Ag-MoS2 composite lubricating coating and preparation method thereof

By doping Ag in the MoS2 coating, a nanocomposite structure is constructed, and the Ag-MoS2 composite coating is deposited using non-equilibrium magnetron sputtering technology, which solves the problem of large friction coefficient of the metal-doped MoS2 coating in the existing technology and achieves Provides low friction coefficient and long life lubrication effect.

CN118726907APending Publication Date: 2024-10-01LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410774081.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing metal-doped MoS2 coating has a large friction coefficient in the space environment, which affects the coating life and lubrication performance.

Method used

The 5-30 at.% Ag-doped MoS2 composite lubricating coating is deposited in a vacuum environment through non-equilibrium magnetron sputtering technology. The Ag atomic percentage and coating thickness are adjusted to build a nanocomposite structure to reduce the friction coefficient.

Benefits of technology

Achieve extremely low friction coefficient in vacuum environment, meet the lubrication requirements of spacecraft mechanical moving parts, and extend the life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726907A_ABST
    Figure CN118726907A_ABST
Patent Text Reader

Abstract

The invention provides an Ag-MoS2 composite lubricating coating and a preparation method thereof.The Ag-doped MoS2 composite lubricating coating is prepared through the magnetron sputtering technology, and the atomic percent of Ag is 5-30 at.%. According to the Ag-MoS2 composite lubricating coating and the preparation method thereof, the metal-doped MoS2 coating has the advantages that the friction coefficient of the composite coating in the vacuum environment is reduced, the friction coefficient of the composite coating in the vacuum environment is reduced, and the service life of the composite coating is prolonged. And the requirements of key mechanical moving parts of spacecrafts on the solid lubricating coating are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides an Ag-MoS2 composite lubricating coating and a preparation method thereof, and relates to the technical field of surface protection of moving parts. Background Art

[0002] Satellites, space stations, interstellar probes and other spacecraft face harsh working conditions such as high vacuum, strong radiation and microgravity when serving in the space environment. Space lubricating materials are one of the key factors to ensure the safe, reliable and long-term stable operation of spacecraft motion mechanisms in orbit. MoS2 has a unique layered hexagonal crystal structure, with weak van der Waals forces between layers and low shear force. Therefore, it has excellent self-lubricating properties and is widely used as a solid lubricating material for space. However, the single MoS2 coating prepared by magnetron sputtering has a loose columnar crystal structure, which is difficult to resist the intrusion of oxygen and water vapor, and has obvious deficiencies in wear resistance and load-bearing capacity, thus affecting the coating life.

[0003] Element doping technology is used to improve the density of the coating structure and its load-bearing capacity. Currently, the MoS2 coating is doped with metals such as Cr, Ti, and Zr to increase the coating life, but there are problems such as increased friction coefficient and reduced lubricity. Summary of the invention

[0004] The invention provides an Ag-MoS2 composite lubricating coating and a preparation method thereof, which solves the technical problem of a large friction coefficient of a metal-doped MoS2 coating in the prior art.

[0005] The present invention is achieved in that the composite lubricating coating is composed of 5 to 30 at.% Ag doped MoS2, and the thickness of the composite lubricating coating is 1500 to 3500 nm.

[0006] As a further preselection, the atomic percentage of Ag in the composite lubricating coating is 15 at.%.

[0007] As a further preference, the thickness of the composite lubricating coating is 2500 nm.

[0008] The preparation method of the Ag-MoS2 composite lubricating coating comprises the following steps: (1) Preprocessing The substrate was cleaned for 30 min and dried for later use; (2) Pre-sputtering cleaning The substrate obtained in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, argon gas was introduced, the argon gas flow rate was 30 sccm, the etching pressure was 0.2 Pa, the substrate bias was -400 V, and the pre-sputtering cleaning was 20-30 min; (3) Deposition of Ag-MoS2 composite lubricating coating Unbalanced magnetron sputtering technology was used, the argon flow rate was increased to 70 sccm, the deposition gas pressure was 0.35 Pa, the substrate bias was continuously adjusted to 0 V, and an RF power supply was applied to the MoS2 target. The sputtering power of the MoS2 target was continuously increased to 600 W. At this time, a DC power supply was applied to the pure Ag target, the deposition current was adjusted to 0.1~0.3 A, the rotating frame speed was 0.5 r / min, and the deposition time was 120 min to deposit the Ag-MoS2 composite lubricating coating.

