Smelting method for inhibiting P return of low-carbon steel

By adding self-made cold pressure balls and specific operating steps in the smelting process of low carbon steel, the problem of P return in the later stages of smelting and during the tapping process has been solved, the goal of low phosphorus smelting has been achieved, the dephosphorization rate has been improved and the phosphorus return has been reduced. quantity.

CN118726690APending Publication Date: 2024-10-01WUHAN IRON & STEEL GRP ECHENG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974000.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the smelting process of low carbon steel, the amount of phosphorus returned during the later stages of smelting and during the tapping process does not meet the requirements of low phosphorus smelting, making it difficult to effectively control the phosphorus return problem.

Method used

During the smelting process of low carbon steel, the temperature of the molten pool is controlled by gradually adding self-made cold pressure balls in the converter, and specific operating steps are adopted at the end and during the tapping process, such as pouring slag, adding lime, avoiding alloying and alloying Move back and control back to P.

Benefits of technology

It effectively suppresses the return of phosphorus in the late smelting and tapping process of low carbon steel, increases the dephosphorization rate, reduces the amount of phosphorus return, and achieves the goal of low-phosphorus smelting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a smelting method for inhibiting low-carbon steel from returning to P. The smelting method comprises the following steps: (1) performing normal blowing in the earlier stage and middle stage of converter smelting, detecting w [C] to be less than or equal to 0.15% at the end point of a converter, and after W [P] reaches the standard, gradually adding self-cooling press balls into the converter, and controlling the temperature of a molten pool to be less than or equal to 1610 DEG C; (2) after the end point w [C] is smaller than 0.045%, carbon catching is continued, after the molten steel w [C] enters a low-carbon steel smelting target, top oxygen blowing of an oxygen lance is switched into top argon blowing, stirring is continued for 2-3 min, and the temperature of a molten pool is controlled to range from 1580 DEG C to 1600 DEG C; (3) rarefied slag on the surface of a molten pool is poured before tapping, the slag pouring amount is 2-3 t, lime 2-3 Kg / t steel is added into the converter after slag pouring, then tapping operation is conducted, and no alloy or deoxidizing agent is added in the tapping process to avoid P return; (4) 1-2 t of steel is reserved during tapping, the slag amount in the tapping process is reduced, slag salvaging operation is conducted firstly after tapping, then alloying operation is completed, and P return during alloying is avoided; after the operations are carried out, the return P of the molten steel at the end point of the converter is 0 or 0.0002-0.001% of the further removal P is realized, so that the target of controlling the P when the converter is used for smelting the low-carbon steel is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steelmaking, in particular to a smelting method for inhibiting P recovery in low-carbon steel. Background Art

[0002] The converter has good dephosphorization ability, and the dephosphorization efficiency can generally reach more than 90%. The dephosphorization efficiency of ultra-low phosphorus steel is even higher. However, when smelting ultra-low carbon steel, although the molten steel w[P] can be controlled by effective dephosphorization means during the smelting process, the end point of smelting requires low carbon steel. Generally, the end point of low carbon steel w[C]≤0.040%. Due to process requirements, it is necessary to increase the oxygen supply intensity to force low carbon. Low carbon is often achieved by extending the end point pressure gun time and lowering the pressure gun position. After the carbon content of the molten steel W[C]≤0.040%, in the process of continuously reducing the carbon, Fe is oxidized in large quantities and there will be a rapid temperature increase process. Because dephosphorization is an exothermic reaction, when the end point of smelting low carbon steel is reduced, the temperature rises sharply, which will cause P to return. According to the steelmaking smelting data tracking, the P content changes before and after the end point of low carbon steel carbonization are collected. The amount of molten steel phosphorus return w[p] during the carbon reduction process (i.e., the rapid temperature increase process) is 0.001-0.003%. In addition to the rapid rise in temperature in the late stage of smelting, phosphorus is also easily returned during the tapping of low-carbon steel. The main mechanism is that the low-carbon operation mode must be executed to pull the low-carbon end point, resulting in a thin slag at the end of the converter. The thin slag is easily mixed with the molten steel during the tapping process. The slag mixing process is due to the addition of Si, Mn and other alloys during the alloying process of steel. The Si, Mn and other alloying processes will cause phosphorus to return, resulting in a phosphorus return amount w[p] of 0.001-0.002% during the tapping. Due to process design, low-carbon steel returns phosphorus in the late stage of smelting and during the tapping process during low-carbon smelting. The total phosphorus return amount w[p]% is 0.002-0.005%, which does not meet the requirements of low-phosphorus smelting. Therefore, new technologies are needed to effectively control the phosphorus return in the late stage of smelting and during the tapping process of low-carbon steel. Summary of the invention

