A method for extending the service life of a sodium metal diaphragm prepared by electrolysis

By monitoring the electrolytic efficiency during the electrolysis preparation process of sodium metal and using sodium carbonate-sodium chloride mixture or adding sodium carbonate, the problem of frequent cleaning of the diaphragm caused by impurity bonding is solved, the use cycle of the diaphragm is extended, the production efficiency is improved and the savings are achieved. resource.

CN118727066BActive Publication Date: 2024-12-06INNER MONGOLIA MURRAY ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411223196.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

During the electrolytic preparation of sodium metal, impurities cannot fall off automatically due to the bonding of impurities on the surface of the diaphragm, resulting in frequent cleaning or replacement of the diaphragm, delaying production, and wasting manpower, financial resources and energy.

Method used

By monitoring the electrolytic efficiency during the electrolysis process, when the efficiency is less than 90%, switch the electrolyte to a sodium carbonate-sodium chloride mixture or add sodium carbonate to produce carbon dioxide gas, causing slight vibration of the membrane, peeling off the clogged substance, and making it smaller by buoyancy The volume blockage floats for fishing.

Benefits of technology

It effectively extends the use cycle of the diaphragm, saves manpower, financial resources and energy, reduces environmental pollution, and improves production efficiency and benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of sodium metal preparation, and discloses a method for extending the service life of a sodium metal diaphragm prepared by electrolysis. The method comprises the following steps: continuously introducing sodium chloride into the molten electrolyte of an electrolytic cell for electrolysis, maintaining the mass fraction of sodium chloride in the molten electrolyte constant, monitoring the electrolysis efficiency, and when the electrolysis efficiency is less than 90%, switching the sodium chloride to a sodium carbonate-sodium chloride mixture; or, adding sodium carbonate to the electrolytic cell; continuing electrolysis until the electrolysis efficiency is greater than 90%, switching the sodium carbonate-sodium chloride mixture to sodium chloride; removing impurities on the surface. The present invention adopts two different methods to add sodium carbonate to the electrolytic cell, effectively extending the service life of the diaphragm, and realizing the replacement of the diaphragm every 6 months. At the same time, due to the reduced frequency of cleaning and replacing the diaphragm, a large amount of manpower, financial resources and energy are saved, pollution to the environment is reduced, and production efficiency and benefits are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallic sodium preparation, and in particular to a method for prolonging the service life of a metallic sodium diaphragm prepared by electrolysis. Background Art

[0002] The current method of producing metallic sodium is to electrolyze molten sodium chloride. In order to lower the melting point of sodium chloride and save energy, the electrolyte is usually a ternary electrolyte, namely sodium chloride (NaCl), calcium chloride (CaCl 2 ) and barium chloride (BaCl 2 ). During the electrolytic preparation of metallic sodium, a diaphragm is placed between the anode and the cathode. The main function of the diaphragm is to isolate the chlorine gas produced by the anode and the liquid metallic sodium produced by the cathode during the electrolysis process, and to prevent the two from contacting and causing a reverse reaction as much as possible.

[0003] The anodes used in the electrolytic preparation of metallic sodium are mostly graphite electrodes. However, during the electrolysis process, due to the combined effects of chlorine corrosion and high temperature, graphite will peel off and produce graphite fragments of different sizes; at the same time, the raw material sodium chloride in the electrolysis process contains metal impurities such as iron and potassium. The above two types of impurities from different sources will adhere to the surface of the diaphragm as the molten electrolyte flows during the electrolysis process. As the electrolysis proceeds, the above impurities continue to accumulate and adhere on the surface of the diaphragm and cannot fall off automatically, eventually leading to diaphragm blockage, affecting the flow of electrolyte between the anode and cathode, increasing resistance, and thus reducing electrolysis efficiency. Therefore, production personnel are required to remove the diaphragm from the electrolytic cell for cleaning or replacing it with a new one. However, since the process of removing and replacing the diaphragm will delay a lot of production time, while delaying production, it will also bring a lot of waste of manpower, financial resources and energy. Summary of the invention