[0009] As a further preference, the pre-sputtering cleaning time in step (2) is 25 min.

[0010] As a further preference, in the step (3), the Ag deposition current is 0.2 A.

[0011] As a further preference, the substrate in step (1) is ultrasonically cleaned using anhydrous ethanol and petroleum ether.

[0012] As a further preference, the substrate in step (1) is a steel substrate.

[0013] The beneficial effect of the present invention is that the MoS2-based composite lubricating coating with a nano-composite structure is constructed by doping with Ag metal elements. The composite lubricating coating has an extremely low friction coefficient under vacuum. When the vacuum degree is lower than 0.001Pa, the friction coefficient can be as low as 0.0071, which can meet the requirements of key mechanical moving parts of spacecraft for solid lubricating coatings. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0015] Figure 1 is a cross-sectional SEM image of the composite coating of Example 1; Figure 2 is a friction coefficient diagram of the composite coating of Example 1 under a vacuum environment; Figure 3 is a friction coefficient diagram of the composite coating of Example 2 under a vacuum environment; Figure 4 Graph showing the coefficient of friction of the composite coating of Example 3 in a vacuum environment. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0017] A method for preparing a Ag-MoS2 composite lubricating coating, the specific steps are as follows: (1) Preprocessing The 9Cr18 steel substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then dried and placed in a drying chamber for later use; (2) Pre-sputtering cleaning The steel substrate treated in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, ion etching of the substrate surface was started, Ar was introduced with a flow rate of 30 sccm, an etching pressure of 0.2 Pa, and a substrate bias of -400 V, and the steel block sample was pre-sputtered and cleaned with Ar plasma for 20 min; (3) Deposition of Ag-MoS2 composite lubricating coating Using unbalanced magnetron sputtering technology, the Ar flow rate was increased to 70 sccm, the deposition gas pressure was 0.35 Pa, the substrate bias was continuously adjusted to 0 V, and an RF power supply was applied to the MoS2 target. The sputtering power of the MoS2 target was continuously increased to 600 W. At this time, a DC power supply was applied to the pure Ag target, the deposition current was adjusted to 0.1 A, the rotating frame speed was 0.5 r / min, and the deposition time was 120 min to deposit the Ag-MoS2 composite lubricating coating.

[0018] See also Figure 1 The total thickness of the coating prepared in Example 1 is 3500 nm, in which the atomic percentage of Ag is 5 at.%.

[0019] See also Figure 2 The tribological properties of the coating prepared in Example 1 were tested using a CSM vacuum friction tester. The friction test was started when the vacuum degree was lower than 0.001 Pa. The load applied during the friction process was 3 N and the rotation speed was 500 r / min. The average friction coefficient of the coating in a vacuum environment was 0.0078. Example

[0020] A method for preparing a Ag-MoS2 composite lubricating coating, the specific steps are as follows: (1) Preprocessing The 9Cr18 steel substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then dried and placed in a drying chamber for later use; (2) Pre-sputtering cleaning The steel substrate treated in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, ion etching of the substrate surface was started, Ar was introduced with a flow rate of 30 sccm, an etching pressure of 0.2 Pa, and a substrate bias of -400 V, and the steel block sample was pre-sputtered and cleaned with Ar plasma for 25 min; (3) Deposition of Ag-MoS2 composite lubricating coating Using unbalanced magnetron sputtering technology, the Ar flow rate was increased to 70 sccm, the deposition gas pressure was 0.35 Pa, the substrate bias was continuously adjusted to 0 V, and an RF power supply was applied to the MoS2 target. The sputtering power of the MoS2 target was continuously increased to 600 W. At this time, a DC power supply was applied to the pure Ag target, the deposition current was adjusted to 0.2 A, the rotating frame speed was 0.5 r / min, and the deposition time was 120 min to deposit the Ag-MoS2 composite lubricating coating.

[0021] The total thickness of the coating prepared in Example 2 is 2500 nm, and the Ag atomic percentage is 15 at.%.

