Special cooling liquid for high-speed shafting shaft sleeve and preparation method of special cooling liquid
By using a combination of organic alkali, water-soluble rust inhibitor and lubricant in the coolant of the high-speed shaft sleeve, the problem that the existing coolant cannot effectively prevent rust and reduce cavitation corrosion is solved, achieving low foaming, lubrication and The anti-rust effect extends the service life of the high-speed shaft sleeve.
Patent Information
- Application Number
- CN202410837633.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
The existing coolant cannot effectively prevent rust, cavitation corrosion and friction and wear in high-speed shafting bushings, and the precipitation of conventional defoaming agents increases friction damage and cannot meet the special process requirements of high-speed shafting bushings.
Using a combination of organic bases, water-soluble rust inhibitors, anti-rust auxiliaries and lubricants, including alcoholamines, carboxylic acid soaps, polyethylene glycol and other ingredients, a cooling system with low foaming, lubrication and anti-rust properties is designed. Liquid formula, through specific proportions and preparation methods, ensures that the coolant maintains excellent performance under high-pressure circulation conditions.
It can reduce friction and wear, reduce cavitation corrosion, significantly improve the anti-rust effect, extend the service life of high-speed shafting bushings, and maintain excellent thermal conductivity without using defoaming agents.
Abstract
Description
Technical Field
[0001] The invention relates to a special coolant for a high-speed shaft system sleeve and a preparation method thereof, belonging to the field of lubricating fluids. Background Art
[0002] Coolant is used in heating systems, and its main function is to control the temperature of the heating system. Through circulation, the coolant can absorb the heat generated by the heating body and bring it to the radiator for heat dissipation, thereby keeping the heating system within a suitable operating temperature range. This not only ensures the efficient operation of the heating system, but also prevents damage caused by overheating.
[0003] The coolant for high-speed shaft sleeves has high requirements for rust resistance. After the coolant circulates in the high-speed shaft sleeves, it is generally required to have an anti-rust period of half a year to one year. The coolant must have excellent thermal conductivity so that the coolant can effectively take away the heat generated by the rotation of the high-speed shaft system and maintain the high-speed shaft system at a normal operating temperature. At present, the research on coolants is mostly focused on antifreeze, environmental protection, aluminum corrosion and thermal conductivity.
[0004] After changing the anti-rust ingredients of the coolant for many times, the inventor still found that rust pits appeared quickly on the high-speed shaft sleeve. The inventor believes that in view of the special use process of the high-speed shaft sleeve coolant - high-pressure circulation (the circulation process is maintained by a high-pressure pump), there are special requirements for the coolant foam, thermal conductivity, lubricity, etc.: if there is a lot of foam, cavitation corrosion is likely to occur; if lubricity is not considered, the friction of the sleeve is likely to cause wear. These cavitation corrosion and wear locations are prone to further pitting. Therefore, resisting rust cannot simply study the anti-rust ingredients. The coolant in the prior art cannot meet the needs of the high-speed shaft sleeve under working conditions, and has not been designed and tested according to the special process of the high-speed shaft sleeve. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention provides a special coolant for a high-speed shaft sleeve, which has low foaming, lubrication and rust prevention properties, meets the requirements of the high-speed shaft sleeve in a working state, and provides a preparation method of the special coolant for a high-speed shaft sleeve.
[0006] The technical solution adopted by the present invention to solve the technical problem is: In the first aspect, the present application provides a special coolant for a high-speed shaft system sleeve, which includes 1%~2% of an organic base, 1%~2% of a water-soluble rust inhibitor, 0.5%~1% of a rust-proof auxiliary agent, 0.3%~0.5% of a lubricant, and the remainder of water by mass; the organic base is an alcohol amine, the lubricant is a carboxylic acid soap, and the rust-proof auxiliary agent is one of polyethylene glycol, block polyether, polyether polyol, and borate.
