Method for electroplating zinc-nickel alloy on inner pipe fitting of steel shock pad

Through degreasing, activation, zinc-nickel electroplating and passivation treatment, combined with optimized zinc-nickel alloy plating solution components and conditions, the problem of easy corrosion of the inner tube of the steel shock absorber is solved, and high corrosion resistance and hardness are achieved and wear resistance, and reduces the toxicity of the electroplating solution, and has environmental protection characteristics.

CN118727083APending Publication Date: 2024-10-01NINGBO TUOPU GROUP CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410883523.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The inner tube of the steel shock-absorbing pad is prone to corrosion, which affects its aesthetics, service life and load-bearing capacity. Moreover, the existing zinc-nickel alloy electroplating method has the problem of high toxicity of the electroplating solution.

Method used

The methods of degreasing, activation, zinc-nickel electroplating, activation and passivation are used, and the electroplating zinc-nickel alloy plating solution components are zinc chloride, nickel chloride, ammonium chloride, triethanolamine and auxiliary brightener to control the electroplating conditions. Such as temperature, pH value and cathode current density, conduct pre-electrolysis to remove heavy metal impurities, and optimize plating solution configuration and maintenance.

Benefits of technology

It significantly improves the corrosion resistance, hardness and wear resistance of the pipe fittings inside the steel shock absorber, reduces hydrogen embrittlement, and the electroplating solution has low toxicity, which is beneficial to environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727083A_ABST
    Figure CN118727083A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of steel part surface processing, in particular to a method for electroplating zinc-nickel alloy on a steel shock pad inner pipe fitting, which comprises the following steps of: removing oil from the steel shock pad inner pipe fitting, and washing with flowing water after oil removal; after activating or weakly etching the pipe fitting in the steel shock pad, flushing with flowing water; electroplating zinc and nickel on the pipe fitting in the steel shock pad, washing with flowing water, and blow-drying; the steel part is placed in a 0.5%-1.5% sulfuric acid solution to be activated for 5 s to 15 s, and flowing water is used for flushing; passivating the pipe fitting in the steel shock pad, washing with flowing water, and drying by blowing; an electroplating solution for electroplating zinc and nickel comprises the following components: 50g / L-65g / L of zinc chloride, 140g / L of nickel chloride, 220g / L-230g / L of ammonium chloride, 25g / L of triethanolamine, ammonia water, 50ml / L of a cylinder opening agent and 10ml / L of an auxiliary brightener; the electroplating solution can effectively electroplate zinc and nickel on the inner pipe fitting of the steel shock pad so as to solve the problem that the inner pipe of the steel shock pad is corroded, and has the environment-friendly characteristics that the electroplating solution is low in toxicity, and environment protection is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface processing of steel parts, in particular to a method for electroplating zinc-nickel alloy on inner pipe parts of steel shock-absorbing pads. Background Art

[0002] Shock absorber is an important automotive accessory that can play multiple roles in reducing vibration, protecting the vehicle and passengers during driving.

[0003] The material of the inner tube of the shock absorber is also an important factor affecting its working effect. Generally speaking, the inner tube of the shock absorber adopts rigid materials with high strength, high hardness and high elasticity, such as steel, titanium alloy, etc., in order to provide good shock absorption effect. However, the characteristics of titanium alloy such as high processing difficulty, high price, poor wear resistance, difficult welding, easy oxidation, etc., result in the disadvantages of relatively high processing and production costs, which also limits its application scope. As an important engineering material, steel has the advantages of high strength, weldability, machinability, good wear resistance and good economy, but it also has the disadvantage of being easy to corrode. This will not only affect its aesthetics and service life, but also reduce its bearing capacity and threaten the safety of the project. Therefore, it is particularly important to carry out anti-corrosion and anti-rust treatment on steel structures.

[0004] Electroplated zinc-nickel alloy not only has excellent corrosion resistance, but also has good cost performance. Electroplated zinc-nickel alloy has good corrosion resistance and low hydrogen embrittlement, which greatly improves the surface quality. The corrosion resistance of electroplated zinc-nickel alloy is reflected in the fact that the stable potential of zinc-nickel alloy is more negative than that of steel. It is an anodic coating relative to steel and plays an electrochemical protective role. However, its potential is more positive than that of zinc coating, and its corrosion electromotive force is smaller than that of zinc coating, so its corrosion current is small, so its corrosion resistance is higher than that of zinc coating.