[0003] The purpose of the present invention is to provide a smelting method for inhibiting the return of phosphorus in low-carbon steel due to the design of the low-carbon steel smelting process. In the low-carbon smelting, phosphorus is returned in the late stage of smelting and during the steel-making process, and the total phosphorus return amount w[p] is 0.002-0.005%, which does not meet the requirements of low-phosphorus smelting.

[0004] A smelting method for inhibiting P recovery in low-carbon steel of the present invention comprises the following steps: (1) During the early and middle stages of converter smelting, normal blowing is performed. When the converter endpoint detection w[C] is ≤0.15% and w[P] reaches the control target, self-cooling balls are gradually added to the converter to control the molten pool temperature to ≤1610°C. The specific relationship between the addition of self-cooling balls and the C content in the molten steel is as follows: When 0.08%≤w[C]≤0.15%, the weight of the self-cooling balls added to the converter is 2-3kg / t steel; When 0.045%≤w[C]<0.08%, the weight of the self-cooling balls added to the converter is 3-4kg / t steel; When w[C]<0.045%, the weight of the self-cooling balls added into the converter is 4-5.5kg / t steel; The self-cold pressed balls contain the following components in percentage by weight: FeO: 65-80%, Fe: 12-20%, Al2O3: 12-18%, and the rest are impurity elements; (2) After the end point w[C] is less than 0.045%, carbon removal is continued. When the carbon content w[C] of the molten steel reaches the target for low-carbon steel smelting, that is, when top oxygen decarburization is no longer required, the oxygen lance top-blown oxygen is switched to top-blown argon. The oxygen lance is continuously used to blow argon for 2-3 minutes to stir the molten pool, and the molten pool temperature is controlled at 1580-1600°C. (3) Before tapping, pour out the slag, and pour out the thin slag on the surface of the molten pool. The amount of slag poured is 2-3 tons. After the slag is poured, the amount of slag in the converter will decrease. At this time, add 2-3 kg / t of lime into the converter, and then perform the tapping operation. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process; (4) When tapping, 1-2t of steel is retained to reduce the amount of slag in the tapping process. After tapping, slag removal is performed first, and then alloying is performed to avoid alloying back to P. After the above operations, sampling and testing are performed after tapping at the end of the converter. The molten steel returns to P of 0, or w[P] is reduced by 0.0002-0.001%, achieving the goal of controlling P during converter smelting of low-carbon steel.

[0005] The self-cold pressed balls described in the present invention are made by mixing the self-produced converter slag and LF ladle furnace slag with components meeting the requirements with pure Fe obtained through magnetic separation and then pressing them.

[0006] The design principles of the process steps and parameters in the present invention are as follows: (1) During the early and middle stages of converter smelting, normal blowing is performed. After the predicted final carbon value of the converter w[C] is ≤0.15%, self-cooling balls are gradually added to the converter to control the molten pool temperature ≤1610℃. This is because the self-cooling balls contain FeO: 65-80%, Fe: 12-20%. After adding the self-cooling balls, ① according to the dephosphorization effect, since the dephosphorization reaction is 2[P]+5(FeO)+4(CaO)=(4CaO•P2O5)+Fe, the self-cooling balls contain high FeO, which promotes the dephosphorization reaction after adding, and can play a role in simulating the rephosphorization reaction or even further dephosphorization; ② according to the cooling effect, the self-cooling balls are added due to the addition of Pure Fe is similar to ore, and its cooling coefficient is the highest among converter coolants, making it the best coolant. The FeO in the self-cooled briquette can trigger a dephosphorization reaction (an exothermic reaction), while the melting of pure iron is an endothermic reaction. The present invention rationally proportions the content of FeO and pure Fe so that the above exothermic reaction and endothermic reaction reach a heat balance. Therefore, after adding the self-cooled briquette, it can simultaneously play a role in simulating rephosphorization and preventing the temperature of the molten steel from rising, and the pure iron can be directly recovered; ③ The FeO and Al2O3 in the briquette have a good slag-reducing effect, which can improve the fluidity of the slag and promote dephosphorization, and can also play a role in simulating rephosphorization or even further dephosphorization.