[0004] The purpose of the present invention is to provide a method for extending the service life of a diaphragm for preparing metallic sodium by electrolysis, so as to solve the problem that impurities adhere to the surface of the diaphragm and cannot fall off automatically, and the diaphragm needs to be frequently cleaned or replaced, resulting in production delays and waste of manpower, financial resources and energy.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for extending the service life of a sodium metal diaphragm prepared by electrolysis, comprising the following steps:

[0007] (1) continuously introducing solid sodium chloride into the molten electrolyte of the electrolytic cell for electrolysis, and maintaining the mass fraction of sodium chloride in the molten electrolyte constant; monitoring the electrolysis efficiency during the electrolysis process, and when the electrolysis efficiency is less than 90%, switching the introduced raw material from solid sodium chloride to a sodium carbonate-sodium chloride mixture;

[0008] (2) The electrolysis is continued until the electrolysis efficiency is ≥90%, and then the raw material introduced is switched from a sodium carbonate-sodium chloride mixture to solid sodium chloride to remove impurities on the surface;

[0009] Alternatively, the method comprises the following steps:

[0010] Step 1, continuously introducing solid sodium chloride into the molten electrolyte of the electrolytic cell for electrolysis, and maintaining the mass fraction of sodium chloride in the molten electrolyte constant; monitoring the electrolysis efficiency during the electrolysis process, and when the electrolysis efficiency is less than 90%, continuously introducing solid sodium chloride into the electrolytic cell, and adding sodium carbonate into the electrolytic cell;

[0011] Step 2: Continue electrolysis until the electrolysis efficiency is ≥ 90% to remove impurities on the surface.

[0012] Preferably, in the method, the molten electrolyte in step (1) and step 1 comprises the following raw materials by mass fraction: 35-40% sodium chloride, 40-45% calcium chloride, and 20-25% barium chloride.

[0013] Preferably, in the method, the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (1) is 0.1-30%.

[0014] Preferably, in the method, when sodium carbonate is added to the electrolytic cell in step 1, the total mass of the added sodium carbonate is 0.1-20% of the mass of the molten electrolyte.

[0015] Preferably, in the method, when sodium carbonate is added to the electrolytic cell in step 1, the sodium carbonate is added all at once or in batches.

[0016] Preferably, in the method, the batch addition is specifically: adding in 2 to 10 batches on average, and the interval time between each batch is 25 to 120 minutes.

[0017] Preferably, in the method, the melting point of the scooping material used to remove surface impurities in step (2) and step 2 is greater than 660°C.

[0018] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention adds sodium carbonate to the electrolytic cell in two different ways: "switching sodium chloride to a sodium chloride-sodium carbonate mixture" or "adding sodium carbonate to the electrolytic cell". Sodium carbonate generates carbon dioxide (CO 2) gas, which will cause slight vibrations in the diaphragm during the gas formation process. The vibrations are transmitted to the diaphragm through the molten electrolyte, causing the blockage to fall off the diaphragm, thus successfully peeling off the blockage on the diaphragm. Since the density of the blockage is higher than that of the molten electrolyte, the blockage will sink to the bottom of the electrolytic cell. At the same time, sodium carbonate produces CO during electrolysis. 2 Tiny bubbles will adhere to the surface of small-volume blockages, increase the buoyancy of small-volume blockages, and make them float on the surface of molten electrolyte. At this time, small-volume blockages on the surface of electrolyte can be picked up by tools; large-volume blockages will not affect the mass transfer of the diaphragm because they have sunk to the bottom. By adopting the above method, the service life of the diaphragm can be effectively extended, saving a lot of manpower, financial resources and energy, reducing pollution to the environment, and improving production efficiency and benefits. DETAILED DESCRIPTION

[0020] The present invention provides a method for extending the service life of a sodium metal diaphragm prepared by electrolysis, comprising the following steps:

[0021] (1) continuously introducing solid sodium chloride into the molten electrolyte of the electrolytic cell for electrolysis, and maintaining the mass fraction of sodium chloride in the molten electrolyte constant; monitoring the electrolysis efficiency during the electrolysis process, and when the electrolysis efficiency is less than 90%, switching the introduced raw material from solid sodium chloride to a sodium carbonate-sodium chloride mixture;

[0022] (2) The electrolysis is continued until the electrolysis efficiency is ≥90%, and then the raw material introduced is switched from a sodium carbonate-sodium chloride mixture to solid sodium chloride to remove impurities on the surface;

