Plating assistant agent for hot-dip coating of aluminum-zinc alloy by solvent method and coating process of plating assistant agent

Through the combination of modified surfactants and specific process steps, the problem of insufficient stability and pollution of the plating aid is solved, the quality and environmental protection of the aluminum-zinc alloy coating are improved, and the stability and environmental protection of the coating are improved.

CN118726883APending Publication Date: 2024-10-01ZHENJIANG ZHONGYUAN ELECTRIC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411014084.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing plating fluxes have insufficient stability, pollution problems and difficulty in subsequent processing during use, resulting in inconsistent coating quality and environmental pollution.

Method used

Modified surfactants are prepared using a solvent method, including alkylphenol polyoxyethylene ether, sodium alkylbenzene sulfonate and polyethylene glycol, combined with potassium chloride, zinc chloride, boric acid, sodium nitrate, potassium sulfate and diphosphate. Sodium hydride forms aluminum-zinc alloy coating through specific process steps such as surface cleaning, flux treatment, drying, hot plating and cooling.

Benefits of technology

It significantly improves the stability and environmental protection of the coating, reduces pollution and difficulty in subsequent processing, reduces production costs, and improves the adhesion and corrosion resistance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965208890000071
    Figure BDA0004965208890000071
Patent Text Reader

Abstract

The invention provides a plating assistant for hot-dip coating of an aluminum-zinc alloy by a solvent method and a coating process of the plating assistant. The plating assistant comprises the following components in percentage by mass: 30-50% of potassium chloride; 40-60% of zinc chloride; 0.1-1% of boric acid; 0.1-1% of sodium nitrate; 0.1-1% of potassium sulfate; 0.1%-1% of sodium dihydrogen phosphate; and 0.1 to 0.5 percent of a modified surfactant. The process comprises the steps of base material treatment, plating assistant treatment, drying treatment, hot dipping treatment, cooling treatment and post-treatment, and various properties of an aluminum-zinc alloy coating, especially corrosion resistance and adhesive force, are remarkably improved by using a modified surfactant; the modified surface active agent enhances the protection effect of the plating assistant and improves the binding force of a plating layer and a base material, so that the plating layer is more uniform, and the phenomena of falling and foaming are reduced. And meanwhile, the coating process parameters of the plating assistant for the solvent method hot-dip aluminum-zinc alloy are optimized, so that the adhesive force, the corrosion resistance and the process stability of the coating are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of a plating aid, and more specifically to a plating aid for hot-dip aluminum-zinc alloy by a solvent method and a plating process thereof. Background Art

[0002] Hot-dip aluminum-zinc alloy is an anti-corrosion coating material widely used in the fields of construction, automobiles, home appliances, etc. The aluminum-zinc alloy coating not only has excellent corrosion resistance, but also has the high-temperature oxidation resistance of aluminum and the electrochemical protection of zinc. Therefore, aluminum-zinc alloy coating plays an important role in many industrial applications. In the process of hot-dip aluminum-zinc alloy, the selection and use of plating agents are key factors affecting the quality of the coating. The main function of the plating agent is to promote the adhesion and uniformity of the coating by reducing the oxide layer on the surface of the substrate.

[0003] At present, surfactants are often added to the plating solution to improve the effect, but the current added surfactants have the following problems:

[0004] (1) Unstable plating effect: The plating effect of traditional surfactants is not stable enough in actual use and is easily affected by environmental factors (and the surface state of the substrate, resulting in large fluctuations in the quality of the coating and difficulty in ensuring consistency;

[0005] (2) Pollution problem: Some chemical components of existing surfactants are highly toxic or difficult to degrade, which causes environmental pollution during their production and use.

[0006] (3) Subsequent treatment is difficult: After using traditional surfactants, the plating agent remaining on the surface of production equipment and products is often difficult to remove and requires a large amount of water and chemical cleaning agents to be treated. This not only increases production costs, but also generates a large amount of wastewater and waste, further increasing the environmental burden.

[0007] Therefore, in order to improve the quality of the coating, the plating solution needs to be further improved. Summary of the invention

[0008] In order to solve the shortcomings of the prior art, a solvent-based hot-dip aluminum-zinc alloy plating aid and a plating process thereof are provided. The specific scheme is as follows:

[0009] A plating aid for hot-dip aluminum-zinc alloy by solvent method, the plating aid comprises the following components in percentage by mass: 30-50% potassium chloride; 40-60% zinc chloride; 0.1-1% boric acid; 0.1-1% sodium nitrate; 0.1-1% potassium sulfate; 0.1-1% sodium dihydrogen phosphate; and 0.1-0.5% modified surfactant.

