Al-Mg-Si alloy material, preparation process thereof and high-voltage component annular aluminum alloy coil

Through the Al-Mg-Si alloy material and its preparation process, the toughness and cooling problems of aluminum coils in high-voltage components are solved, and a high-strength and well-cooled high-voltage component ring-shaped aluminum alloy coil is achieved, which meets the requirements of high-voltage electrical components. Use demand.

CN118726802APending Publication Date: 2024-10-01JIANGSU ASIA-PACIFIC AVIATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410718946.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The application of existing aluminum coils in high-voltage components is limited by their poor toughness and high calorific value, resulting in limited use in high-voltage electrical applications.

Method used

Al-Mg-Si alloy material and its preparation process are used to prepare high-strength aluminum alloy profiles with water cooling holes through steps such as smelting, refining, casting, homogenization and extrusion, which are used to prepare ring-shaped aluminum for high-voltage components. Alloy coil.

Benefits of technology

It achieves good electrical conductivity and mechanical properties, and ensures good cooling characteristics, meeting the strength and cooling needs of high-voltage electric coils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726802A_ABST
    Figure CN118726802A_ABST
Patent Text Reader

Abstract

The invention provides an Al-Mg-Si alloy material, a preparation process thereof and an annular aluminum alloy coil of a high-voltage assembly. The Al-Mg-Si alloy material comprises the following components in percentage by mass: 0.4-0.5% of silicon, 0.1-0.2% of iron, less than or equal to 0.05% of copper, less than or equal to 0.05% of manganese, 0.5-0.7% of magnesium, less than or equal to 0.1% of zinc and the balance of aluminum and inevitable impurities, and the mass ratio of magnesium to silicon is 1.1-1.6. The Al-Mg-Si alloy material can reach the strength of 6-series aluminum alloy and good subsequent processability, can meet the requirement of customers for conductivity, and can be well used as a raw material of a high-voltage electric coil. The Al-Mg-Si alloy profile prepared through the method is provided with water cooling holes. A high-voltage assembly annular aluminum alloy coil prepared through the Al-Mg-Si alloy profile bar can obtain good electric conductivity and mechanical performance, and the good cooling characteristic can be guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for preparing a high-voltage component annular aluminum alloy coil, which is applicable to the field of transformer coils of aluminum alloy for high-voltage electricity. Background Art

[0002] Coil usually refers to a ring-shaped wire winding. The most common coil applications include: motors, inductors, transformers and loop antennas. The industry generally uses copper or aluminum alloy coils. Compared with copper winding coils, aluminum coils are more economical, thanks to the low unit price and low density of aluminum alloy materials. However, aluminum coils have poor toughness, are easy to break, and generate high heat. Therefore, the use of aluminum coils in high-voltage components is limited. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an Al-Mg-Si alloy material and a preparation process thereof, and a high-voltage component annular aluminum alloy coil. The Al-Mg-Si alloy profile prepared by the present invention has water cooling holes, and the high-voltage component annular aluminum alloy coil made of the above-mentioned rod can obtain good electrical conductivity and mechanical properties and can ensure good cooling characteristics.

[0004] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:

[0005] In a first aspect, an embodiment of the present invention provides an Al-Mg-Si alloy material, comprising the following components in terms of mass percentage:

[0006] Silicon: 0.4-0.5%, Iron: 0.1-0.2%, Copper ≤0.05%, Manganese ≤0.05%, Magnesium: 0.5%-0.7%, Zinc ≤0.1, the remainder is aluminum and unavoidable impurities, among which the mass ratio of magnesium to silicon is 1.1-1.6.

[0007] In a second aspect, an embodiment of the present invention provides a process for preparing the Al-Mg-Si alloy material according to the first aspect, comprising the following steps:

[0008] (1) According to the above-mentioned component ratio, the ingredients except magnesium are charged into a furnace and smelted at a temperature of 750-780°C;

[0009] (2) Add magnesium element to the furnace according to the component ratio, first mechanically stir for 10 to 20 minutes, then electromagnetically stir for 30 to 40 minutes, continue smelting, and slag at the same time;

[0010] (3) Refining: The refining temperature is 760-780°C, the time is 30-35 minutes, and the slag is removed at the same time;

[0011] (4) Casting: The furnace temperature is 790-805°C, titanium boron wire is fed online, Hycast is used for online two-stage degassing and slag removal, Hycast is used for low-pressure vacuum casting, and the casting speed is 110±5 mm / min to obtain cast rods;

[0012] (5) performing homogenization treatment at a temperature of 555 to 575° C. and a holding time of 6 to 6.2 hours;

[0013] (6) The alloy material after homogenization treatment is subjected to extrusion treatment and then aging treatment. After being taken out of the furnace and air-cooled, a high-strength Al-Mg-Si alloy profile is obtained.