[0007] The special coolant for high-speed shaft sleeves provided in the present application has the characteristics of lubrication, low foaming and rust prevention, which is beneficial to reducing pitting corrosion caused by cavitation corrosion and friction wear, and has excellent rust prevention effect; and the low foaming effect is achieved without using a defoaming agent, which can avoid the precipitation of the defoaming agent and increase the friction on the high-speed shaft sleeve.
[0008] Furthermore, the organic base is selected from at least one of monoethanolamine and triethanolamine. The organic base is used to neutralize with some types of rust inhibitors, and after the reaction, it can provide stronger rust prevention ability and maintain the alkali reserve of the product.
[0009] Furthermore, the organic base is a combination of the monoethanolamine and the triethanolamine, and the mass ratio of the monoethanolamine to the triethanolamine is 1: 2. The organic base in this ratio is combined with a specific anti-rust auxiliary agent to achieve an excellent low-foaming effect without using a defoaming agent.
[0010] Furthermore, the lubricant is an alkyl carboxylic acid soap.
[0011] Furthermore, the water-soluble rust inhibitor is selected from at least one of tribasic acid, mixed dibasic acid, and azaphenyl ring polyaminocaproic acid. Furthermore, the water-soluble rust inhibitor is a combination of the mixed dibasic acid and the azaphenyl ring polyaminocaproic acid, and the mass ratio of the mixed dibasic acid to the azaphenyl ring polyaminocaproic acid is 1:1.
[0012] Furthermore, the anti-rust auxiliary agent is selected from at least one of monoethanolamine borate and triethanolamine borate.
[0013] Furthermore, the anti-rust auxiliary agent is a combination of the monoethanolamine borate and the triethanolamine borate, and the mass ratio of the monoethanolamine borate to the triethanolamine borate is 1:1.
[0014] Furthermore, the freezing point of the special coolant for the high-speed shaft sleeve is -2°C to 1°C, and the thermal conductivity is 576 mW / (m·K) to 591 mW / (m·K).
[0015] In the second aspect, the present application provides a method for preparing a special coolant for high-speed shaft sleeves as described in the first aspect, the steps comprising: adding the organic base to deionized water at 25°C~30°C, then adding the lubricant, stirring at 25°C~30°C until the solution is transparent, and finally adding the water-soluble rust inhibitor and rust-proof auxiliary agent, stirring at 25°C~30°C until the solution is transparent, to obtain the special coolant for high-speed shaft sleeves.
[0016] The beneficial effects of the present invention are as follows: the special coolant for high-speed shaft sleeves of the present invention not only takes into account the thermal conductivity and antifreeze properties, but also can reduce the friction and wear of high-speed shaft sleeves, and achieve a low-foaming effect without using a defoaming agent, thereby avoiding damage to the high-speed shaft sleeves caused by the use of a defoaming agent, and is also beneficial to reducing cavitation corrosion. The coolant reduces friction, wear and cavitation corrosion, and cooperates with a rust inhibitor to reduce pitting corrosion, and has an excellent anti-rust effect.
[0017] Other features and advantages of the present application will be set forth in the following description, and in part will become apparent from the description, or may be understood through implementation of the present application. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] It should be understood that, under the premise of no conflict, any and all embodiments of the present invention can be combined with the technical features in any other embodiment or multiple other embodiments to obtain another embodiment. The present invention includes such a combination to obtain another embodiment.
[0020] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.
[0021] Existing coolants are deficient in lubricity, which not only affects their performance in practical applications, but may also cause potential damage to high-speed shaft sleeves. Existing coolants often produce excessive foam, which not only affects the cooling effect of the coolant (still air has a high thermal resistance), but may also cause a series of problems, such as cavitation corrosion. Generally, the additional defoaming agent is not highly compatible with the conventional components of the coolant and is easy to precipitate, which will increase the wear of the high-speed shaft sleeve.