[0005] The prior art discloses a variety of methods for electroplating zinc-nickel alloys, such as a method for electroplating zinc-nickel alloys on steel parts proposed in the Chinese invention patent application with publication number CN104005063A. Therefore, based on the prior art, improvements are made to improve corrosion resistance, hardness and wear resistance, as well as the low toxicity of the electroplating solution, which is beneficial to environmental protection and will be practical. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a method for electroplating zinc-nickel alloy on the inner pipe of a steel shock-absorbing pad effectively to solve the problem of corrosion of the inner pipe of the steel shock-absorbing pad, and has the environmental protection characteristics of low toxicity of the plating solution and being beneficial to environmental protection.

[0007] A method for electroplating zinc-nickel alloy on inner pipes of steel shock-absorbing pads of the present invention:

[0008] 1) Degrease the inner pipes of the steel shock-absorbing pads and rinse them with running water after degreasing;

[0009] 2) After activating or weakly etching the inner pipe of the steel shock-absorbing pad, rinse it with running water;

[0010] 3) Electroplating zinc-nickel on the inner pipes of the steel shock-absorbing pads, rinsing with running water, and drying;

[0011] 4) Activate the steel parts in 0.5%-1.5% sulfuric acid solution for 5s-15s, and rinse with running water;

[0012] 5) Then passivate the inner pipes of the steel shock-absorbing pads, rinse with running water, and blow dry; the plating solution components of zinc-nickel electroplating are: zinc chloride 50g / L~65g / L, nickel chloride 140g / L, ammonium chloride 220g / L~230g / L, triethanolamine (content 80%~85%) 25g / L, ammonia water, cylinder opener 50ml / L, auxiliary brightener 10ml / L.

[0013] Preferably, the conditions for electroplating zinc and nickel are: temperature: 30°C to 40°C, pH value: 5.35 to 5.60, cathode current density DK: 2A / dm2 to 4A / dm2, nickel anode area / zinc anode area 1:2.0 to 1:2.5.

[0014] Preferably, the electroplating solution for zinc-nickel electroplating is prepared as follows:

[0015] 1) First add 1 / 2 volume of water to the electroplating tank, heat it to 50℃~60℃, then add ammonium chloride, stirring while adding to accelerate dissolution. After the ammonium chloride is completely dissolved, add nickel chloride, zinc chloride, triethanolamine, tank opening agent and auxiliary brightener in sequence;

[0016] 2) After all components are dissolved, filter the plating solution with a filter to remove particulate impurities;

[0017] 3) Add water to the specified volume, measure the pH value and adjust it to 5.35-5.40 with aqueous ammonia.

[0018] Preferably, the newly prepared plating solution is pre-electrolyzed to remove heavy metal impurity elements contained in chemical raw materials before being put into production; the heavy metal impurity elements are copper, lead, antimony and the like.

[0019] Preferably, the pre-electrolysis is carried out at a cathode current density of 0.3A / dm2 to 0.4A / dm2, and the pre-electrolysis time is 1 hour to 100 hours, until the coating reaches a silvery white color.

[0020] Preferably, the maintenance method of the electroplating solution for zinc-nickel electroplating is:

[0021] A. pH value control;

[0022] B. Control of Zn / Ni ratio;

[0023] C. Temperature control:

[0024] D. Control of cathode current density:

[0025] E. Addition of cylinder filling agent:

[0026] F. The appropriate ammonium chloride content of the plating solution is 220g / L~230g / L. If the content is too low, the coating will be gray. Analyze and replenish regularly.

[0027] Preferably, maintenance A, pH value control: control the pH value within the range of 5.35 to 5.65, and use hydrochloric acid to adjust the pH to lower it; when the pH of the zinc-nickel electroplating solution is ≤5.2, the coating is pitted; when the pH is ≤5.3, the coating has poor brightness; as the electroplating proceeds, the pH value of the plating solution slowly rises and is adjusted with hydrochloric acid.