[0014] Furthermore, the extrusion process in step (6) comprises the following steps:

[0015] 1) Extruder preparation stage: heat the die barrel to 430-440°C, and the extrusion die temperature is 470-490°C;

[0016] 2) Heat the homogenized cast rod and control the temperature gradient: 510±10℃ at the head, 500±10℃ in the middle, and 490±10℃ at the tail.

[0017] 3) Online spray cooling is used for extrusion, the outflow speed is controlled to be ≥7.0mm / s, the extrusion outlet temperature is 510-530℃, and liquid nitrogen is used to cool the mold cavity during the extrusion process.

[0018] Furthermore, in step (6), the product obtained after the extrusion treatment is subjected to aging treatment at 170-180° C. for 360-390 min.

[0019] Furthermore, the high-strength Al-Mg-Si alloy profile obtained in step (6) has a tensile strength of ≥240 MPa, a yield strength of ≥220 MPa, an elongation after fracture (A) of ≥12%, and an electrical conductivity of ≥53% IACS.

[0020] Furthermore, the high-strength Al-Mg-Si alloy profile obtained in step (6) has a water cooling hole at its center, and the cooling hole diameter d=0.4-0.6L, wherein L is the diameter of the maximum circumscribed circle of the cooling hole.

[0021] In a third aspect, an embodiment of the present invention provides a high voltage component annular aluminum alloy coil, which is made of an Al-Mg-Si alloy profile obtained by the preparation process of the second aspect.

[0022] The technical solution provided by the embodiment of the present invention has the following beneficial effects:

[0023] 1) The Al-Mg-Si alloy material of the present invention can achieve the strength and good subsequent processability of 6 series aluminum alloys, and can also meet the customer's requirements for electrical conductivity, and can be well used as the raw material for high-voltage electric coils.

[0024] 2) The alloy material of the present invention has excellent mechanical properties: tensile strength ≥ 240 MPa, yield strength ≥ 220 MPa, and elongation after fracture (A) ≥ 12%.

[0025] 3) The conductivity of the high voltage component annular aluminum alloy coil made using the alloy material of the present invention is ≥53% IACS, and due to the arrangement of water cooling holes in the rod, the product has good cooling performance, ensuring that the operating temperature is ≤155°C, meeting the cooling requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a diagram of the organizational structure of the Al-Mg-Si alloy material obtained by casting in Comparative Example 1 of the present invention.

[0027] Figure 2 It is a diagram of the organizational structure of the Al-Mg-Si alloy material obtained by casting in Example 1 of the present invention.

[0028] Figure 3 It is a schematic diagram of the cross-sectional structure of an Al-Mg-Si alloy profile obtained by casting according to an embodiment of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] Example

[0031] The Al-Mg-Si alloy material is formed into Examples 1-3 and Comparative Examples 1-2 according to different composition ratios (see Table 1 below), wherein the magnesium-silicon ratio of Comparative Example 1 exceeds the upper limit required, and that of Comparative Example 2 exceeds the lower limit. The magnesium-silicon ratio of Examples 1-3 is in the range of 1.1-1.6.