[0022] The following examples develop a special coolant for high-speed shaft sleeves by designing the formula of the coolant. At present, the coolant products on the market often focus on one aspect, such as antifreeze or heat conduction, or focus on inhibiting the corrosion of aluminum alloys. The present invention comprehensively considers the working conditions of the high-speed shaft sleeves, so that the coolant has excellent rust resistance, lubricity and low foaming properties, and is more suitable for cooling high-speed shaft sleeves. Combined with the working characteristics of the high-speed shaft sleeves, the additives are mainly matched to ensure that the system has good thermal conductivity and a certain degree of lubricity while selecting a suitable rust inhibitor. While meeting the requirements of heat conduction, lubrication and rust prevention, a lubrication solution with better low foaming performance is selected.
[0023] The embodiment of the present application provides a coolant for high-speed shaft sleeves with good thermal conductivity, low foaming and lubricity. The coolant for high-speed shaft sleeves includes the following components, calculated by mass percentage: 1% to 2% organic base; 1% to 2% water-soluble rust inhibitor; 0.5% to 1% rust-proof auxiliary agent; 0.3% to 0.5% lubricant; and the balance is deionized water.
[0024] The organic base is preferably selected from: monoethanolamine, triethanolamine.
[0025] The water-soluble rust inhibitor is preferably selected from the group consisting of mixed dibasic acids, tribasic acids, and azaphenyl ring polyaminocaproic acid.
[0026] The rust-proof auxiliary agent is preferably selected from: monoethanolamine borate and triethanolamine borate.
[0027] The lubricant is preferably selected from the group consisting of polyethylene glycol, block polyether, polyether polyol, and carboxylic acid soap.
[0028] The preparation method is as follows: add an organic base to deionized water at 25°C~30°C, then add a lubricant, stir at 25°C~30°C until the solution is transparent, finally add a rust inhibitor and a rust inhibitor auxiliary, stir at 25°C~30°C until the solution is transparent, and obtain a special coolant for high-speed shaft sleeves.
[0029] Specifically, the sources of raw materials used in each embodiment are as follows: Mixed dibasic acid: GM1 from Nanjing Gutian Chemical Co., Ltd.
[0030] Tribasic acid: CI-03 from Tianjin Haoruisen Chemical Trading Co., Ltd.
[0031] Azaphenyl ring polyaminocaproic acid: NEUF 985 from Notai Biotechnology (Hefei) Co., Ltd.
[0032] Monoethanolamine borate: Guangzhou Yingtianluo Trading Co., Ltd. 205M.
[0033] Triethanolamine borate: Dexu New Materials (Guangzhou) Co., Ltd. DX-621.
[0034] Monoethanolamine: MEA from Tianjin Yitaicheng Chemical Technology Co., Ltd.
[0035] Triethanolamine: TEA from Tianjin Yitaicheng Chemical Technology Co., Ltd.
[0036] Polyethylene glycol: PEG400 from Shaanxi Panlong Yihai Pharmaceutical Co., Ltd.
[0037] Block polyether: BASF (China) Co., Ltd. 1740.
[0038] Alkyl carboxylic acid soap: Dexu New Materials (Guangzhou) Co., Ltd. DX-NF109A.
[0039] The prepared embodiments and comparative examples were tested according to the following test methods: ① The test method of lubrication performance is to use a four-ball friction tester to test the lubricity of the special coolant for high-speed shaft sleeves in accordance with GB / T 12583-199.
[0040] ② Thermal conductivity test method: test with a thermal conductivity tester.
[0041] ③ Test method for the difficulty of producing foam: take 2000ml sample and put it into a circulating foam machine. Under a pressure of 2.3psi, circulate for 30 minutes and measure the foam height.
[0042] ④ Anti-rust test method: use a wet heat test chamber to test the anti-rust performance of the special coolant for high-speed shaft sleeves in accordance with GB / T 2361-1992.
[0043] The following table directly compares the dosage differences and performance differences between the embodiments and the comparative examples.
[0044] The performance test of the special coolant for high-speed shaft sleeve prepared in Example 1 was carried out, and the test results are shown in Table 1.