[0007] (2) After the end point w[C] is less than 0.045%, carbon extraction is continued. When the carbon content w[C] of the molten steel reaches the target for low-carbon steel smelting, that is, no top oxygen decarburization is required, the oxygen lance top oxygen blowing is switched to top argon blowing, and the argon blowing and stirring are continued with the oxygen lance for 2-3 minutes to control the molten pool temperature at 1580-1600°C. During this period (i.e., after w[C] is less than 0.045%), the oxygen content of the molten steel is between 300-550ppm. The top lance argon blowing and stirring can realize the reaction of free oxygen and residual carbon in the molten steel to complete natural decarburization and further reduce the carbon content. In addition, the switching of the oxygen lance to argon blowing can avoid the temperature rise of the molten pool caused by continuous oxygen supply; (3) Before tapping, pour out the slag, and pour out the thin slag on the surface of the molten pool. The amount of slag poured is 2-3 tons. After the slag is poured out, the amount of slag in the converter will decrease. At this time, add 2-3 kg / t of lime into the converter to thicken the slag and increase the viscosity of the slag. Then, the tapping operation is carried out. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process. (4) When tapping, leave 1-2t of steel to reduce the amount of slag in the tapping process. After tapping, perform slag removal first, and then complete alloying operation to avoid alloying back to P. After the above operations, take samples for testing after tapping at the converter end point, and the molten steel returns to P of 0, or w[P] is reduced by 0.0002-0.001%, achieving the goal of controlling P during converter smelting of low-carbon steel.

[0008] The method of the present invention is made by the inventor after a detailed theoretical analysis of the whole process of low-carbon steel converter smelting. When the carbon is reduced at the end of low-carbon steel smelting, the temperature of the smelting molten pool will rise sharply. The dephosphorization reaction is an exothermic reversible reaction. The sharp rise in the terminal temperature will cause the reaction to proceed in reverse, resulting in the return of P to the molten steel. In addition, the slag is mixed out during the steel tapping process, and the P will also be returned during the alloying of the steel tapping. By studying the mechanism of P return, the present invention intervenes in the rapid temperature rise process of pulling low carbon at the end of smelting, and adds coolant (self-cooling and pressing balls of the present invention) correspondingly during this period to avoid a sharp rise in temperature when pulling low carbon; it is difficult to simulate P return in the process of tapping low carbon steel, but through the study of the mechanism, the low carbon steel slag is too thin, and it is difficult to avoid the mixing of steel slag, but the mixing of steel slag will not directly return to P, because Si, Mn and other elements participate in the reaction during the alloying process of steel tapping, which leads to P return. In the process of tapping, adding deoxidizer to the ladle will cause the oxygen in the steel and FeO in the slag to change and decrease, and the deoxidation products SiO2, Al2O3 and other elements enter the slag, which reduces the basicity of the slag, breaks the equilibrium state of the deoxidation reaction, is conducive to the decomposition and reduction of (P2O5), and part of the phosphorus is reduced back to the molten steel to cause P return. After understanding the mechanism of P return in low carbon steel tapping, the present invention also intervenes in it, so that the timing of deoxidizer and alloying in the process of tapping low carbon steel is shifted back, and alloy is added after tapping to avoid P return in tapping.

[0009] The beneficial effects of the present invention are as follows: (1) The present invention controls the return to P through four key operations, and effectively solves the problem of easy return to P in the late stage of low-carbon steel converter smelting by simulating the timing of temperature rise and steel tapping deoxidation and alloying; (2) The present invention improves the dephosphorization rate of the converter by simulating the P return during the steel-making process of the low-carbon steel converter; (3) The process flow of the present invention is simple and clear, highly operable and easy to control. DETAILED DESCRIPTION

[0010] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. The serial numbers of the following embodiments are only for description and do not represent the advantages and disadvantages of the embodiments.