[0032] Table 1 Elemental composition of Al-Mg-Si alloy materials in Comparative Examples 1-2 and Examples 1-3

[0033] Compare Projects silicon iron copper magnesium manganese Zinc aluminum Magnesium-silicon ratio Comparative Example 1 0.405 0.193 0.014 0.682 0.0103 0.0087 margin 1.684 Comparative Example 2 0.461 0.156 0.041 0.501 0.0084 0.0193 margin 1.086 Example 1 0.419 0.14 0.00283 0.542 0.0045 0.0075 margin 1.294 Example 2 0.436 0.132 0.000326 0.585 0.0025 0.0043 margin 1.342 Example 3 0.437 0.14 0.000281 0.579 0.0035 0.0033 margin 1.325

[0034] The Al-Mg-Si alloy materials in Comparative Examples 1-2 and Examples 1-3 were prepared using the same preparation process, including the following steps:

[0035] (1) According to the above-mentioned component proportions, except for magnesium, the ingredients are charged into a furnace for smelting at a temperature of 765°C;

[0036] (2) Add magnesium element to the furnace according to the component ratio, and stir mechanically for 15 minutes and electromagnetically for 30 minutes, continue smelting, and slag removal at the same time;

[0037] (3) Refining, temperature is 770°C, time is 30 min, and slag is removed at the same time;

[0038] (4) Casting: The furnace temperature is 795°C, titanium boron wire is fed online, Hycast is used for online two-stage degassing and slag removal, Hycast is used for low-pressure vacuum casting, and the casting speed is 110 mm / min;

[0039] (5) homogenization treatment was performed at 540°C for 10 hours;

[0040] (6) The alloy material after homogenization treatment is subjected to extrusion treatment, and then aging treatment is performed. After being air-cooled out of the furnace, a high-strength Al-Mg-Si alloy profile is obtained. The center of the Al-Mg-Si alloy profile has a water cooling hole, and the cooling hole diameter d=0.4-0.6L, where L is the diameter of the maximum circumscribed circle of the cooling hole, such as Figure 3 shown.

[0041] The extrusion process includes the following steps:

[0042] 1) Extruder preparation stage: heat the die barrel to 435°C and the extrusion die temperature to 480°C;

[0043] 2) Heat the homogenized cast rod and control the temperature gradient: 510°C at the head, 500°C in the middle, and 490°C at the tail.

[0044] 3) Online spray cooling is adopted for extrusion, and the outflow speed needs to be controlled to be ≥7.0mm / s, and the extrusion outlet temperature is 510-530℃; liquid nitrogen is used to cool the mold cavity during the extrusion process.

[0045] The aging treatment (T6) includes the following steps: framing aging after extrusion, the product metal needs to be controlled to be aged at 175°C for 360 minutes, and high conductivity Al-Mg-Si alloy profiles can be obtained after air cooling after being taken out of the furnace.

[0046] like Figure 1 As shown, it is a diagram of the organizational structure of the Al-Mg-Si alloy material obtained by casting in comparative example 1 of the present invention. It can be seen that since the Mg / Si in comparative example 1 is greater than 1.6, the organizational uniformity in the alloy material is reduced, and the grains tend to be coarsened compared with embodiment 1.

[0047] like Figure 2, which is a diagram of the organizational structure of the Al-Mg-Si alloy material obtained by casting in Example 1 of the present invention. It can be seen that the organizational grains of the alloy material in Example 1 are uniform.

[0048] The high-strength Al-Mg-Si alloy profiles obtained in Comparative Examples 1-2 and Examples 1-3 were made into profile products with the same size and cooling hole size (the cooling hole d=0.5L was selected in the product cross-section), and the mechanical properties and electrical conductivity of the profile products in Comparative Examples 1-2 and Examples 1-3 were statistically analyzed. The results are shown in Table 2.

[0049] Table 2 Mechanical properties and electrical conductivity (T6 state) of Al-Mg-Si alloy profiles in Comparative Examples 1-2 and Examples 1-3

[0050]

[0051] From the above table, it can be seen that the Al-Mg-Si alloy profiles in Examples 1-3 can meet the following mechanical properties: tensile strength ≥ 240MPa, yield strength ≥ 220MPa, elongation after fracture (A) ≥ 15%; and when the product is at room temperature 20°C, the electrical conductivity ≥ 53% IACS. In Comparative Example 1, the aluminum-silicon ratio in the aluminum alloy material is too high, and the mechanical properties of the obtained Al-Mg-Si alloy profile are significantly reduced, and the electrical conductivity is also reduced. In Comparative Example 2, the aluminum-silicon ratio in the aluminum alloy material is too low, and the electrical conductivity of the obtained Al-Mg-Si alloy profile is reduced.

