Polycrystalline silicon carbide substrate having density gradient and method for producing same
By introducing density gradients into polycrystalline SiC wafers, the problems of high on-resistance and high manufacturing costs are solved, more efficient electrical signal transmission and a flatter surface are achieved, and manufacturing costs are reduced.
Patent Information
- Application Number
- CN202410372564.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-22
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
The existing silicon carbide (SiC) wafers have high on-resistance due to uneven density during the manufacturing process, which hinders the transmission of electrical signals. The manufacturing cost of high-density wafers is high, and the surface of low-density wafers is rough, making it difficult to planarize and polish.
Polycrystalline SiC wafers with density gradient are used to form density gradients through sintering processes or chemical vapor deposition processes to reduce on-resistance and improve surface flatness.
Lower on-resistance and flatter surfaces are achieved, reducing manufacturing costs and improving the bonding strength of subsequent layers and the efficiency of electronic devices.
Smart Images

Figure CN118727149A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a polycrystalline silicon carbide (SiC) base substrate or wafer including a first density at a first side, a second density at a second side opposite the first side, and a density gradient increasing from the second side to the first side. Background Art
[0002] The semiconductor industry has shown great interest in silicon carbide (SiC), particularly for use in the manufacture of electronic devices or components (eg, diodes, transistors, or other similar power applications).
[0003] The development and manufacture of silicon carbide-based electronic devices is limited by factors such as the electrical and mechanical properties of the silicon carbide wafers that are formed.Many silicon carbide wafers have uniform (eg, the same or substantially the same) density across the length, width, and thickness of the wafer.
[0004] Before coupling or forming additional layers on the silicon carbide wafer, the surface of the silicon carbide wafer may be planarized and polished so that the surface is flat and smooth. For example, for a silicon carbide wafer with a higher density, the voids are smaller and may be fewer, resulting in a smoother surface. However, a higher density wafer uses more material to increase the density, which increases the manufacturing cost. However, a higher density is beneficial for subsequent manufacturing steps. Summary of the invention
[0005] The present disclosure relates to embodiments that provide a silicon carbide (SiC) wafer, which may be a polycrystalline SiC wafer having a density gradient between a first side and a second side. The SiC wafer may be formed using a sintering process followed by a temperature treatment to form the density gradient. Alternatively, the sintering process may be combined with chemical vapor deposition to form the density gradient.
[0006] At least one embodiment includes a polycrystalline SiC wafer or substrate having a first side and a second side opposite the first side. A first density is located on the first side of the polycrystalline silicon carbide (SiC) material. A second density is located on the second side of the polycrystalline silicon carbide (SiC) material, the second density being greater than the first density. A density gradient is located between the first side and the second side. The density gradient may increase in density in a density gradient direction from the first side of the polycrystalline SiC wafer to the second side. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] In order to better understand the embodiments, reference will now be made to the accompanying drawings by way of example. In the accompanying drawings, unless the context otherwise indicates, the same reference numerals represent the same or similar elements or actions. The sizes and relative proportions of the elements in the accompanying drawings are not necessarily drawn to scale. For example, some of these elements may be enlarged and positioned to improve the readability of the accompanying drawings.
[0008] Figure 1A is a side perspective view of an embodiment of a polycrystalline silicon carbide (SiC) substrate having a density gradient; and
[0009] Figure 1B yes Figure 1A An enlarged and enhanced view of a cross section 1B-1B of an embodiment of a polycrystalline SiC substrate in FIG.
[0010] Figure 1C yes Figure 1A An enlarged and enhanced view of section 1C-1C of an embodiment of a polycrystalline SiC substrate in FIG.
[0011] Figure 1D yes Figure 1A An enlarged and enhanced view of a cross section 1D-1D of an embodiment of a polycrystalline SiC substrate in FIG.
