppant crushing experiments with different bulk densities is also different, and its mass m. (approximately 0.1 g) is calculated according to formula (7).
[0154] m p =24.7ρ bulk ……………………………………(7)
[0155] Where:
[0156] m p ——Sample mass, in grams (g);
[0157] ρ bulk - Bulk density, in grams per cubic centimeter (g / cm 3 ).
[0158] 11.5.2 Use a sample divider to reduce the sieved sample to the calculated mass, which shall not exceed 5 g.
[0159] 11.5.3 Weigh the sample mass m p .
[0160] 11.5.4 Pour the weighed sample into the crushing chamber. The proppant laying surface in the crushing chamber should be as flat as possible. To ensure that the surface where the proppant sample is laid is flush, the proppant should be poured smoothly into the crushing chamber. If the sieved and weighed sample is poured out of the crushing chamber, start again from step 11.5.2.
[0161] 11.5.5 Insert the piston into the crushing chamber containing the weighed proppant sample without applying any external force except gravity.
[0162] 11.5.6 Rotate the piston 180° clockwise once without applying any pressure to ensure that the proppant sample placement surface is flush.
[0163] 11.5.7 Carefully lift the crushing chamber and place it directly into the press, so that it is directly under the press support plate. Do not shake or bump the crushing chamber, as this may cause the proppant pack to sink, causing the particle pack to change shape or particles to rearrange when pressurized.
[0164] 11.5.10 Pressurize the piston of the crushing chamber at a steady rate (see 11.5.8) for 1 minute. The time to reach the rated pressure should be limited to within 5% of the time at this loading rate. If the pressure exceeds ±2.5% of the predetermined pressure, the test should be stopped and restarted with a new sample. The use of an automatic loading press is highly recommended.
[0165] 11.5.11 Maintain this pressure for 2 min.
[0166] 11.5.12 After unloading the pressure, remove the crushing chamber from the press.
[0167] 11.5.13 Carefully pour the sample into the same set of sieves used in step 11.4.2, scraping the sample from the bottom of the crushing chamber to ensure that all the sample is poured out.
[0168] 11.5.14 Place the sieve assembly into a vibrating sieve machine and vibrate for 10 minutes.
[0169] 11.5.15 Carefully weigh the mass m of the crushed material in the pan and record it with an accuracy of 0.1 g.
[0170] 11.5.16 Calculate the crushing rate m'pan of the crushed sample according to formula (9) and submit the test results according to the crushing rate of the crushed sample. For the proppant crushing test, prepare three samples according to 11.4 and conduct three tests under the same crushing stress. The average value is taken as the result.
[0171]
[0172] Where:
[0173] m′ pan ——Proppant breakage rate, expressed as a percentage;
[0174] m pan ——The mass of particles produced in the experiment, in grams (g);
[0175] m s ——The mass of the proppant, in grams (g).
[0176] This experimental method is used to test the performance of 40-70 mesh proppant. The performance data of 40-70 mesh proppant are as follows:
[0177] Quartz sand Traditional lamination Emulsion Polymerization Coating Crushing rate (52MPa) / % 39.4 9.2 1.3 <![CDATA[True density / g / cm 3 > 2.8 2.6 2.0 Bulk density / g / cm3 1.54 1.36 1.03
[0178] As can be seen from the above table, the coated proppant prepared by the emulsion polymerization method of the present invention has a lower breakage rate and bulk density, which ensures the strength of the outer coating resin. The high-performance epoxy resin and curing agent are used to make the formed resin outer layer able to withstand a pressure of 52MPa, thereby ensuring the high permeability of the coated proppant underground.
[0179] In summary, the present invention can effectively improve the surface interface effect between the proppant raw material particles by setting the step of treating the surface of the proppant raw material, so as to achieve the purpose of improving the rheological properties and stability of the proppant raw material particles; by setting the steps of preparing the epoxy resin-proppant mixed solution and preparing the milky white mixed solution, the proppant raw material and the epoxy resin are fully mixed by emulsion polymerization, and the resin is evenly distributed on the proppant surface, which will not be affected by the surface morphology of the proppant, and the sphericity of the proppant after the coating is extremely high, and the crushing rate after compression is extremely low, which is a revolutionary breakthrough compared with the traditional preparation method; and the coated proppant prepared by the present invention can reduce the thicker resin layer coated with ceramsite or quartz sand, and the apparent density of the obtained coated proppant is lower, which can effectively reduce the sedimentation problem caused by the excessive density of the proppant when the proppant is injected into the formation, greatly reducing the density of the proppant, and having a good market application prospect. Therefore, the present invention effectively overcomes the various shortcomings in the prior art and has a high industrial utilization value.
[0180] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization, characterized in that: The steps include: Step 1, pretreatment of proppant raw materials: select 5-15 parts of proppant raw materials with a particle size of 40-200 mesh, wash them in ethanol aqueous solution, and dry them for later use; Step 2, treating the surface of the proppant raw material: weighing 0.05-0.3 parts of coupling agent and dissolving it in water, treating the surface of the proppant raw material for 4 hours to improve the surface interface effect between the proppant raw material particles; Step 3, preparing an epoxy resin-proppant mixed solution: weighing 1-10 parts of epoxy resin and mixing it into the proppant raw material treated in step 2, the mixing time is 1 hour, and obtaining an epoxy resin-proppant mixed solution; Step 4, preparing a milky white mixed solution: weighing 5-20 parts of a 10% polyvinyl alcohol solution and dropping it into the epoxy resin-proppant mixed solution, stirring to form a milky white mixed solution; Step 5, obtaining the finished product of the coated proppant: weigh 1-3 parts of the curing agent and add it to the milky white mixed liquid. After curing for 2 hours, take out the coated proppant and place it in an oven at 120° C. to continue curing for 2 hours to obtain the finished product of the coated proppant.
2. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The reaction environment temperature of step 2, step 3 and step 5 is 50-90°C.
3. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The stirring speed of step 4 is 600-1000 rpm.
4. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 3, characterized in that: The total volume of the milky white mixed liquid system in step 4 is 70-90 ml.
5. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The proppant raw material used in step 1 is quartz sand or ceramsite.
6. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The coupling agent used in step 2 is a silane coupling agent, which is obtained by addition reaction of silyl chloroform (HSiCl3) and an unsaturated olefin with a reactive group under the catalysis of platinum chloroacid, followed by alcoholysis, including any of KH550, KH-560, KH-570, A151, A171, and A172.
7. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The epoxy resin used in step 3 includes any type of E51, AG80, or Hyne.
8. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The polyvinyl alcohol used in step 4 includes any type of 0588, 1788, 1799, and 2488.
9. The method for preparing a high-sphericity and high-strength coated proppant by emulsion polymerization according to claim 1, characterized in that: The curing agent used in step 5 includes an aromatic curing agent and a modified aromatic amine curing agent, wherein the aromatic curing agent includes any one of m-phenylenediamine, 4,4-diaminodiphenyl sulfone, and 4,4-diaminodiphenylmethane, and the modified aromatic amine curing agent includes any one of JH-0420-1 and JH-0422.