[0052] The Al-Mg-Si alloy profiles in Example 1 were produced in the same production equipment and under the same preparation process with the same size but different cooling hole sizes, which were respectively recorded as products a, b, c, and d, as shown in Table 3; and the mechanical properties, electrical conductivity and cooling effect of each product were statistically analyzed, as shown in Table 4.

[0053] Table 3 Aperture sizes in products a, b, c and d

[0054] product Cooling hole size a d=0.3L b d=0.5L c d=0.7L d d=0, no cooling hole

[0055] Table 4 Mechanical properties and electrical conductivity of products a, b, c, d (T6 state)

[0056]

[0057] From the table above, we can see that products a, b, and d can all achieve the following mechanical properties: tensile strength ≥ 240MPa, yield strength ≥ 220MPa, elongation after fracture (A) ≥ 15%; and when the product is at room temperature 20°C, the conductivity ≥ 53% IACS; however, during the operation of the equipment, the water cooling effect of product b can achieve the expected effect, while product a has a small cooling hole size and exhibits poor cooling effect, while product c has a large cooling hole size, a corresponding thin wall thickness, and poor elongation, which affects the processing of the coil. Product d has the worst water cooling effect because it does not have cooling holes and cannot meet actual production needs.

[0058] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. An Al-Mg-Si alloy material, characterized in that: According to mass percentage, it includes the following components: Silicon: 0.4-0.5%, Iron: 0.1-0.2%, Copper ≤0.05%, Manganese ≤0.05%, Magnesium: 0.5%-0.7%, Zinc ≤0.1, the remainder is aluminum and unavoidable impurities, among which the mass ratio of magnesium to silicon is 1.1-1.

6.

2. The preparation process of the Al-Mg-Si alloy material according to claim 1, characterized in that: The following steps are involved: (1) According to the above-mentioned component ratio, the ingredients except magnesium are charged into a furnace and smelted at a temperature of 750-780°C; (2) Add magnesium element to the furnace according to the component ratio, stir mechanically for 10 to 20 minutes, then stir electromagnetically for 30 to 40 minutes, continue smelting, and slag at the same time; (3) Refining: The refining temperature is 760-780℃, the time is 30-35min, and the slag is removed at the same time; (4) Casting: The furnace temperature is 790-805°C, titanium boron wire is fed online, Hycast is used for online two-stage degassing and slag removal, Hycast is used for low-pressure vacuum casting, and the casting speed is 110±5 mm / min to obtain cast rods; (5) Performing homogenization treatment at a temperature of 555 to 575°C and a holding time of 6 to 6.2 hours; (6) The alloy material after homogenization treatment is extruded and then aged. After being air-cooled out of the furnace, a high-strength Al-Mg-Si alloy profile is obtained.

3. The preparation process of the Al-Mg-Si alloy material according to claim 2, characterized in that: The extrusion process in step (6) comprises the following steps: 1) Extruder preparation stage: heat the die barrel to 430-440°C, and the extrusion die temperature is 470-490°C; 2) Heat the homogenized cast rod and control the temperature gradient: 510±10℃ at the head, 500±10℃ in the middle, and 490±10℃ at the tail; 3) Online spray cooling is used for extrusion, the outflow speed is controlled to be ≥7.0mm / s, the extrusion outlet temperature is 510-530℃, and liquid nitrogen is used to cool the mold cavity during the extrusion process.

4. The preparation process of the Al-Mg-Si alloy material according to claim 2, characterized in that: In step (6), the product obtained after the extrusion treatment is subjected to aging treatment at 170 to 180° C. for 360 to 390 minutes.

5. The preparation process of the Al-Mg-Si alloy material according to claim 2, characterized in that: The high-strength Al-Mg-Si alloy profile obtained in step (6) has a tensile strength of ≥240 MPa, a yield strength of ≥220 MPa, an elongation after fracture (A) of ≥12%, and an electrical conductivity of ≥53% IACS.

6. The process for preparing the Al-Mg-Si alloy material according to claim 2, characterized in that: The high-strength Al-Mg-Si alloy profile obtained in step (6) has a water cooling hole at its center, and the cooling hole diameter d=0.4-0.6L, where L is the diameter of the maximum circumscribed circle of the cooling hole.

7. A high voltage component annular aluminum alloy coil, characterized in that: The Al-Mg-Si alloy profile is made by the preparation process according to any one of claims 2 to 6.