[0012] Figure 2A Yes Figure 1A-Figure 1D A side perspective view of an embodiment of a polycrystalline SiC substrate including a single crystal layer as shown in;
[0013] Figure 2B Yes Figure 2A The cross section shown in 2B-2B is coupled to the single crystal layer as shown in Figure 1A-Figure 1D An enlarged and enhanced view of a location on the surface of an embodiment of a polycrystalline SiC substrate shown in;
[0014] Figure 3 Yes Figure 1A-Figure 1D A flow chart of a method for manufacturing an embodiment of a polycrystalline SiC substrate shown in;
[0015] Figure 4A and Figure 4B Yes Figure 3 The manufacturing method shown in the embodiment and Figure 1A-Figure 1D side views of at least some corresponding steps of manufacturing in; and
[0016] Figure 5 is Figure 2A and Figure 2B Flow chart of a method for fabricating a single crystal layer on an embodiment of a polycrystalline SiC substrate. DETAILED DESCRIPTION
[0017] In the following description, certain details are set forth in order to provide a thorough understanding of various embodiments of the apparatus, methods, and articles. However, those skilled in the art will appreciate that other embodiments may be practiced without these details. In other cases, well-known structures and methods associated with, for example, silicon carbide substrates or layers (e.g., polycrystalline silicon carbide, single crystal silicon carbide, etc.), semiconductor manufacturing processes, etc., are not shown or described in detail in some figures to avoid unnecessarily obscuring the description of the embodiments.
[0018] Unless the context requires otherwise, throughout the specification and the claims that follow, the word "comprise" and variations such as "comprising" and "comprises" are to be interpreted in an open, inclusive sense, i.e., "including, but not limited to."
[0019] References throughout the specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment. Thus, appearances of the phrases "in one embodiment" or "in an embodiment" in various places throughout the specification are not necessarily referring to the same embodiment or all embodiments. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments to obtain further embodiments.
[0020] Headings are provided for convenience only and do not interpret the scope or meaning of the disclosure or the claims.
[0021] The sizes and relative positions of the elements in the drawings are not necessarily drawn to scale. For example, the shapes of the various elements and angles may not be drawn to scale, and some of these elements may be enlarged and positioned to improve the readability of the drawings.
[0022] The use of "transverse" means that a surface, sidewall, or similar or analogous structure or feature is at an angle relative to another corresponding surface, sidewall, or similar or analogous corresponding structure or feature. For example, if a first surface is transverse to a first sidewall, then the first surface may be at an angle equal to 25 degrees, 35 degrees, 45 degrees, 75 degrees, 90 degrees, 120 degrees, etc.
[0023] Generally speaking, polycrystalline silicon carbide (SiC) substrates, wafers or layers have been used in various electronic devices and components (e.g., semiconductor dies, semiconductor packages, semiconductor transistors, etc.). These polycrystalline SiC substrates have a resistivity that causes resistance along an electrical path through the polycrystalline SiC substrate. This resistance hinders the electrical signal as it passes through the electrical path, which is referred to as on-resistance (R on The on-resistance (R on ) limits the efficiency or electrical characteristics of electronic devices made of polycrystalline SiC substrates. For example, if the on-resistance (R on ) is high, it may prevent electrical signals from fully passing through the polycrystalline SiC substrate to its destination, resulting in functional errors within the electronic device or component.
[0024] When forming a polycrystalline SiC substrate, the density affects the formation of voids or otherwise affects the roughness of the surface on which subsequent layers or devices are formed. The present disclosure relates to manufacturing polycrystalline SiC substrates with flat surfaces, which are cheaper and produce fewer voids. This is in contrast to conventional polycrystalline SiC substrates that are initially formed using a sintering process in which there are large voids between grains. These voids may exist in or adjacent to the surface of a conventional polycrystalline SiC substrate to be flattened and polished (i.e., leveled). Prior to flattening and polishing, the surface of a conventional polycrystalline SiC substrate may be relatively rough and uneven, in part due to different grain sizes and crystal structures.
[0025] After planarization and polishing, the surface of a conventional polycrystalline SiC substrate is flat (i.e., flat) and smooth (i.e., polished). However, during such planarization and polishing processes, voids present on the surface of a conventional polycrystalline SiC substrate or adjacent to the surface of a conventional polycrystalline SiC substrate form dents or depressions. After surface planarization and polishing, another layer is typically formed on the surface of a conventional polycrystalline SiC substrate. When the layer is formed on the surface of a conventional polycrystalline SiC substrate having dents and depressions, defect voids are formed between the layer and the surface. These defect voids may increase the on-resistance (R) as described above. on ), resulting in that a semiconductor package or device including this layer and a conventional polycrystalline SiC substrate cannot operate within efficiency tolerances.