[0010] Furthermore, the modified surfactant is composed of the following components: alkylphenol polyoxyethylene ether; sodium alkylbenzene sulfonate; polyethylene glycol.

[0011] Furthermore, the preparation method of the modified surfactant is as follows: alkylphenol polyoxyethylene ether and sodium alkylbenzene sulfonate are mixed in a ratio of 1:1, and stirred at 80° C. for 30 minutes, and finally polyethylene glycol is added and stirred for 10 minutes.

[0012] A coating process of a solvent-based hot-dip aluminum-zinc alloy plating aid, the coating process comprising the following steps:

[0013] S1. Substrate treatment: Select aluminum-zinc alloy substrate, clean the surface, use degreasing agent to clean at 60℃ for 10 minutes to remove oil stains and impurities; use sulfuric acid solution for pickling; finally rinse with deionized water;

[0014] S2, plating agent treatment: prepare a plating agent according to the composition of 30-50% potassium chloride; 40-60% zinc chloride; 0.1-1% boric acid; 0.1-1% sodium nitrate; 0.1-1% potassium sulfate; 0.1-1% sodium dihydrogen phosphate; 0.1-0.5% modified surfactant, heat the prepared plating agent solution; immerse the treated substrate in the plating agent solution for 5 minutes to ensure that the plating agent is evenly covered on the surface of the substrate;

[0015] S3, Drying treatment: Take out the substrate from the plating agent solution and use compressed air to blow dry its surface; put it in an oven and dry it at 120°C for 10 minutes to ensure that the plating agent is completely dry and form a dense protective layer, avoiding the presence of moisture in the subsequent hot-dip process, reducing the defects of the coating, and thus improving the corrosion resistance;

[0016] S4, hot-dip treatment: immerse the dried substrate into a molten aluminum-zinc alloy bath; keep the immersion time at 2 minutes to make the aluminum-zinc alloy evenly cover the surface of the substrate;

[0017] S5. Cooling treatment: Take out the substrate from the aluminum-zinc alloy bath and quickly put it into the water cooling tank for cooling. The water temperature is 25°C. The cooling time is 30 seconds to ensure that the coating solidifies quickly and prevents oxidation.

[0018] S6. Post-processing: Take out the cooled substrate from the water cooling tank and wash it again with deionized water; apply anti-rust oil on the surface of the substrate for protective treatment; place it in a dry and ventilated place.

[0019] Furthermore, the concentration of sulfuric acid during the pickling of S1 is 5%.

[0020] Furthermore, the pickling parameters in S1 are that the pickling temperature is 20-30° C. and the time is 2 min.

[0021] Furthermore, the S2 plating aid solution is heated to 80° C. so that the plating aid is evenly covered on the surface of the substrate, further improving the uniformity and density of the coating.

[0022] Furthermore, the temperature of the aluminum-zinc alloy bath in S4 is 400-500°C. By controlling the temperature of the aluminum-zinc alloy bath at 400-500°C and maintaining the immersion time at 2 minutes, the coating is evenly covered on the surface of the substrate, ensuring the stability and repeatability of the process.

[0023] Beneficial effects:

[0024] The present invention provides a solvent-based hot-dip aluminum-zinc alloy plating aid and a plating process thereof, which has the following characteristics:

[0025] Beneficial effects:

[0026] (1) The use of modified surfactants significantly improves the various properties of aluminum-zinc alloy coatings, especially in terms of corrosion resistance and adhesion. Modified surfactants enhance the protective effect of the plating aid and improve the bonding strength between the coating and the substrate, making the coating more uniform and reducing shedding and blistering, thereby ensuring the stability and consistency of the coating quality.

[0027] (2) Compared with traditional surfactants, the ingredients used in modified surfactants are more environmentally friendly, reducing the use of toxic or difficult-to-degrade chemical ingredients, thereby reducing the risk of environmental pollution. At the same time, the residues of the plating agent are easier to remove, reducing the difficulty of subsequent treatment and the impact on the environment.

[0028] (3) The modified surfactant improves the stability and effectiveness of the plating agent, reducing the rework rate due to coating quality problems. In addition, since the residue is easy to remove, the amount of water and chemical cleaning agents used in the cleaning step is reduced, thereby reducing production costs.

[0029] (4) By reducing the use of toxic chemical components, the plating aid of the present invention helps to improve the working environment in the production process, reduce the risk of workers being exposed to harmful substances, and improve the safety level of the factory.