[0028] Preferably, maintenance B, Zn / Ni ratio control: the ratio of zinc to nickel content in the zinc-nickel plating solution is controlled at 0.7-0.9; the ratio of zinc content to nickel content in the plating solution (Zn / Ni ratio) is not only the main parameter that determines the nickel content of the coating, but also has a significant impact on the appearance of the coating, and must be strictly controlled; the appropriate Zn / Ni ratio of the plating solution is preferably controlled within the range of 0.7-0.9. If the Zn / Ni ratio is too high (≥1.0), the coating will be gray when the bath temperature is low (≤35°C) and the cathode current density is low (≤1.5A / dm2); on the contrary, if the Zn / Ni ratio is too low (≤0.5), the nickel content of the coating may exceed 15%, which is no longer beneficial to improving the corrosion resistance of the coating, and the brittleness increases.

[0029] Preferably, the Zn / Ni ratio in the zinc-nickel electroplating solution is detected; the area ratio of the zinc anode to the nickel anode is adjusted according to the detection result and the change trend; the Zn / Ni ratio of the plating solution can be determined by chemical analysis or other simple methods.

[0030] Preferably, in step 5), the passivation treatment of the inner pipe of the steel shock-absorbing pad is specifically carried out under the neutralization conditions of the following components: potassium sodium tartrate 2% to 5%, sodium chloride 5% to 10%, sodium nitrate 10% to 20%, chromium nitrate 10% to 18%, sulfuric acid 0.5% to 1%, sodium fluorosilicate 1.5% to 2.5%, nitric acid 4% to 7%, hydrochloric acid 0.5% to 1%, cobalt chloride 1.5% to 2.5%, water balance; the passivation conditions are: temperature: 30°C to 40°C, time: 30min to 35min. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the axonometric structure of the inner pipe of the steel shock-absorbing pad of the present invention;

[0032] Figure 2 It is a schematic cross-sectional view of the inner pipe of the steel shock-absorbing pad of the present invention. DETAILED DESCRIPTION

[0033] In order to facilitate understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0034] Example 1

[0035] A method for electroplating zinc-nickel alloy on inner pipes of steel shock-absorbing pads is as follows:

[0036] 1) Degrease the inner pipes of the steel shock-absorbing pads and rinse them with running water after degreasing;

[0037] 2) After activating or weakly etching the inner pipe of the steel shock-absorbing pad, rinse it with running water;

[0038] 3) Electroplating zinc-nickel on the inner pipes of the steel shock-absorbing pads, rinsing with running water, and drying;

[0039] 4) Activate the steel parts in 0.5%-1.5% sulfuric acid solution for 5s-15s, and rinse with running water;

[0040] 5) Then passivate the inner pipes of the steel shock-absorbing pads, rinse with running water, and blow dry.

[0041] (1) In the above method, in step 1), the degreasing of the inner pipe of the steel shock-absorbing pad is chemical degreasing, specifically, the degreasing is carried out under the following component solution and conditions. Specifically, the degreasing is carried out under the following component solution and conditions: the chemical degreasing solution is 60g / L to 80g / L of sodium hydroxide, 30g / L to 50g / L of disodium phosphate, 30g / L to 50g / L of sodium carbonate, 10g / L to 30g / L of sodium silicate, and the remainder is water. The chemical degreasing conditions are: temperature: 75℃ to 95℃, time: 5min to 15min.

[0042] (2) In the above method, the weak etching of the inner pipe of the steel shock-absorbing pad in step 2) is specifically: placing it in a 3% to 5% hydrochloric acid solution at room temperature (25° C. to 35° C.) for 8 seconds to 11 seconds.

[0043] (3) In the above method, in step 3), the steel inner pipe of the shock absorbing pad is electroplated in a plating solution having the following components:

[0044] a. Process parameters

[0045] The specific components are: zinc chloride 50g / L~65g / L, nickel chloride 140g / L, ammonium chloride 220g / L~230g / L, triethanolamine (content 80%~85%) 25g / L, ammonia water (appropriate amount), cylinder opening agent 50ml / L, auxiliary brightener 10ml / L;

[0046] The specific conditions are: temperature: 35℃~38℃, pH value: 5.35~5.60, cathode current density DK: 2A / dm2~4A / dm2, nickel anode area / zinc anode area 1:2.0~1:2.5, zinc / nickel content ratio: 0.7~0.9, stirring method: cathode movement, filtration: continuous or intermittent filtration.

