Application of wafer surface treatment liquid
By using a wafer surface treatment solution containing silane coupling agents and organic solvents, the problem of contamination residue and collapse of high aspect ratio structures during cleaning and drying is solved, thereby improving the cleaning effect and avoiding adhesion.
Patent Information
- Application Number
- CN202310349454.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
In the manufacturing process of semiconductor chips, high aspect ratio structures are prone to problems of residual contaminants and structural collapse during cleaning and drying. In particular, the traditional IPA drying process can cause gate adhesion and collapse.
Provide a wafer surface treatment solution containing 0.1-20% silane coupling agent and organic solvent, used to clean and dry high aspect ratio wafers, and avoid adhesion and collapse by adjusting the IPA contact angle.
It effectively increases the contact angle of IPA, preventing it from adhering during the drying process, avoiding grid collapse, and improving the cleaning effect.
Smart Images

Figure BDA0004160959370000052 
Figure BDA0004160959370000061 
Figure BDA0004160959370000071
Abstract
Description
Technical Field
[0001] The invention relates to application of a wafer surface treatment liquid. Background Art
[0002] With the continuous development of the semiconductor industry, integrated circuits are gradually developing towards high integration and ultra-fine line widths. Therefore, more and more high aspect ratio structures are involved in the chip manufacturing process (in the semiconductor industry, structures with a depth / height and width ratio greater than or equal to 10 are generally defined as high aspect ratio). High aspect ratio structures not only face huge challenges during etching and deposition, but also have great problems in cleaning after etching. On the one hand, the current mainstream cleaning method is still wet cleaning based on water chemistry. For these micro-nano structures with small openings but large depths, it is difficult for liquids to enter the bottom of the grooves to achieve the purpose of cleaning; on the other hand, once the cleaning liquid enters the deep grooves, it is difficult to remove the liquid under the action of surface tension, resulting in residual contaminants, which become a potential threat to subsequent processes, and even cause device failure in severe cases. At the same time, the capillary force existing during the drying process of these high aspect ratio structures may also cause the collapse of these structures, resulting in device failure.
[0003] In the traditional IPA (isopropyl alcohol) spin-drying process, when the gate AR ratio (aspect ratio) is greater than or equal to 10, a large force will be generated between the IPA and the gate (from the surface tension of IPA), and the gate will adhere to the gate during the spin-drying process, causing the gate to collapse during the drying process. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the problem of gate collapse during the spin-drying process in the prior art, and provide an application of a wafer surface treatment liquid. After the wafer is treated with the surface treatment liquid of the present invention, the IPA contact angle is significantly increased, and no adhesion occurs between the gates during the drying process, thereby avoiding the occurrence of gate collapse.
[0005] The present invention mainly solves the above technical problems through the following technical means.
[0006] The present invention provides an application of a wafer surface treatment liquid in cleaning wafers. The raw materials of the wafer surface treatment liquid include the following components in mass fractions: 0.1-20% of a silane coupling agent and an organic solvent; the sum of the mass fractions of the components is 100%; the organic solvent makes up the balance;
[0007] The silane coupling agent is: Among them, R 1 , R 2 and R 3 Independently C1-C 10 Alkyl, amino, carboxyl, -NHC(O)NHR 4、C1-C 10 Alkoxy, hydroxyl or H; said R 1 , R 2 and R 3 Not hydroxyl or H at the same time;
[0008] R 4 is hydrogen or C1-C6 alkyl;
[0009] The organic solvent is one or more of C1-C4 alcohol solvents, propylene glycol methyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene.
[0010] In a certain embodiment of the present invention, the wafer surface treatment liquid can be used to clean the etched wafer, preferably, specifically comprising the following steps:
[0011] (1) Soak the etched wafer in an IPA cleaning solution (e.g., for 1 minute), take it out and dry it;
[0012] (2) The wafer obtained in step (1) is then immersed in the wafer surface treatment solution as described above (for example, for 1 minute), taken out and dried (for example, blown dry with nitrogen). In one embodiment of the present invention, the wafer is a high aspect ratio wafer.
[0013] In a certain embodiment of the present invention, the ratio of the depth to the width of the wafer is greater than or equal to 10, preferably 10-100, more preferably 10-50, and further preferably 10-15.
[0014] In a certain embodiment of the present invention, the content of the silane coupling agent is 5-20%; more preferably 5-15%; for example 5%, 8%, 10% or 15%.
[0015] In a certain embodiment of the present invention, the R 1 , R 2 and R 3 Independently C1-C 10 Alkoxy, -NH2 or -COOH.
[0016] In a certain embodiment of the present invention, the C1-C4 alcohol solvent is isopropyl alcohol (IPA).