[0026] Costs can be reduced by manufacturing conventional polycrystalline SiC substrates with low density. However, low density forms a relatively rough surface due to a larger number of defect voids. This results in ridges and raised areas remaining even after the surface of the low-density polycrystalline SiC substrate is polished and flattened.
[0027] The present disclosure relates to one or more embodiments of a polycrystalline SiC substrate having a density gradient such that a first density at a first surface of the substrate is less than a second density at a second surface of the substrate opposite to the first surface. The second density at the second surface can allow for more efficient polishing and flattening of the second surface to increase the bonding strength between layers of material (e.g., semiconductor material, silicon material, etc.) subsequently formed on the second surface. At the same time, the cost of manufacturing a polycrystalline SiC substrate with a density gradient is reduced in the overall manufacturing cost compared to manufacturing a high-density conventional polycrystalline SiC. In other words, a polycrystalline SiC substrate with a density gradient has the advantage of manufacturing a flatter and less rough surface than a low-density conventional polycrystalline SiC substrate and being cheaper than a high-density conventional polycrystalline SiC substrate.
[0028] At least one embodiment of the apparatus of the present disclosure is summarized as follows. The apparatus includes a polycrystalline silicon carbide (SiC) wafer, the polycrystalline silicon carbide (SiC) wafer including a first side and a second side opposite to the first side. A first density is located on the first side of the polycrystalline silicon carbide (SiC) wafer, and a second density is located on the second side of the polycrystalline silicon carbide (SiC) wafer. The second density is greater than the first density. A density gradient is located between the first side and the second side, and the density gradient increases in density in a density gradient direction from the first side of the polycrystalline silicon carbide (SiC) wafer to the second side.
[0029] At least one embodiment of the method of the present disclosure is summarized as follows. The method includes forming a polycrystalline silicon carbide (SiC) substrate. After forming the polycrystalline silicon carbide (SiC) substrate, a density gradient is generated between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite to the first side by exciting mass transfer directed in a mass transfer direction from a first side of the polycrystalline silicon carbide base substrate to a second side opposite to the first side. Exciting mass transfer includes exposing the first side of the polycrystalline silicon carbide (SiC) substrate to a first temperature that transfers mass away from the first side of the polycrystalline silicon carbide (SiC) substrate, and exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a second temperature that transfers mass toward the second side of the polycrystalline silicon carbide (SiC) substrate, the second temperature being less than the first temperature. A polycrystalline silicon carbide (SiC) substrate is cooled to generate a first density on a first side of the polycrystalline silicon carbide (SiC) substrate, a second density greater than the first density on a second side of the polycrystalline silicon carbide (SiC) substrate, and a density gradient between the first side and the second side of the polycrystalline silicon carbide (SiC) substrate.
[0030] At least one embodiment of the method of the present disclosure is summarized as follows. The method includes generating a density gradient between a first side of a polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite to the first side. Generating the density gradient between the first side and the second side includes exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a chemical vapor deposition process, thereby infusing silicon (Si) and carbon (C) into the second side of the polycrystalline silicon carbide (SiC) substrate.
[0031] Figure 1A A side perspective view of a polycrystalline silicon carbide (SiC) substrate 100 having a density gradient is provided. The polycrystalline silicon carbide (SiC) substrate 100 may be referred to as the substrate 100 hereinafter. The substrate 100 may be a wafer, which may be Figure 1A The cylindrical shape shown in .
[0032] The substrate 100 includes a first surface 102 and a second surface 104 opposite to the first surface 102. The first sidewall 106 is transverse to the first surface 102 and the second surface 104 and extends from the first surface 102 to the second surface 104. The roughness of the second surface 104 is less than or equal to 5 angstroms. and is flat, such that the second surface 104 is flat (ie, polished, smooth, planarized, and flat). Figure 1A The first surface 102 may be a rear surface, a back surface, a bottom surface, or a lower surface, and based on the orientation of the substrate 100 shown in FIG. Figure 1A In the orientation of the substrate 100 shown in FIG. 1 , the second surface 104 may be a front surface, a top surface, or an upper surface.