[0023] Alternatively, the method comprises the following steps:

[0024] Step 1, continuously introducing solid sodium chloride into the molten electrolyte of the electrolytic cell for electrolysis, and maintaining the mass fraction of sodium chloride in the molten electrolyte constant; monitoring the electrolysis efficiency during the electrolysis process, and when the electrolysis efficiency is less than 90%, continuously introducing solid sodium chloride into the electrolytic cell, and adding sodium carbonate into the electrolytic cell;

[0025] Step 2: Continue electrolysis until the electrolysis efficiency is ≥ 90% to remove impurities on the surface.

[0026] In the present invention, step (1) and step 1 further independently include a slotting process before continuously introducing solid sodium chloride into the molten electrolyte in the electrolytic cell for electrolysis.

[0027] In the present invention, the groove opening treatment is performed using the molten electrolyte.

[0028] In the present invention, the role of the grooving process is to reduce the melting point of the sodium chloride solid and save energy.

[0029] In the present invention, the molten electrolyte in step (1) and step 1 preferably comprises the following raw materials by mass fraction: 35-40% sodium chloride (NaCl), 10% calcium chloride (CaCl 2 ) 40~45%, barium chloride (BaCl 2 ) 20~25%, further preferably comprising: sodium chloride 38~40%, calcium chloride 40~42%, barium chloride 20~22%, more preferably comprising: sodium chloride 40%, calcium chloride 40%, barium chloride 20%.

[0030] In the present invention, the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (1) is preferably 0.1-30%, more preferably 3-20%, and more preferably 20%.

[0031] In the present invention, the feeding rate of the sodium chloride solid and the mass of the molten electrolyte in the electrolytic cell are not limited, and schemes well known to those skilled in the art can be adopted.

[0032] In the present invention, when sodium carbonate is added to the electrolytic cell in step 1, the total mass of the added sodium carbonate is preferably 0.1-20% of the mass of the molten electrolyte, more preferably 3-10%, and more preferably 10%.

[0033] In the present invention, when adding sodium carbonate to the electrolytic cell in step 1, the sodium carbonate is preferably added all at once or in batches, and more preferably added all at once.

[0034] In the present invention, the batchwise addition is preferably: added in 2 to 10 batches on average, more preferably 6 to 10 batches, more preferably 6 batches; the interval time between each batch is preferably 25 to 120 min, more preferably 25 to 40 min, more preferably 40 min.

[0035] In the present invention, the melting point of the scooping material used to remove surface impurities in step (2) and step 2 is preferably greater than 660°C.

[0036] In the present invention, the material of the scooping material is not limited, and a material with a melting point greater than 660° C. known to those skilled in the art can be used. Optionally, the scooping material is preferably stainless steel, copper, nickel, tungsten-iron alloy or manganese-iron alloy.

[0037] In the present invention, the scooped material can be selected as a round hole or a square hole. The diameter of the round hole is preferably 1-2 mm, more preferably 1-1.5 mm, and more preferably 1 mm; the side length of the square hole is preferably 1-1.5 mm, more preferably 1-1.2 mm, and more preferably 1 mm.

[0038] In the present invention, the calculation formula of the electrolysis efficiency in step (1), step (2), step 1 and step 2 is as shown in formula 1:

[0039] Formula 1;

[0040] In formula 1, r is the electrolysis efficiency, unit: %; v t is the actual output of metallic sodium per 10 minutes, unit: kg / 10min; v 0 The theoretical output of metallic sodium per 10 minutes, unit: kg / 10min.

[0041] There are usually two methods for monitoring electrolysis efficiency: the first is to reflect the electrolysis efficiency by measuring the change in the furnace temperature of the electrolytic cell. Because the current is constant during the electrolysis process, when the electrolysis efficiency decreases, the heat generated by the current will increase, and the furnace temperature of the electrolytic cell will increase significantly. The second method is to determine it through the change in the output of metallic sodium. When the electrolysis efficiency decreases, the output of metallic sodium will decrease accordingly. Since temperature monitoring is difficult and less safe, the second method is usually used, that is, monitoring the electrolysis efficiency through the output of metallic sodium.