[0017] In a certain embodiment of the present invention, the organic solvent is a C1-C4 alcohol solvent and / or propylene glycol methyl ether acetate.
[0018] In a certain embodiment of the present invention, the organic solvent is isopropyl alcohol, propylene glycol methyl ether acetate or a mixed solvent of isopropyl alcohol and propylene glycol methyl ether acetate.
[0019] In one embodiment of the present invention, R1 , R 2 and R 3 In the above, C1-C 10 Alkoxy is independently C1-C6 alkoxy, preferably methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy, such as methoxy.
[0020] In a certain embodiment of the present invention, the silane coupling agent is:
[0021] In a certain embodiment of the present invention, the alcohol solvent is isopropanol.
[0022] In a certain embodiment of the present invention, the organic solvent is isopropyl alcohol and / or propylene glycol methyl ether acetate.
[0023] In a certain embodiment of the present invention, when the organic solvent is a mixed solution of isopropyl alcohol and propylene glycol methyl ether acetate, the mass ratio of the isopropyl alcohol to the propylene glycol methyl ether acetate is 1:(1-2).
[0024] In a certain embodiment of the present invention, the pH value of the wafer surface treatment solution is 7-12.
[0025] In a certain embodiment of the present invention, the wafer surface treatment solution comprises: 5-15% and an organic solvent; the organic solvent making up the balance;
[0026] The organic solvent is isopropanol, propylene glycol methyl ether acetate or a mixed solvent of isopropanol and propylene glycol methyl ether acetate in a mass ratio of 1:(1-2).
[0027] In some embodiments, the wafer surface treatment solution comprises raw materials comprising any of the following components in mass fractions:
[0028] Option 1: 5% and isopropyl alcohol, the isopropyl alcohol making up the balance;
[0029] Scenario 2: 8% and isopropyl alcohol, the isopropyl alcohol making up the balance;
[0030] Option 3: 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;
[0031] Option 4: 15% and isopropyl alcohol, the isopropyl alcohol making up the balance;
[0032] Option 5: 5% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;
[0033] Option 6: 8% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;
[0034] Option 7: 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;
[0035] Option 8: 15% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;
[0036] Option 9: 5% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1 makes up the balance;
[0037] Option 10: 8% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1 makes up the balance;
[0038] Option 11: 10% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1 makes up the balance;
[0039] Option 12: 15% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1 makes up the balance;
[0040] Preferably, the raw materials of the wafer surface treatment liquid are composed of any of the above schemes.
[0041] In some embodiments, the wafer surface treatment solution is used to clean wafers with a high aspect ratio.
[0042] The term "high aspect ratio" of the present invention; in the semiconductor industry, a structure having a ratio of depth to width greater than or equal to 10 is generally defined as having a high aspect ratio.
[0043] The "room temperature" of the present invention refers to 25±5°C.
[0044] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0045] The reagents and raw materials used in the present invention are commercially available.
[0046] The positive improvement effect of the present invention is that after the surface treatment liquid of the present invention is used to clean the wafer, the IPA contact angle increases significantly, the surface changes from hydrophilic to hydrophobic, and no adhesion occurs between the gates during the drying process, thereby avoiding the occurrence of gate collapse. DETAILED DESCRIPTION
[0047] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0048] The surface treatment liquid was prepared according to the ingredients and proportions of each example in Table 1, mixed evenly, and stirred at room temperature for 1 hour (without any order of addition).
[0049] Table 1
[0050]
[0051]
[0052] Note: * indicates mass percentage; ** indicates mass ratio; “ / ” indicates non-existence.
[0053] This test was conducted using TEOS (tetraethoxysilane) and SiN (silicon nitride) wafers.
[0054] Experimental methods:
[0055] 1. Cut the wafer with aspect ratio of 10 into 30*30mm test pieces;
[0056] 2. Soak the test piece in IPA cleaning solution for 1 minute and take it out;
[0057] 3. Immerse the test pieces in the surface treatment solutions described in Table 1 for 1 min, take them out and blow dry them with nitrogen;
[0058] 4. The contact angle of the test piece was tested using a contact angle tester (AttensionThetaLite), the test solution was IPA, the surface roughness was tested at the same time, and the surface of the test piece was observed by electron microscopy; the results are shown in Table 2 below.
[0059] Table 2
[0060]
[0061]
[0062] It can be seen from the test results that after being immersed in the surface treatment liquid, the IPA contact angle increases significantly, and no adhesion occurs between the gates during the drying process, thus avoiding the occurrence of gate collapse.