[0033] The first density of the substrate 100 is located at the first surface 102 and the second density of the substrate 100 is located at the second surface 104. The first density of the substrate 100 is different from the second density of the substrate 100. For example, the first density is less than the second density. The substrate 100 having a density gradient includes a density gradient direction represented by an arrow 108, which points in a direction away from the first surface 102 and toward the second surface 104. The density gradient of the substrate 100 increases along the substrate 100 between the first surface 102 and the second surface 104 in the density gradient direction 108. The density gradient increases along the density gradient direction 108, so that the first density at the first surface 102 is the lowest density of the density gradient, and the second density at the second surface 104 is the highest density of the density gradient. In at least one embodiment, the first density is between 2.75-3.05 grams per cubic centimeter (i.e., 2.75-3.05 g / cm 3 ) or equal to the upper and lower limits of the range (i.e., equal to 2.75 g / cm 3 Or equal to 3.05g / cm 3 In at least one embodiment, the second density is between 3.05 and 3.20 grams per cubic centimeter (i.e., 3.05-3.20 g / cm 3 ) or equal to the upper and lower limits of the range (i.e., equal to 3.05 g / cm 3 Or equal to 3.20g / cm 3 In some embodiments, the second density may be in the range of 3.10-3.20 grams per cubic centimeter (i.e., 3.10-3.20 g / cm 3 ) or may be equal to the upper and lower limits of the range (i.e., equal to 3.10 g / cm 3 Or equal to 3.20g / cm 3 In some embodiments, the second density may range from 3.10 to 3.26 grams per cubic centimeter (ie, 3.10 g / cm 3 -3.26g / cm3 ) or may be equal to the upper and lower limits of the range (i.e., equal to 3.10 g / cm 3 Or equal to 3.26g / cm 3 ).
[0034] In some embodiments, the first density at the first surface 102 of the substrate 100 may be 2.5-3.0 g / cm 3 and the second density at the second surface may be in the range of 3.0-3.3 g / cm 3 In some embodiments, the second density at the second surface 104 of the substrate 100 may be 3.2-3.3 g / cm 3 The percentage of voids present at or adjacent to the first surface 102 of the substrate 100 is in the range of 20% to 25%, or may be equal to the upper and lower limits of the range. The percentage of voids present at or adjacent to the second surface 104 of the substrate 100 is in the range of 2% to 0.5%, or may be equal to the upper and lower limits of the range.
[0035] In some embodiments, the density increases linearly as the density increases from a first density at the first surface 102 of the substrate 100 to a second surface 104 of the substrate 100 .
[0036] The substrate 100 includes a first thickness 110. The first thickness 110 may be in a range of 200 micrometers (μm) to 1.2 millimeters (mm), or may be equal to the upper and lower limits of the range (i.e., equal to 200 micrometers (μm) or equal to 1.2 millimeters (mm)). In some embodiments, the first thickness 110 may be greater than 1.2 millimeters (mm) or may be less than 200 micrometers (μm). In some embodiments, the first thickness 110 may be substantially equal to 1 millimeter (mm).
[0037] The corresponding grains at the first surface 102 of the substrate 100 or in close proximity to the first surface 102 of the substrate 100 (e.g., in the region having the first density) may have a size ranging from 1 micrometer (μm) to 20 micrometers (μm) or equal to the upper and lower limits of the range. The corresponding grains at the second surface 104 of the substrate 100 or in close proximity to the second surface 104 of the substrate 100 (e.g., in the region having the second density) may have a size ranging from 10 micrometers (μm) to 30 micrometers (μm) or equal to the upper and lower limits of the range. The corresponding grains at the midpoint between the first surface 102 and the second surface 104 may have a size ranging from 5 micrometers (μm) to 25 micrometers (μm) or equal to the upper and lower limits of the range. The corresponding grains at the first surface 102 of the substrate 100 or in close proximity to the boundary of the first surface 102 of the substrate 100 may have a size ranging from 1 micrometer (μm) to 20 micrometers (μm) or equal to the upper and lower limits of the range. The corresponding grains at or adjacent to the second surface 104 of the substrate 100 may have a size ranging from 10 micrometers (μm) to 30 micrometers (μm) or equal to the upper and lower limits of the range. The respective voids at or adjacent to the first surface 102 of the substrate 100 (e.g., in the region with the first density) may be in the range of 5 micrometers (μm) to 50 micrometers (μm) or equal to the upper and lower limits of the range, and preferably, the respective voids at or adjacent to the first surface 102 of the substrate 100 (e.g., in the region with the first density) may be in the range of 25 micrometers (μm) to 40 micrometers or equal to the upper and lower limits of the preferred range. The respective voids at or adjacent to the second surface 104 of the substrate 100 may have a size less than or equal to 5 micrometers (μm). Each void at or proximate to the first surface 102 of the substrate 100 may have a size less than or equal to 10 micrometers (μm).