[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Example 1

[0044] This embodiment provides a method for extending the service life of a sodium metal diaphragm prepared by electrolysis, comprising the following steps:

[0045] (1) Add 500 kg of ternary electrolyte (NaCl:CaCl 2 :BaCl 2 The mass fraction of =40%:40%:20%) is used for slotting;

[0046] (2) After the slotting treatment, sodium chloride solid is continuously introduced into the ternary electrolyte of the electrolytic cell for electrolysis. The feeding rate of sodium chloride solid is 120 kg / h, and the mass fraction of NaCl in the ternary electrolyte is kept constant. Under the above conditions, v 0 is 7.79kg; monitor the electrolysis efficiency during the electrolysis process. When the electrolysis efficiency in the electrolytic cell drops to 85% (at this time v tWhen the feeding rate is 6.62 kg / 10 min), the pure sodium chloride solid introduced into the feeding system is switched to a sodium carbonate-sodium chloride mixture containing 0.1 wt% sodium carbonate, and the feeding rate of the sodium carbonate-sodium chloride mixture is maintained at 120 kg / h;

[0047] (3) After 320 min of continuous electrolysis, the efficiency recovered to 97.5%, i.e., v t When the concentration of sodium carbonate and sodium chloride is restored to 7.6 kg / 10 min, the sodium carbonate-sodium chloride mixture is stopped and the raw material in the feeding system is switched to pure sodium chloride solid; a stainless steel scoop net with a square hole side length of 1 mm is used to scoop out the black material floating on the surface of the electrolytic cell. According to calculations, the total amount of sodium carbonate added in the above process is 0.48 kg.

[0048] Example 2

[0049] The difference between Example 2 and Example 1 is that the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (2) is 3 wt %; the continuous electrolysis time in step (3) is 180 min, the total amount of sodium carbonate is 10.8 kg, and the other parameter conditions are the same as those in Example 1.

[0050] Example 3

[0051] The difference between Example 3 and Example 1 is that the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (2) is 10 wt %; the continuous electrolysis time in step (3) is 150 min, the total amount of sodium carbonate is 30 kg, and the other parameter conditions are the same as those in Example 1.

[0052] Example 4

[0053] The difference between Example 4 and Example 1 is that the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (2) is 20 wt %; the continuous electrolysis time in step (3) is 140 min, the total amount of sodium carbonate is 55.92 kg, and the other parameter conditions are the same as those in Example 1.

[0054] Example 5

[0055] The difference between Example 5 and Example 1 is that the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (2) is 30 wt %; the continuous electrolysis time in step (3) is 130 min, the total amount of sodium carbonate is 77.4 kg, and the other parameter conditions are the same as those in Example 1.

[0056] It can be seen from Examples 1 to 5 that as the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture increases, the electrolysis efficiency recovery time is significantly shortened; however, when the sodium carbonate content increases from 20% to 30%, the decrease in the electrolysis efficiency recovery time is significantly reduced. Therefore, further increasing the sodium carbonate content does not significantly shorten the electrolysis efficiency recovery time.

[0057] Example 6

[0058] This embodiment provides a method for extending the service life of a sodium metal diaphragm prepared by electrolysis, comprising the following steps:

[0059] (1) Add 500 kg of ternary electrolyte (NaCl:CaCl 2 :BaCl 2 The mass fraction of =40%:40%:20%) is used for slotting;

[0060] (2) After the slotting treatment, sodium chloride solid is continuously introduced into the ternary electrolyte of the electrolytic cell for electrolysis. The feeding rate of sodium chloride solid is 120 kg / h, and the mass fraction of NaCl in the ternary electrolyte is kept constant. Under the above conditions, v 0 is 7.79kg; the electrolysis efficiency is monitored during the electrolysis process. When the electrolysis efficiency in the electrolytic cell drops to 89% (at this time v t When the mass of sodium carbonate is 0.1% of the mass of the molten electrolyte, 0.5 kg of sodium carbonate is added to the electrolytic cell at one time; the feeding rate of sodium chloride solid is maintained at 120 kg / h;

[0061] (3) After 260 min of continuous electrolysis, the efficiency recovered to 92%, that is, v t Restore to 7.17kg / 10min; use a pure copper scoop net with a round hole of 1mm in diameter to scoop out the black material floating on the inner surface of the electrolytic cell.