[0047] b. Configuration method

[0048] 1. First add 1 / 2 volume of water to the electroplating tank, heat it to 50℃~60℃, then add ammonium chloride, stirring while adding to accelerate dissolution. After the ammonium chloride is completely dissolved, add nickel chloride, zinc chloride, triethanolamine, tank opener and auxiliary brightener in sequence.

[0049] 2. After all components are dissolved, filter the plating solution with a filter to remove particulate impurities.

[0050] 3. Add water to the specified volume. Measure the pH value and adjust it to 5.35-5.40 with ammonia water.

[0051] 4. Before the newly prepared plating solution is put into production, it must be pre-electrolyzed to remove heavy metal impurities such as copper, lead, and antimony contained in the chemical raw materials. The pre-electrolysis is carried out at a cathode current density of 0.3A / dm2 to 0.4A / dm2, and the pre-electrolysis time is generally several hours to dozens of hours, until the coating reaches a silvery white color.

[0052] c. Electroplating tank maintenance

[0053] pH control: The appropriate pH value of the plating solution is in the range of 5.35 to 5.65. When pH is ≤5.2, the coating is pitted; when pH is ≤5.3, the coating has poor brightness. As the electroplating progresses, the pH value of the plating solution rises slowly and is adjusted with hydrochloric acid.

[0054] Control of Zn / Ni ratio: The ratio of zinc content to nickel content in the plating solution (Zn / Ni ratio) is not only the main parameter that determines the nickel content of the coating, but also has a significant impact on the appearance of the coating, and must be strictly controlled. The appropriate Zn / Ni ratio of the plating solution is preferably controlled within the range of 0.7 to 0.9. When the Zn / Ni ratio is too high (≥1.0), the coating will be gray when the bath temperature is low (≤35°C) and the cathode current density is low (≤1.5A / dm2). On the contrary, when the Zn / Ni ratio is too low (≤0.5), the nickel content of the coating may exceed 15%, which is no longer beneficial to improving the corrosion resistance of the coating, but increases brittleness. The Zn / Ni ratio of the plating solution can be determined by chemical analysis or other simple methods. Adjust the area ratio of the zinc anode to the nickel anode in a timely manner according to the measurement results and the trend of change.

[0055] Temperature control: The operating temperature of this process is relatively wide (30℃~40℃). Except for roller plating and situations where the shape of the plated parts is too complicated, the electroplating operating temperature is generally selected to be 35℃~38℃.

[0056] Control of cathode current density: The choice of cathode current density depends on the shape of the plated piece. The general principle is to use a larger current density while ensuring the quality of the coating, increase the coating deposition speed, and shorten the electroplating time. Rack plating generally chooses 2A / dm2~4A / dm2, and barrel plating is about 1.0A / dm2.

[0057] Addition of replenishing agent: The consumption of replenishing agent is 100ml / KAhr. Excessive replenishing agent will cause unevenness and airflow stripes in the high current area of ​​the plated part. On the contrary, insufficient replenishing agent will result in insufficient brightness of the coating.

[0058] The appropriate ammonium chloride content of the plating solution is 220g / L to 230g / L. If the content is too low, the coating will be gray. Analyze and replenish regularly.

[0059] (4) The above method further includes dehydrogenating the inner pipe of the steel shock-absorbing pad between steps 3) and 4), specifically, placing the blow-dried steel parts in an oven at a temperature of 180°C to 200°C for drying for 24 hours, and then rinsing with running water.

[0060] (5) In the above method, the activation treatment of the inner pipe of the steel shock-absorbing pad in step 4) is specifically: placing the steel part in a 0.5%-1.5% sulfuric acid solution for activation for 5s to 15s.

[0061] (6) In the above method, the passivation treatment of the inner pipe of the steel shock-absorbing pad in step 5) is specifically carried out under the following component passivation solution neutralization conditions: 2% to 5% potassium sodium tartrate, 5% to 10% sodium chloride, 10% to 20% sodium nitrate, 10% to 18% chromium nitrate, 0.5% to 1% sulfuric acid, 1.5% to 2.5% sodium fluorosilicate, 4% to 7% nitric acid, 0.5% to 1% hydrochloric acid, 1.5% to 2.5% cobalt chloride, and the balance water. The passivation conditions are: temperature: 30°C to 40°C, time: 30min to 35min.