[0045] Table 1 Element Example 1 Deionized water 96.1 TEA 1.2 MEA 0.6 PEG400 DX-NF109A 0.3 1740 GM1 0.6 CI-03 NEUF 985 0.6 205M 0.3 DX-621 0.3 Wet heat rust prevention, d 8 PB, kg 28 Foam height, cm 3 Thermal conductivity, mW / (m·K) 590.60 Freezing point, ℃ -1 It should be noted that the values without units specified in the table are assumed to be the amount of the component used by mass, the same below.
[0046] Embodiment 2, embodiment 3, embodiment 4, and embodiment 5 provide a total of 4 kinds of special coolants for high-speed shaft sleeves, which differ from embodiment 1 in that the organic base is different, and the formula thereof is shown in Table 2. The preparation method of the special coolant for high-speed shaft sleeves in embodiment 2 to embodiment 5 is the same as that in embodiment 1. The special coolant for high-speed shaft sleeves prepared in embodiment 2 to embodiment 5 is subjected to performance tests, and the test results are shown in Table 2.
[0047] Table 2 Element Example 1 Example 2 Example 3 Example 4 Example 5 Deionized water 96.1 96.1 95.9 96.1 96.1 TEA 1.2 0.6 1.8 0.9 MEA 0.6 1.2 1.8 0.9 PEG400 DX-NF109A 0.3 0.3 0.3 0.3 0.3 1740 GM1 0.6 0.6 0.6 0.6 0.6 CI-03 NEUF 985 0.6 0.6 0.6 0.6 0.6 205M 0.3 0.3 0.3 0.3 0.3 DX-621 0.3 0.3 0.3 0.3 0.3 Wet heat rust prevention, d 8 4 5 3 5 PB, kg 28 24 24 22 24 Foam height, cm 3 4 5 7 3 Thermal conductivity, mW / (m·K) 590.60 580.60 577.34 576.36 579.43 Freezing point, ℃ -1 -2 0 -1 -1 By comparing Example 1 with Examples 2 to 5, it can be found that the addition of the organic base in Example 1 has a better anti-rust effect. The thermal conductivity is improved to a certain extent and the foam is lower when this solution is adopted.
[0048] Comparative Example 1, Comparative Example 2, Example 6, Example 7, Example 8, and Example 9 provide a total of 6 kinds of high-speed shaft sleeve special coolants, which differ from Example 1 in that the lubricant is matched differently, and the formula is shown in Table 3. The preparation method of the high-speed shaft sleeve special coolant in Comparative Example 1, Comparative Example 2, and Examples 6 to 9 is the same as that in Example 1. The performance test of the high-speed shaft sleeve special coolant prepared in Comparative Example 1, Comparative Example 2, and Examples 6 to 9 is performed, and the test results are shown in Table 3.
[0049] Table 3 Element Example 1 Comparative Example 1 Comparative Example 2 Example 6 Example 7 Example 8 Example 9 Deionized water 96.1 96.3 96.2 96.0 95.9 96.1 96.1 TEA 1.2 1.2 1.2 1.2 1.2 1.2 1.2 MEA 0.6 0.6 0.6 0.6 0.6 0.6 0.6 PEG400 0.3 DX-NF109A 0.3 0.1 0.2 0.4 0.5 1740 0.3 GM1 0.6 0.6 0.6 0.6 0.6 0.6 0.6 CI-03 NEUF 985 0.6 0.6 0.6 0.6 0.6 0.6 0.6 205M 0.3 0.3 0.3 0.3 0.3 0.3 0.3 DX-621 0.3 0.3 0.3 0.3 0.3 0.3 0.3 Wet heat rust prevention, d 8 6 7 7 7 6 6 PB, kg 28 24 26 28 28 26 22 Foam height, cm 3 4 3 4 3 5 4 Thermal conductivity, mW / (m·K) 590.60 580.60 588.34 586.56 589.43 577.34 576.36 Freezing point, ℃ -1 -2 0 -1 -1 0 -1 By comparing Example 1 with Comparative Example 1, Comparative Example 2, and Example 6 to Example 9, it can be found that the lubrication scheme of Example 1 has a better lubrication effect, and the lubrication performance does not improve significantly with the increase of the added content.