[0062] Example 7

[0063] The difference between Example 7 and Example 6 is that in step (2), when the electrolysis efficiency in the electrolytic cell drops to 86% (at this time v t The mass of sodium carbonate input at one time is 15 kg, and the mass of sodium carbonate is 3% of the mass of the molten electrolyte; the electrolysis time in step (3) is 230 min, and the efficiency is restored to 95%, that is, v t The pressure was restored to 7.4 kg / 10 min, and other parameters were the same as those in Example 6.

[0064] Example 8

[0065] The difference between Example 8 and Example 6 is that in step (2), when the electrolysis efficiency in the electrolytic cell drops to 85% (at this time v t The mass of sodium carbonate input at one time is 50 kg, and the mass of sodium carbonate is 10% of the mass of the molten electrolyte. The electrolysis time in step (3) is 210 min, and the efficiency is restored to 97.5%, that is, v tThe pressure was restored to 7.6 kg / 10 min, and other parameters were the same as those in Example 6.

[0066] Example 9

[0067] The difference between Example 9 and Example 6 is that in step (2), when the electrolysis efficiency in the electrolytic cell drops to 85% (at this time v t The mass of sodium carbonate input at one time is 80 kg, and the mass of sodium carbonate is 16% of the mass of the molten electrolyte. The electrolysis time in step (3) is 200 min, and the efficiency is restored to 97.5%, that is, v t The pressure was restored to 7.6 kg / 10 min, and other parameters were the same as those in Example 6.

[0068] As can be seen from Examples 6 to 9, when sodium carbonate is directly added to the electrolytic cell, the time for electrolysis efficiency recovery gradually shortens as the amount of sodium carbonate used increases; however, when the amount of sodium carbonate increases from 50 kg to 80 kg, the decrease in the time taken for electrolysis efficiency recovery becomes significantly smaller. Therefore, continuing to increase the amount of sodium carbonate used does not significantly shorten the time for electrolysis efficiency recovery.

[0069] Compared with the solution of adding sodium chloride-sodium carbonate mixture in Examples 1 to 5, Examples 6 to 9 adopt a method of directly adding sodium carbonate at one time. Although the time for electrolysis efficiency recovery is slightly longer, its advantage is that there is no need to pre-mix sodium carbonate and sodium chloride solids, which simplifies the operation procedure and avoids the possible extension of electrolysis efficiency recovery time or waste of sodium carbonate due to uneven mixing.

[0070] Example 10

[0071] This embodiment provides a method for extending the service life of a sodium metal diaphragm prepared by electrolysis, comprising the following steps:

[0072] (1) Add 500 kg of ternary electrolyte (NaCl:CaCl 2 :BaCl 2 The mass fraction of =40%:40%:20%) is used for slotting;

[0073] (2) After the slotting treatment, sodium chloride solid is continuously introduced into the ternary electrolyte of the electrolytic cell for electrolysis. The feeding rate of sodium chloride solid is 120 kg / h, and the mass fraction of NaCl in the ternary electrolyte is kept constant. Under the above conditions, v 0 is 7.79kg; the electrolysis efficiency is monitored during the electrolysis process. When the electrolysis efficiency in the electrolytic cell drops to 89% (at this time v tWhen the mass of sodium carbonate is 6.94 kg / 10 min), sodium carbonate is added to the electrolytic cell in two times, with an interval of 120 min. The mass of each addition is 0.25 kg, and the total amount of sodium carbonate is 0.1% of the mass of the molten electrolyte. The feeding rate of sodium chloride solid is maintained at 120 kg / h.

[0074] (3) After 240 min of continuous electrolysis, the efficiency recovered to 91%, that is, v t Restore to 7.09kg / 10min; use a pure copper scoop net with a round hole of 2mm in diameter to scoop out the black material floating on the inner surface of the electrolytic cell.