[0011] Example 1 The low carbon steel smelted in this embodiment requires that w[C] is ≤0.040% and w[P] is ≤0.009% when tapped from the converter. The specific operation is as follows: A smelting method for inhibiting the recovery of P in low-carbon steel comprises the following steps: (1) During the early and middle stages of converter smelting, normal blowing was performed. The converter endpoint detection showed that w[C] was 0.15% and w[P] was 0.009%. Self-cooling balls were gradually added to the converter to control the molten pool temperature to ≤1610°C. The specific relationship between the addition of self-cooling balls and the C content in the molten steel was as follows: When 0.08%≤w[C]≤0.15%, the weight of the self-cooling briquettes added to the converter is 2kg / t steel; When 0.045%≤w[C]<0.08%, the weight of the self-cooling briquettes added to the converter is 3kg / t steel; When w[C]<0.045%, the weight of the self-cooling balls added into the converter is 4kg / t steel; The self-cold pressed balls contain the following components in percentage by weight: FeO: 70%, Fe: 12%, Al2O3: 17%, and the rest are impurity elements; after the addition of the self-cold pressed balls, the molten pool temperature is 1608°C, and the detected steel liquid w[P] is 0.0088% at this time; (2) After the end point w[C] is less than 0.045%, carbon removal is continued. When the carbon content w[C] of the molten steel is 0.040%, that is, no top oxygen decarburization is required, the oxygen lance top blowing oxygen is switched to top blowing argon, and argon is continuously blown with the oxygen lance for 2 minutes to stir. The molten pool temperature is controlled at 1600°C. At this time, sampling is taken for testing. The molten steel w[C] is 0.040% and w[P] is 0.0088%; (3) Before tapping, the slag is first poured out to remove the thin slag on the surface of the molten pool. The amount of slag poured is 3 tons. After the slag is poured out, the amount of slag in the converter decreases accordingly. At this time, 2 kg / t of lime is added to the converter, and then the tapping operation is carried out. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process; (4) 1 t of steel is retained during steel tapping to reduce the amount of slag discharged during the steel tapping process. Slag removal is performed first after steel tapping, and alloying is then performed after slag removal to avoid alloying back to P. After the above operations, samples are taken for testing after steel tapping at the converter end point. The w[C] and w[P] of the molten steel are 0.039% and 0.0088%, respectively, achieving the goal of controlling P during converter smelting of low-carbon steel.

[0012] Example 2 The low carbon steel smelted in this embodiment requires that w[C] is ≤0.040% and w[P] is ≤0.008% when tapped from the converter. The specific operation is as follows: A smelting method for inhibiting the recovery of P in low-carbon steel comprises the following steps: (1) During the early and middle stages of converter smelting, normal blowing was performed. The converter endpoint detection w[C] was 0.15% and w[P] was 0.008%. Self-cooling balls were gradually added to the converter to control the molten pool temperature to ≤1610°C. The specific relationship between the addition of self-cooling balls and the C content in the molten steel is as follows: When 0.08%≤w[C]≤0.15%, the weight of the self-cooling balls added to the converter is 2.5kg / t steel; When 0.045%≤w[C]<0.08%, the weight of the self-cooling balls added into the converter is 3.5kg / t steel; When w[C]<0.045%, the weight of the self-cooling balls added into the converter is 4.5kg / t steel; The self-cold pressed balls contain the following components in percentage by weight: FeO: 65%, Fe: 20%, Al2O3: 14%, and the rest are impurity elements; after the addition of the self-cold pressed balls, the molten pool temperature is 1605°C, and the detected steel liquid w[P] is 0.008% at this time; (2) After the end point w[C] is less than 0.045%, carbon removal is continued. When the steel liquid w[C] is 0.040%, that is, no top oxygen decarburization is required, the oxygen lance top blowing oxygen is switched to top blowing argon, and the oxygen lance is used to continue blowing argon for 2.5 minutes. The molten pool temperature is controlled at 1595°C. At this time, sampling is taken for testing. The steel liquid w[C] is 0.039% and w[P] is 0.008%; (3) Before tapping, the slag is first poured out to remove the thin slag on the surface of the molten pool. The amount of slag poured is 2.5 tons. After the slag is poured out, the amount of slag in the converter decreases. At this time, 2.5 kg / t of lime is added to the converter, and then the tapping operation is carried out. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process; (4) After steel tapping, 1.5t of steel is retained to reduce the amount of slag in the steel tapping process. Slag removal is performed first after steel tapping, and alloying is performed after slag removal to avoid alloying back to P. After the above operations, samples are taken for testing after steel tapping at the converter end point. The w[C] and w[P] of the molten steel are 0.038% and 0.008%, respectively, achieving the goal of controlling P during converter smelting of low-carbon steel.