[0050] Embodiment 10, embodiment 11, embodiment 12, embodiment 13, embodiment 14, embodiment 15 provide 6 kinds of high-speed shafting sleeve special coolants, which are different from embodiment 1 in that the rust inhibitors are matched differently, and their formulas are shown in Table 4. The preparation method of the high-speed shafting sleeve special coolant in embodiment 10 to embodiment 15 is the same as that in embodiment 1. The performance test of the high-speed shafting sleeve special coolant prepared in embodiment 10 to embodiment 15 is carried out, and the test results are shown in Table 4.
[0051] Table 4 Element Example 1 Example 10 Embodiment 11 Example 12 Example 13 Embodiment 14 Embodiment 15 Deionized water 96.1 96.1 96.1 96.0 95.9 96.1 96.1 TEA 1.2 1.2 1.2 1.2 1.2 1.2 1.2 MEA 0.6 0.6 0.6 0.6 0.6 0.6 0.6 PEG400 DX-NF109A 0.3 0.3 0.3 0.3 0.3 0.3 0.3 1740 GM1 0.6 0.6 0.8 0.4 1.2 CI-03 0.6 0.6 NEUF 985 0.6 0.6 0.4 0.8 1.2 205M 0.3 0.3 0.3 0.3 0.3 0.3 0.3 DX-621 0.3 0.3 0.3 0.3 0.3 0.3 0.3 Wet heat rust prevention, d 8 5 5 6 6 6 5 PB, kg 28 26 26 24 28 26 28 Foam height, cm 3 4 5 4 4 5 4 Thermal conductivity, mW / (m·K) 590.60 585.60 583.34 584.56 584.43 579.34 587.36 Freezing point, ℃ -1 -2 0 -1 1 0 0 By comparing Example 1 with Examples 10 to 15, it can be found that the rust inhibitor compounding scheme of Example 1 has a better rust prevention effect, and the rust inhibitor compounding scheme using this dosage range combination can achieve the longest wet heat rust prevention cycle.
[0052] Embodiment 16, embodiment 17, embodiment 18, embodiment 19 provide 4 kinds of high-speed shafting sleeve special coolants, which are different from embodiment 1 in that the anti-rust auxiliary agent is matched differently, and the formula is shown in Table 5. The preparation method of the high-speed shafting sleeve special coolant in embodiment 16 to embodiment 19 is the same as that in embodiment 1. The performance test of the high-speed shafting sleeve special coolant prepared in embodiment 16 to embodiment 19 is performed, and the test results are shown in Table 5.
[0053] Table 5 Element Example 1 Example 16 Embodiment 17 Embodiment 18 Embodiment 19 Deionized water 96.1 96.1 96.1 96.0 95.9 TEA 1.2 1.2 1.2 1.2 1.2 MEA 0.6 0.6 0.6 0.6 0.6 PEG400 DX-NF109A 0.3 0.3 0.3 0.3 0.3 1740 GM1 0.6 0.6 0.8 0.4 CI-03 0.6 0.6 NEUF 985 0.6 0.6 0.4 0.8 205M 0.3 0.6 0.2 0.4 DX-621 0.3 0.6 0.4 0.2 Wet heat rust prevention, d 8 4 4 6 6 PB, kg 28 26 26 24 28 Foam height, cm 3 6 8 7 8 Thermal conductivity, mW / (m·K) 590.60 585.60 583.34 584.56 584.43 Freezing point, ℃ -1 -2 0 -1 1 By comparing Example 1 with Examples 16 to 19, it can be found that the anti-rust auxiliary agent compounding scheme of Example 1 has a better anti-rust effect, and the anti-rust auxiliary agent compounding scheme using this dosage range combination can achieve the longest wet heat anti-rust cycle and the foam height is low.