[0062] (7) In the above method, the running water washing is washing in running water at 40°C to 60°C for 1 min to 2 min and or washing in running water at 10°C to 38°C for 1 min to 2 min.

[0063] Example 2

[0064] The composition of the electroplating solution for zinc-nickel electroplating is:

[0065] Ammonium chloride is 225g / L, nickel chloride is 140g / L, zinc chloride is 60g / L, triethanolamine is 25g / L, tank opener is 50ml / L, auxiliary brightener is 10ml / L; pH value is 5.35;

[0066] The newly prepared plating solution is pre-electrolyzed before being put into production to remove heavy metal impurities such as copper, lead, antimony, etc. contained in the chemical raw materials; the pre-electrolysis is carried out at a cathode current density of 0.35A / dm2 for 30 hours until the coating reaches a silvery white color.

[0067] Example 3

[0068] The components and conditions of the passivation solution are: 3% potassium sodium tartrate, 7% sodium chloride, 15% sodium nitrate, 15% chromium nitrate, 0.7% sulfuric acid, 2% sodium fluorosilicate, 6% nitric acid, 0.7% hydrochloric acid, 2% cobalt chloride, and the balance is water. The passivation conditions are: temperature: 35°C, time: 33 minutes.

[0069] The main functions achieved by the present invention are:

[0070] 1. Through a series of treatments such as degreasing, activation or weak etching, electroplating zinc and nickel, activation and passivation, the inner pipe of the steel shock absorber is effectively electroplated with zinc and nickel to solve the problem of corrosion of the inner pipe of the steel shock absorber in the automotive field;

[0071] 2. Excellent corrosion resistance:

[0072] The corrosion resistance of the steel shock absorber inner pipe fittings with zinc-nickel alloy electroplating on the surface is 4 to 8 times that of the pure zinc coating, which can effectively provide protection for the steel shock absorber inner pipe fittings. Even in the case of very thin coating, it also shows high corrosion resistance.

[0073] 3. Thermal fatigue resistance:

[0074] After the coating was rapidly cooled and heat treated from -60℃ to 250℃, the corrosion resistance did not change, showing the excellent thermal fatigue resistance of the steel shock absorber inner pipe with zinc-nickel alloy electroplated on the surface;

[0075] 4. Low hydrogen embrittlement:

[0076] The hydrogen embrittlement rate of the steel shock absorber inner pipe fittings with zinc-nickel alloy electroplating on the surface is only 1.5%, which is lower than the embrittlement rate of pure zinc plating (generally more than 40%) and bright cadmium plating (about 18%).

[0077] 5. Hardness and wear resistance: The steel pipe fittings of shock absorber pads with zinc-nickel alloy electroplating on the surface are harder than those with pure zinc electroplating on the surface. Therefore, the steel pipe fittings of shock absorber pads with zinc-nickel alloy electroplating on the surface have better wear resistance; the coating has high hardness and is scratch-resistant;

[0078] 6. Environmental protection characteristics: The plating solution has low toxicity and is beneficial to environmental protection.

[0079] The method for electroplating zinc-nickel alloy on the inner pipe of a steel shock-absorbing pad of the present invention has common mechanical installation, connection or setting methods, which can be implemented as long as the beneficial effects can be achieved; technicians in the industry only need to install and operate it according to the accompanying instruction manual, without the need for creative labor by technicians in this field.

[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for electroplating zinc-nickel alloy on inner pipes of steel shock-absorbing pads. 1) Degrease the inner pipes of the steel shock-absorbing pads and rinse them with running water after degreasing; 2) After activating or weakly etching the inner pipe of the steel shock-absorbing pad, rinse it with running water; 3) Electroplating zinc-nickel on the inner pipes of the steel shock-absorbing pads, rinsing with running water, and drying; 4) Activate the steel parts in 0.5%-1.5% sulfuric acid solution for 5s-15s, and rinse with running water; 5) Then passivate the inner pipes of the steel shock-absorbing pad, rinse with running water, and blow dry; It is characterized in that The plating solution components of zinc-nickel electroplating are: 50g / L~65g / L zinc chloride, 140g / L nickel chloride, 220g / L~230g / L ammonium chloride, 25g / L triethanolamine (content 80%~85%), ammonia water, 50ml / L tank opener, and 10ml / L auxiliary brightener.