[0030] (5) By optimizing the plating process parameters of the solvent-based hot-dip aluminum-zinc alloy plating aid, the adhesion, corrosion resistance and process stability of the coating were significantly improved. DETAILED DESCRIPTION

[0031] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0032] Embodiment 1:

[0033] (1) Preparation of plating aid

[0034] The components of the plating agent are as follows:

[0035] Potassium chloride: 40%

[0036] Zinc chloride: 50%

[0037] Boric acid: 0.5%

[0038] Sodium nitrate: 0.5%

[0039] Potassium sulfate: 0.5%

[0040] Sodium dihydrogen phosphate: 0.5%

[0041] Modified surfactant: 0.3%

[0042] (2) Preparation of modified surfactants

[0043] First, alkylphenol polyoxyethylene ether and sodium alkylbenzene sulfonate were mixed in a ratio of 1:1 and stirred at 80°C for 30 minutes.

[0044] Polyethylene glycol was then added and stirring was continued for 10 minutes.

[0045] (3) Plating process

[0046] S1. Substrate treatment: The aluminum-zinc alloy substrate was cleaned with a degreasing agent at 60° C. for 10 minutes, pickled (sulfuric acid concentration 5%, temperature 25° C., time 2 minutes), and rinsed with deionized water.

[0047] S2. Plating flux treatment: The plating flux solution is heated to 80°C and the substrate is immersed for 5 minutes.

[0048] S3. Drying treatment: Blow dry the surface of the substrate at 120°C for 10 minutes.

[0049] S4, hot-dip treatment: the substrate is immersed in a 400°C aluminum-zinc alloy bath for 2 minutes.

[0050] S5. Cooling treatment: water temperature 25°C, cooling for 30 seconds.

[0051] S6. Post-processing: clean with deionized water, apply anti-rust oil, dry and ventilate.

[0052] Embodiment 2:

[0053] (1) Preparation of plating aid

[0054] The components of the plating flux are as follows:

[0055] Potassium chloride: 35%

[0056] Zinc chloride: 55%

[0057] Boric acid: 0.8%

[0058] Sodium nitrate: 0.2%

[0059] Potassium sulfate: 0.3%

[0060] Sodium dihydrogen phosphate: 0.7%

[0061] Modified surfactant: 0.2%

[0062] (2) Preparation of modified surfactants

[0063] First, alkylphenol polyoxyethylene ether and sodium alkylbenzene sulfonate were mixed in a ratio of 1:1 and stirred at 80°C for 30 minutes.

[0064] Polyethylene glycol was then added and stirring was continued for 10 minutes.

[0065] (3) Plating process

[0066] S1. Substrate treatment: The aluminum-zinc alloy substrate was cleaned with a degreasing agent at 60° C. for 10 minutes, pickled (sulfuric acid concentration 5%, temperature 25° C., time 2 minutes), and rinsed with deionized water.

[0067] S2. Plating flux treatment: The plating flux solution is heated to 80°C and the substrate is immersed for 5 minutes.

[0068] S3. Drying treatment: Blow dry the surface of the substrate at 120°C for 10 minutes.

[0069] S4, hot-dip treatment: the substrate is immersed in a 400°C aluminum-zinc alloy bath for 2 minutes.

[0070] S5. Cooling treatment: water temperature 25°C, cooling for 30 seconds.

[0071] S6. Post-processing: clean with deionized water, apply anti-rust oil, dry and ventilate.

[0072] Embodiment 3:

[0073] (1) Preparation of plating aid

[0074] The components of the plating flux are as follows:

[0075] Potassium chloride: 45%

[0076] Zinc chloride: 50%

[0077] Boric acid: 0.4%

[0078] Sodium nitrate: 0.4%

[0079] Potassium sulfate: 0.2%

[0080] Sodium dihydrogen phosphate: 0.5%

[0081] Modified surfactant: 0.4%

[0082] (2) Preparation of modified surfactants

[0083] First, alkylphenol polyoxyethylene ether and sodium alkylbenzene sulfonate were mixed in a ratio of 1:1 and stirred at 80°C for 30 minutes.

[0084] Polyethylene glycol was then added and stirring was continued for 10 minutes.

[0085] (3) Plating process

[0086] S1. Substrate treatment: The aluminum-zinc alloy substrate was cleaned with a degreasing agent at 60° C. for 10 minutes, pickled (sulfuric acid concentration 5%, temperature 25° C., time 2 minutes), and rinsed with deionized water.

[0087] S2. Plating flux treatment: The plating flux solution is heated to 80°C and the substrate is immersed for 5 minutes.

[0088] S3. Drying treatment: Blow dry the surface of the substrate at 120°C for 10 minutes.

[0089] S4, hot-dip treatment: the substrate is immersed in a 400°C aluminum-zinc alloy bath for 2 minutes.

[0090] S5. Cooling treatment: water temperature 25°C, cooling for 30 seconds.