Claims
1. Application of a wafer surface treatment liquid in cleaning wafers, It is characterized in that The raw materials of the wafer surface treatment liquid include the following components in mass fraction: 0.1-20% of silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The silane coupling agent is: Among them, R 1 , R 2 and R 3 Independently for C 1 -C 10 Alkyl, amino, carboxyl, -NHC(O)NHR 4 , C 1 -C 10 Alkoxy, hydroxyl or H; said R 1 , R 2 and R 3 At least one is C 1 -C 10 Alkoxy; R 4 is hydrogen or C 1 -C 6 alkyl; The organic solvent is C 1 -C 4 One or more of alcohol solvents, propylene glycol methyl ether acetate, N,N'-dimethylformamide, n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene.
2. Use of the wafer surface treatment solution as claimed in claim 1 in cleaning wafers, It is characterized in that The wafer surface treatment liquid can be used to clean the etched wafer, preferably, it comprises the following steps: (1) Soak the etched wafer in IPA cleaning solution and then take it out; (2) Then, the wafer described in step (1) is immersed in the wafer surface treatment solution described in claim 1, taken out and dried.
3. Use of the wafer surface treatment solution as claimed in claim 1 in cleaning wafers, It is characterized in that The wafer surface treatment solution meets one or both of the following conditions: (1)R 1 , R 2 and R 3 In the C 1 -C 10 The alkoxy groups are independently C 1 -C 6 Alkoxy; (2) C 1 -C 4 The alcohol solvent is isopropyl alcohol.
4. Use of the wafer surface treatment solution as claimed in claim 3 in cleaning wafers, It is characterized in that R 1 , R 2 and R 3 In the C 1 -C 10 Alkoxy is independently methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy.
5. Use of the wafer surface treatment solution as claimed in claim 1 in cleaning wafers, It is characterized in that The wafer surface treatment solution meets one or more of the following conditions: (1) The wafer is a high aspect ratio wafer; preferably, the ratio of the depth to the width of the wafer is greater than or equal to 10, more preferably 10-15; (2) R 1 , R 2 and R 3 Independently for C 1 -C 10 Alkoxy, -NH 2 or -COOH; and R 1 , R 2 and R 3 Not the same; (3) The organic solvent is C 1 -C 4 Alcohol solvents and / or propylene glycol methyl ether acetate; (4) The content of the silane coupling agent is 5-20%.
6. Use of the wafer surface treatment solution as claimed in claim 5 in cleaning wafers, It is characterized in that The wafer surface treatment solution meets one or more of the following conditions: (1) R 1 , R 2 and R 3 are independently methoxy, -NH 2 or -COOH; and R 1 , R 2 and R 3 Not the same; (2) The organic solvent is isopropyl alcohol, propylene glycol methyl ether acetate, or a mixed solvent of isopropyl alcohol and propylene glycol methyl ether acetate; (3) The content of the silane coupling agent is 5-15%, for example, 5%, 8%, 10% or 15%.
7. Use of the wafer surface treatment solution as claimed in claim 1 in cleaning wafers, It is characterized in that The wafer surface treatment solution meets one or both of the following conditions: (1) When the organic solvent is C 1 -C 4 When the mixed solvent of alcohol solvent and propylene glycol methyl ether acetate, the C 1 -C 4 The mass ratio of the alcohol solvent to the propylene glycol methyl ether acetate is 1:(1-2); (2) The silane coupling agent is:
8. Use of the wafer surface treatment solution as claimed in claim 1 in cleaning wafers, It is characterized in that It includes: 5-15% and an organic solvent; the organic solvent making up the balance; The organic solvent is isopropanol, propylene glycol methyl ether acetate or a mixed solvent of isopropanol and propylene glycol methyl ether acetate in a mass ratio of 1:(1-2).
9. Use of the wafer surface treatment solution as claimed in claims 1 to 8 in cleaning wafers, It is characterized in that The wafer surface treatment liquid, its raw materials include any of the following components in mass fractions: Option 1: 5% and isopropyl alcohol, the isopropyl alcohol making up the balance; Scenario 2: 8% and isopropyl alcohol, the isopropyl alcohol making up the balance; Option 3: 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Option 4: 15% and isopropyl alcohol, the isopropyl alcohol making up the balance; Option 5: 5% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Option 6: 8% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Option 7: 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Option 8: 15% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Option 9: 5% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1 makes up the balance; Option 10: 8% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 1:1 makes up the balance; Option 11: 10% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1 makes up the balance; Option 12: 15% and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1, and a mixed solvent of propylene glycol methyl ether acetate and isopropyl alcohol in a mass ratio of 2:1 is used to make up the balance.
10. Use of the wafer surface treatment liquid according to any one of claims 1 to 9 in cleaning wafers, It is characterized in that The wafer surface treatment liquid is composed of the silane coupling agent and the organic solvent; the type and mass fraction of the silane coupling agent and the type and mass fraction of the organic solvent are as described in any one of claims 1 to 9.