[0075] Embodiment 11

[0076] The difference between Example 11 and Example 10 is that in step (2), when the electrolysis efficiency in the electrolytic cell drops to 86% (at this time v t The amount of sodium carbonate added was 6.7 kg / 10 min, and the sodium carbonate was added in 6 times, with an interval of 40 min. The mass of each addition was 2.5 kg, and the total amount of sodium carbonate was 3% of the mass of the molten electrolyte. The electrolysis time of step (3) was 240 min, and the efficiency was restored to 95%, that is, v t Restored to 7.4 kg / 10 min, other parameter conditions are the same as Example 10.

[0077] Example 12

[0078] The difference between Example 12 and Example 10 is that in step (2), when the electrolysis efficiency in the electrolytic cell drops to 85% (at this time v t The amount of sodium carbonate added was 6.62 kg / 10 min), and sodium carbonate was added in 10 times, with a sodium carbonate addition every 25 min. The mass of each addition was 5 kg, and the total amount of sodium carbonate used was 10% of the mass of the molten electrolyte. The electrolysis time of step (3) was 250 min, and the efficiency was restored to 97.5%, that is, v t Restored to 7.6 kg / 10 min, other parameter conditions are the same as Example 10.

[0079] In Examples 1 to 12, the carbon dioxide generated during the electrolysis process is separated from the chlorine during the chlorine collection and liquefaction process, and is directly discharged into the atmosphere or made into dry ice after being monitored as qualified.

[0080] In summary, an electrolytic cell with a molten electrolyte mass of 500 kg needs to replace the diaphragm every 3 months without using the method described in the present invention. Each time the diaphragm is replaced, the shutdown time is 10 days. In order to maintain the temperature in the electrolytic cell and prevent the molten electrolyte from solidifying and causing the electrolytic cell to be scrapped, the electrolytic cell needs to be powered continuously, thus causing a large amount of electricity, manpower, and material resources. After being processed by the schemes of Examples 1 to 12, the service life of the diaphragm is significantly extended, and the diaphragm can be replaced every 6 months, and the service life is doubled; at the same time, due to the reduced frequency of cleaning and replacing the diaphragm, a large amount of energy, manpower, material resources and financial resources are saved in the process of metallic sodium production.

[0081] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for extending the service life of a sodium metal diaphragm prepared by electrolysis, characterized in that: The following steps are involved: (1) continuously introducing solid sodium chloride into the molten electrolyte of the electrolytic cell for electrolysis, and maintaining the mass fraction of sodium chloride in the molten electrolyte constant; monitoring the electrolysis efficiency during the electrolysis process, and when the electrolysis efficiency is less than 90%, switching the introduced raw material from solid sodium chloride to a sodium carbonate-sodium chloride mixture; (2) The electrolysis is continued until the electrolysis efficiency is ≥90%, and then the raw material introduced is switched from a sodium carbonate-sodium chloride mixture to solid sodium chloride to remove impurities on the surface; Wherein, the mass fraction of sodium carbonate in the sodium carbonate-sodium chloride mixture in step (1) is 0.1-30%; Alternatively, the method comprises the following steps: Step 1, continuously introducing solid sodium chloride into the molten electrolyte of the electrolytic cell for electrolysis, and maintaining the mass fraction of sodium chloride in the molten electrolyte constant; monitoring the electrolysis efficiency during the electrolysis process, and when the electrolysis efficiency is less than 90%, continuously introducing solid sodium chloride into the electrolytic cell, and adding sodium carbonate into the electrolytic cell; Step 2: Continue electrolysis until the electrolysis efficiency is ≥ 90%, and remove the impurities on the surface; Wherein, when adding sodium carbonate to the electrolytic cell in step 1, the total mass of the added sodium carbonate is 0.1-20% of the mass of the molten electrolyte.

2. The method according to claim 1, characterized in that: The molten electrolyte in step (1) and step 1 comprises the following raw materials by mass fraction: 35-40% sodium chloride, 40-45% calcium chloride, and 20-25% barium chloride.

3. The method according to claim 1 or 2, characterized in that: When adding sodium carbonate into the electrolytic cell in step 1, the sodium carbonate is added at once or in batches.

4. The method according to claim 3, characterized in that The batch addition specifically includes: adding in 2 to 10 batches on average, and the interval time between each batch is 25 to 120 minutes.

5. The method according to claim 1, characterized in that The melting point of the scooping material used to remove surface impurities in step (2) and step 2 is greater than 660°C.