2. The method for electroplating zinc-nickel alloy on the inner tube of a steel shock-absorbing pad as claimed in claim 1, characterized in that: The conditions for electroplating zinc and nickel are: temperature: 30℃~40℃, pH value: 5.35~5.60, cathode current density DK: 2A / dm2~4A / dm2, nickel anode area / zinc anode area 1:2.0~1:2.

5.

3. The method for electroplating zinc-nickel alloy on the inner tube of a steel shock-absorbing pad according to claim 1, characterized in that: The electroplating solution for electroplating zinc-nickel in step 3) is prepared as follows: S1. First add 1 / 2 volume of water to the electroplating tank, heat it to 50℃~60℃, then add ammonium chloride, stirring while adding to accelerate dissolution; after the ammonium chloride is completely dissolved, add nickel chloride, zinc chloride, triethanolamine, tank opening agent and auxiliary brightener in sequence; S2. After all components are dissolved, filter the plating solution with a filter to remove particulate impurities; S3. Add water to the specified volume, measure the pH value and adjust it to 5.35-5.40 with ammonia water.

4. A method for electroplating zinc-nickel alloy on inner tubes of steel shock-absorbing pads as claimed in claim 3, characterized in that: The newly prepared plating solution is pre-electrolyzed to remove heavy metal impurities contained in chemical raw materials before being put into production.

5. The method for electroplating zinc-nickel alloy on the inner tube of a steel shock-absorbing pad as claimed in claim 4, characterized in that: The pre-electrolysis is carried out at a cathode current density of 0.3A / dm2 to 0.4A / dm2, and the pre-electrolysis time is 1 hour to 100 hours, until the coating reaches a silvery white color.

6. The method for electroplating zinc-nickel alloy on the inner tube of a steel shock-absorbing pad as claimed in claim 1, characterized in that: Maintenance method of zinc-nickel electroplating solution: A. pH value control; B. Control of Zn / Ni ratio; C. Temperature control: D. Control of cathode current density: E. Addition of cylinder filling agent: F. The appropriate ammonium chloride content of the plating solution is 220g / L~230g / L. If the content is too low, the coating will be gray. Analyze and replenish regularly.

7. A method for electroplating zinc-nickel alloy on inner tubes of steel shock-absorbing pads as claimed in claim 6, characterized in that: pH control: Control the pH value within the range of 5.35 to 5.65, and use hydrochloric acid to adjust the pH to a lower level.

8. The method for electroplating zinc-nickel alloy on the inner tube of a steel shock-absorbing pad as claimed in claim 6, characterized in that: Control of Zn / Ni ratio: The ratio of zinc to nickel content in the zinc-nickel plating solution is controlled at 0.7-0.

9.

9. A method for electroplating zinc-nickel alloy on inner tubes of steel shock-absorbing pads as claimed in claim 8, characterized in that: Detect the Zn / Ni ratio in the zinc-nickel electroplating solution; adjust the area ratio of the zinc anode to the nickel anode based on the test results and change trends.

10. The method for electroplating zinc-nickel alloy on the inner tube of a steel shock-absorbing pad as claimed in claim 1, characterized in that: In step 5), the passivation treatment of the inner pipe fittings of the steel shock-absorbing pad is specifically carried out under the neutralization conditions of the following components: potassium sodium tartrate 2% to 5%, sodium chloride 5% to 10%, sodium nitrate 10% to 20%, chromium nitrate 10% to 18%, sulfuric acid 0.5% to 1%, sodium fluorosilicate 1.5% to 2.5%, nitric acid 4% to 7%, hydrochloric acid 0.5% to 1%, cobalt chloride 1.5% to 2.5%, water balance; the passivation conditions are: temperature: 30°C to 40°C, time: 30min to 35min.

Citation Information

Patent Citations

  • Method for electroplating zinc and nickel alloy on steel work

    CN104005063A