[0054] Different from the existing coolant which only focuses on antifreeze, thermal conductivity or inhibiting aluminum alloy corrosion, the embodiment of the present application fully combines the characteristics of the use process and reasonably matches the additives to ensure that the coolant has good thermal conductivity, improves the heat transfer efficiency, and also has a certain antifreeze ability, and is more suitable for the bearing steel material, providing a good and stable working environment for the high-speed shaft system. The embodiment of the present application adopts alkyl carboxylic acid soap to increase its lubricity and reduce equipment friction and wear. At the same time, the organic base and rust-proof auxiliary agent are carefully screened and reasonably formulated. In this way, the present invention can make the foam amount of the coolant meet the use requirements without adding any defoaming agent, which not only effectively reduces the risk of cavitation corrosion, but also avoids the damage that the defoaming agent may cause to the shaft sleeve and other parts. The embodiment of the present application also combines the characteristics of the use process and reasonably matches the rust inhibitor and the rust-proof auxiliary agent to ensure good rust-proof performance and increase the service life of the high-speed shaft system.
[0055] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0056] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A special coolant for high-speed shaft sleeve, characterized in that: The composition comprises 1% to 2% of an organic base, 1% to 2% of a water-soluble rust inhibitor, 0.5% to 1% of a rust-inhibiting auxiliary agent, 0.3% to 0.5% of a lubricant, and the balance of water by mass; the organic base is an alcohol amine, the lubricant is a carboxylic acid soap, and the rust-inhibiting auxiliary agent is one of polyethylene glycol, block polyether, polyether polyol, and boric acid ester.
2. The high-speed shafting sleeve special coolant according to claim 1 is characterized in that: The organic base is selected from at least one of monoethanolamine and triethanolamine.
3. The high-speed shafting sleeve special coolant according to claim 2 is characterized in that: The organic base is a combination of the monoethanolamine and the triethanolamine, and the mass ratio of the monoethanolamine to the triethanolamine is 1:
2.
4. The special coolant for high-speed shafting sleeve according to claim 1, characterized in that: The lubricant is an alkyl carboxylic acid soap.
5. The special coolant for high-speed shafting sleeve according to claim 1, characterized in that: The water-soluble rust inhibitor is selected from at least one of tribasic acid, mixed dibasic acid, and azaphenyl ring polyaminocaproic acid.
6. The special coolant for high-speed shafting sleeve according to claim 5, characterized in that: The water-soluble rust inhibitor is a combination of the mixed dibasic acid and the azaphenyl ring polyaminocaproic acid, and the mass ratio of the mixed dibasic acid to the azaphenyl ring polyaminocaproic acid is 1:
1.
7. The special coolant for high-speed shafting sleeve according to claim 1, characterized in that: The anti-rust auxiliary agent is selected from at least one of monoethanolamine borate and triethanolamine borate.
8. The special coolant for high-speed shafting sleeve according to claim 7, characterized in that: The anti-rust auxiliary agent is a combination of the monoethanolamine borate and the triethanolamine borate, and the mass ratio of the monoethanolamine borate to the triethanolamine borate is 1:
1.
9. The high-speed shafting sleeve special coolant according to claim 1, characterized in that: The freezing point is -2℃~1℃, and the thermal conductivity is 576 mW / (m·K)~591 mW / (m·K).
10. A method for preparing a special coolant for high-speed shafting sleeves according to any one of claims 1 to 9, characterized in that: The steps include: The organic base is added to deionized water at 25°C to 30°C, and then the lubricant is added, and stirred at 25°C to 30°C until the solution is transparent. Finally, the water-soluble rust inhibitor and rust-proof auxiliary agent are added, and stirred at 25°C to 30°C until the solution is transparent to obtain the special coolant for high-speed shaft sleeves.