[0022] See also Figure 3 The tribological properties of the coating prepared in Example 2 were tested using a CSM vacuum friction tester. The friction test was started when the vacuum degree was lower than 0.001 Pa. The load applied during the friction process was 3 N and the rotation speed was 500 r / min. The average friction coefficient of the coating in a vacuum environment was 0.0071. Example

[0023] A method for preparing a Ag-MoS2 composite lubricating coating, the specific steps are as follows: (1) Preprocessing The 9Cr18 steel substrate was ultrasonically cleaned with anhydrous ethanol and petroleum ether for 30 min respectively, and then dried and placed in a drying chamber for later use; (2) Pre-sputtering cleaning The steel substrate treated in step (1) is placed in a vacuum chamber and evacuated to a vacuum degree of less than 0.001 Pa, ion etching of the substrate surface was started, Ar was introduced with a flow rate of 30 sccm, an etching pressure of 0.2 Pa, and a substrate bias of -400 V, and the steel block sample was pre-sputtered and cleaned with Ar plasma for 30 min; (3) Deposition of Ag-MoS2 composite lubricating coating Using unbalanced magnetron sputtering technology, the Ar flow rate was increased to 70 sccm, the deposition gas pressure was 0.35 Pa, the substrate bias was continuously adjusted to 0 V, and an RF power supply was applied to the MoS2 target. The sputtering power of the MoS2 target was continuously increased to 600 W. At this time, a DC power supply was applied to the pure Ag target, the deposition current was adjusted to 0.3 A, the rotating frame speed was 0.5 r / min, and the deposition time was 120 min to deposit the Ag-MoS2 composite lubricating coating.

[0024] The total thickness of the coating prepared in Example 3 is 1500 nm, and the Ag atomic percentage is 30 at.%.

[0025] See also Figure 4 The tribological properties of the coating prepared in the embodiment were tested using a CSM vacuum friction tester. The friction test was started when the vacuum degree was lower than 0.001 Pa. The load applied during the friction process was 3 N and the rotation speed was 500 r / min. The average friction coefficient of the coating in a vacuum environment was 0.0092.

[0026] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Ag-MoS 2 Composite lubricating coating, It is characterized in that The composite lubricating coating is composed of 5-30 at.% Ag doped MoS 2 The composite lubricating coating has a thickness of 1500 to 3500 nm.

2. The Ag-MoS according to claim 1 2 Composite lubricating coating, It is characterized in that The atomic percentage of Ag in the composite lubricating coating is 15 at.%.

3. The Ag-MoS according to claim 1 2 Composite lubricating coating, It is characterized in that The thickness of the composite lubricating coating is 2500 nm.

4. The Ag-MoS according to claim 1 2 Preparation method of composite lubricating coating, It is characterized in that The steps include: (1) Preprocessing The substrate was cleaned for 30 min and dried for later use; (2) Pre-sputtering cleaning Place the substrate obtained in step (1) into a vacuum chamber, evacuate the chamber to a vacuum degree of less than 0.001 Pa, introduce argon gas at a flow rate of 30 sccm, an etching pressure of 0.2 Pa, a substrate bias voltage of -400 V, and perform pre-sputtering cleaning for 20 to 30 min; (3) Deposition of Ag-MoS 2 Composite lubricating coating The unbalanced magnetron sputtering technology was used, the argon flow rate was increased to 70 sccm, the deposition pressure was 0.35 Pa, and the substrate bias was continuously adjusted to 0 V. 2 Applying RF power to the target material continuously increases the MoS 2 The sputtering power of the target material was increased to 600 W. At this time, a DC power supply was applied to the pure Ag target, the deposition current was adjusted to 0.1-0.3 A, the rotating frame speed was 0.5 r / min, and the deposition time was 120 min to deposit Ag-MoS 2 Composite lubricating coating.

5. The preparation method according to claim 4, It is characterized in that The pre-sputtering cleaning time in step (2) is 25 min.

6. The preparation method according to claim 4, It is characterized in that The Ag deposition current in step (3) is 0.2 A.

7. The preparation method according to claim 4, It is characterized in that The substrate in step (1) is ultrasonically cleaned using anhydrous ethanol and petroleum ether.

8. The preparation method according to claim 4, It is characterized in that The substrate in step (1) is a steel substrate.

Citation Information

Patent Citations

  • Molybdenum disulfide silver-doped vulcanized film and preparation method and application thereof

    CN112210753A

Cited By

  • Method for improving quality of magnetron sputtering molybdenum disulfide film and improving friction performance through precious metal micro-doping

    CN120006229A