[0013] Example 3 The low carbon steel smelted in this embodiment requires that w[C] is ≤0.040% and w[P] is ≤0.007% when tapping from the converter. The specific operation is as follows: A smelting method for inhibiting the recovery of P in low-carbon steel comprises the following steps: (1) During the early and middle stages of converter smelting, normal blowing was performed. The converter endpoint detection showed that w[C] was 0.15% and w[P] was 0.007%. Self-cooling balls were gradually added to the converter to control the molten pool temperature to ≤1610°C. The specific relationship between the addition of self-cooling balls and the C content in the molten steel was as follows: When 0.08%≤w[C]≤0.15%, the weight of the self-cooled briquettes added to the converter is 3kg / t steel; When 0.045%≤w[C]<0.08%, the weight of the self-cooling balls added into the converter is 4kg / t steel; When w[C]<0.045%, the weight of the self-cooling balls added into the converter is 5kg / t steel; The self-cold pressed balls contain the following components in percentage by weight: FeO: 75%, Fe: 12%, Al2O3: 12%, and the rest are impurity elements; after the addition of the self-cold pressed balls, the molten pool temperature is 1603°C, and the detected steel liquid w[P] is 0.0065% at this time; (2) After the end point w[C] is less than 0.045%, carbon removal is continued. When the carbon content w[C] of the molten steel reaches the target for low-carbon steel smelting, that is, no top-blowing oxygen decarburization is required, the oxygen lance top-blowing oxygen is switched to top-blowing argon, and the argon is continuously blown with the oxygen lance for stirring for 3 minutes. The molten pool temperature is controlled at 1585°C. At this time, sampling is taken for testing. The molten steel w[C] is 0.038% and w[P] is 0.0065%; (3) Before tapping, pour out the slag, and pour out the thin slag on the surface of the molten pool. The amount of slag poured is 2 tons. After the slag is poured, the amount of slag in the converter decreases. At this time, add 3 kg / t of lime into the converter, and then perform the tapping operation. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process; (4) After steel tapping, 2 tons of steel is retained to reduce the amount of slag in the steel tapping process. After steel tapping, the slag removal operation is carried out first, and then the alloying operation is completed to avoid alloying back to P. After the above operations, sampling and testing are carried out after steel tapping at the converter end. The molten steel w[C] is 0.037%, and w[P] is 0.0065%, achieving the goal of controlling P during converter smelting of low carbon steel.

[0014] Example 4 The low carbon steel smelted in this embodiment requires that w[C] is ≤0.040% and w[P] is ≤0.009% when tapped from the converter. The specific operation is as follows: A smelting method for inhibiting the recovery of P in low-carbon steel comprises the following steps: (1) During the early and middle stages of converter smelting, normal blowing was performed. The converter endpoint detection showed that w[C] was 0.15% and w[P] was 0.009%. Self-cooling balls were gradually added to the converter to control the molten pool temperature to ≤1610°C. The specific relationship between the addition of self-cooling balls and the C content in the molten steel was as follows: When 0.08%≤w[C]≤0.15%, the weight of the self-cooled briquettes added to the converter is 3kg / t steel; When 0.045%≤w[C]<0.08%, the weight of the self-cooling balls added into the converter is 4kg / t steel; When w[C]<0.045%, the weight of the self-cooling balls added into the converter is 5.5kg / t steel; The self-cold pressed balls contain the following components in percentage by weight: FeO: 70%, Fe: 15%, Al2O3: 14%, and the rest are impurity elements; after the addition of the self-cold pressed balls, the molten pool temperature is 1602°C, and the detected steel liquid w[P] is 0.008% at this time; (2) After the end point w[C] is less than 0.045%, carbon removal is continued. When the carbon content w[C] of the molten steel reaches the target for low-carbon steel smelting, that is, no top-blowing oxygen decarburization is required, the oxygen lance top-blowing oxygen is switched to top-blowing argon, and argon is continuously blown with the oxygen lance for stirring for 2 minutes. The molten pool temperature is controlled at 1580°C. At this time, sampling is taken for testing. The molten steel w[C] is 0.037% and w[P] is 0.008%; (3) Before tapping, the slag is first poured out to remove the thin slag on the surface of the molten pool. The amount of slag poured is 3 tons. After the slag is poured out, the amount of slag in the converter decreases accordingly. At this time, 3 kg / t of lime is added to the converter, and then the tapping operation is carried out. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process; (4) After steel tapping, 1.5t of steel is retained to reduce the amount of slag in the steel tapping process. Slag removal is performed first after steel tapping, and alloying is performed after slag removal to avoid alloying back to P. After the above operations, samples are taken for testing after steel tapping at the converter end point. The w[C] and w[P] of the molten steel are 0.036% and 0.008%, respectively, achieving the goal of controlling P during converter smelting of low-carbon steel.