[0091] S6. Post-processing: clean with deionized water, apply anti-rust oil, dry and ventilate.

[0092] Comparative Example:

[0093] The preparation steps are similar to those of Example 1, except that no modified surfactant is used.

[0094] The performance of the aluminum-zinc alloys obtained in Examples 1 to 3 and the comparative example after coating was tested, and the data are as follows:

[0095]

[0096] By comparing the experimental results, it can be seen that the modified surfactant significantly improves the various properties of the aluminum-zinc alloy coating. Specifically, the corrosion resistance of the embodiment is much better than that of the comparative example by 100 hours. This shows that the modified surfactant enhances the protective effect of the plating aid. : The adhesion of all embodiments reaches 5B level, 100% without shedding, while the comparative example is only 3B level. This shows that the modified surfactant improves the bonding strength between the coating and the substrate and reduces shedding and blistering.

[0097] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A solvent-based hot-dip aluminum-zinc alloy plating agent, characterized in that: The plating aid comprises the following components in percentage by mass: 30-50% potassium chloride; 40-60% zinc chloride; 0.1-1% boric acid; 0.1-1% sodium nitrate; 0.1-1% potassium sulfate; 0.1-1% sodium dihydrogen phosphate; and 0.1-0.5% modified surfactant.

2. A solvent-based hot-dip aluminum-zinc alloy plating flux according to claim 1, characterized in that: The modified surfactant is composed of the following components: alkylphenol polyoxyethylene ether; sodium alkylbenzene sulfonate; and polyethylene glycol.

3. A solvent-based hot-dip aluminum-zinc alloy plating agent according to claim 1, characterized in that: The preparation method of the modified surfactant is as follows: alkylphenol polyoxyethylene ether and sodium alkylbenzene sulfonate are mixed in a ratio of 1:1, stirred at 80°C for 30 minutes, and finally polyethylene glycol is added and stirred for 10 minutes.

4. A coating process using a plating aid for hot-dip aluminum-zinc alloy by solvent method, characterized in that: The coating process comprises the following steps: S1. Substrate treatment: Select aluminum-zinc alloy substrate, clean the surface, use degreasing agent to clean at 60℃ for 10 minutes to remove oil stains and impurities; use sulfuric acid solution for pickling; finally rinse with deionized water; S2, plating agent treatment: prepare a plating agent according to the composition of 30-50% potassium chloride; 40-60% zinc chloride; 0.1-1% boric acid; 0.1-1% sodium nitrate; 0.1-1% potassium sulfate; 0.1-1% sodium dihydrogen phosphate; 0.1-0.5% modified surfactant, heat the prepared plating agent solution; immerse the treated substrate in the plating agent solution for 5 minutes to ensure that the plating agent is evenly covered on the surface of the substrate; S3, drying treatment: take out the substrate from the plating agent solution, use compressed air to blow dry its surface; put it in an oven and dry it at 120°C for 10 minutes to ensure that the plating agent is completely dry; S4, hot-dip treatment: immerse the dried substrate into a molten aluminum-zinc alloy bath; keep the immersion time at 2 minutes to make the aluminum-zinc alloy evenly cover the surface of the substrate; S5. Cooling treatment: Take out the substrate from the aluminum-zinc alloy bath and quickly put it into the water cooling tank for cooling. The water temperature is 25°C. The cooling time is 30 seconds to ensure that the coating solidifies quickly and prevents oxidation. S6. Post-processing: Take out the cooled substrate from the water cooling tank and wash it again with deionized water; apply anti-rust oil on the surface of the substrate for protective treatment; place it in a dry and ventilated place.

5. The coating process of a solvent hot-dip aluminum-zinc alloy plating agent according to claim 4, characterized in that: The concentration of sulfuric acid during S1 pickling is 5%.

6. A coating process for a solvent-based hot-dip aluminum-zinc alloy plating agent according to claim 4, characterized in that: The pickling parameters in S1 are pickling temperature of 20-30°C and time of 2 min.

7. A coating process for a solvent-based hot-dip aluminum-zinc alloy plating flux according to claim 4, characterized in that: The S2 flux solution is heated to 80°C.

8. The coating process of a solvent-based hot-dip aluminum-zinc alloy plating agent according to claim 4, characterized in that: The temperature of the aluminum-zinc alloy bath in S4 is 400-500°C.

Citation Information

Patent Citations

  • Manufacturing process of sling hooks

    CN103612070A

  • Plating aid for hot dipping Galfan alloys and plating aid solution

    CN105154804A

  • Hot galvanizing plating leakage preventing method

    CN111979506A

  • Flux and process for hot dip galvanization

    US20070137731A1