[0015] In the conventional mode of producing low carbon steel, the phosphorus recovery w[p] in the low carbon drawing process is about 0.001-0.003%; the phosphorus recovery w[p] in the steel tapping process is about 0.001-0.002%, and the total phosphorus recovery w[p] is about 0.002-0.005%. However, by adopting the method of the present invention to effectively control the temperature of the terminal low carbon drawing process and not adding alloy and deoxidizer in the steel tapping process (i.e., alloying is shifted backward), the total phosphorus recovery w[p] is 0, and even further dephosphorization is performed. By adopting the method of the present invention for low carbon steel smelting, the phosphorus recovery can be significantly improved. See the table below for specific comparison:

[0016] From the data in the above table, it can be seen that compared with the conventional mode, the phosphorus content of low-carbon steel smelted in the present invention is 0, or further dephosphorized by 0.0002-0.001%, which indicates that the method of the present invention can effectively inhibit the phosphorus content of low-carbon steel smelting process.

[0017] The above embodiments are only specific examples for explaining the present invention and do not limit the present invention in any form. Any non-substantial changes made by anyone based on the above contents and forms without departing from the protection scope of the claims of the present invention shall be deemed to fall within the protection scope of the claims of the present invention. The present invention is not limited to the above specific implementation examples.

Claims

1. A smelting method for inhibiting the return of P to low carbon steel, characterized in that The steps include: (1) During the early and middle stages of converter smelting, normal blowing is performed. When the converter endpoint detection w[C] is ≤0.15% and w[P] reaches the control target, self-cooling balls are gradually added to the converter to control the molten pool temperature to ≤1610°C. The specific relationship between the addition of self-cooling balls and the C content in the molten steel is as follows: When 0.08%≤w[C]≤0.15%, the weight of the self-cooling balls added to the converter is 2-3kg / t steel; When 0.045%≤w[C]<0.08%, the weight of the self-cooling balls added to the converter is 3-4kg / t steel; When w[C]<0.045%, the weight of the self-cooling balls added into the converter is 4-5.5kg / t steel; The self-cold pressed balls contain the following components in percentage by weight: FeO: 65-80%, Fe: 12-20%, Al2O3: 12-18%, and the rest are impurity elements; (2) After the end point w[C] is less than 0.045%, carbon removal is continued. When the carbon content w[C] of the molten steel reaches the target for low-carbon steel smelting, that is, when top oxygen decarburization is no longer required, the oxygen lance top-blown oxygen is switched to top-blown argon. The oxygen lance is continuously used to blow argon for 2-3 minutes to stir the molten pool, and the molten pool temperature is controlled at 1580-1600°C. (3) Before tapping, pour out the slag, and pour out the thin slag on the surface of the molten pool. The amount of slag poured is 2-3 tons. After the slag is poured, the amount of slag in the converter will decrease. At this time, add 2-3 kg / t of lime into the converter, and then perform the tapping operation. No alloy or deoxidizer is added during the tapping process to avoid the P reaction after adding alloy or deoxidizer during the tapping process; (4) When tapping, 1-2t of steel is retained to reduce the amount of slag in the tapping process. After tapping, slag removal is performed first, and then alloying is performed to avoid alloying back to P. After the above operations, sampling and testing are performed after tapping at the end of the converter. The molten steel returns to P of 0, or w[P] is reduced by 0.0002-0.001%, achieving the goal of controlling P during converter smelting of low-carbon steel.

2. A smelting method for suppressing P recovery in low carbon steel according to claim 1, characterized in that: The self-made cold-pressed balls are made by mixing the self-produced converter slag and LF ladle furnace slag with components meeting the requirements with pure Fe obtained through magnetic separation and then pressing them.