[0038] Figure 1B yes Figure 1A The first portion 112 of the substrate 100 is at Figure 1B 1 and is adjacent to the second surface 104 of the substrate 100, such that the first portion 112 of the substrate 100 has a corresponding density greater than the first density at the first surface 102 and less than the second density at the second surface 104. Figure 1BThe first portion 112 of the substrate 100 shown in FIG. 1 is located between the first surface 102 and the second surface 104, so the corresponding density of the first portion 112 is less than the corresponding density of the corresponding portion of the substrate 100 closer to the second surface 104 than the first portion 112, and greater than the corresponding density of the corresponding portion of the substrate 100 closer to the first surface 102 than the first portion 112. In other words, the first portion 112 is closer to the second surface 104 than the first surface 102.
[0039] Since the density is slightly less than the second density of the substrate 100 at the second surface 104, very small or very few voids 114 exist between the grains 116 of the substrate 100 at the first portion 112 of the substrate 100. Since the voids 114 are very small or very few in number, the first portion 112 of the substrate 100 has a relatively high density when the first portion 112 is adjacent to the second surface 104 of the substrate 100. The voids 114 may exist between adjacent grains 116, and at least some of the voids 114 may exist along grain boundaries 118 between the grains 116 of the substrate 100.
[0040] Figure 1C yes Figure 1A The second portion 120 of the substrate 100 is at Figure 1C 1 and is adjacent to the first surface 102 of the substrate 100, such that the second portion 112 of the substrate has a corresponding density greater than the first density at the first surface and less than the second density at the second surface 104. Figure 1C The second portion of the substrate 100 shown in FIG. 1 is located between the first surface 102 and the second surface 104, so the corresponding density of the second portion 120 is less than the corresponding density of the corresponding portion of the substrate 100 closer to the second surface 104 than the second portion, and greater than the corresponding density of the corresponding portion of the substrate 100 closer to the first surface 102 of the substrate 100. In other words, the second portion 120 is closer to the first surface 102 than the second surface 104.
[0041] like Figure 1B and 1C As shown in the embodiment of Figure 1B The respective voids 114 between the grains 116 and along the grain boundaries 118 in the second portion 120 shown in FIG. 1 are larger than the respective voids 114 between the grains 116 and along the grain boundaries 118 in the first portion 112. The respective voids 114 in the second portion 120 being larger than the respective voids in the first portion 112 means that the respective density of the second portion 120 is lower than the respective density of the first portion 112.
[0042] In some embodiments of the substrate 100, a first number of corresponding voids 114 present at the first portion 112 may be less than a second number of corresponding voids 114 present at the second portion 120. Since the corresponding voids 114 in the second portion 120 are generally larger and more numerous relative to the corresponding voids 114 present in the first portion 112, the corresponding density of the first portion 112 of the substrate 100 is greater than the corresponding density of the second portion 120 of the substrate 100.
[0043] Figure 1D Yes Figure 1A An enlarged and enhanced view of the cross section 1D-1D of the embodiment of the polycrystalline SiC substrate 100 shown in FIG. Figure 1D As shown in , the second surface 104 includes slight indentations 122 present along the second surface 104. After the second surface 104 is flattened and polished, the voids 114 may cause slight indentations 122 at the second surface 104. The details of flattening and polishing the second surface 104 will be discussed in detail below. However, these slight indentations 122 are much smaller than the indentations when the similar or similar surface of the low-density conventional polycrystalline SiC substrate is flattened and polished. For example, when the similar or similar surface of the low-density conventional polycrystalline SiC substrate is flattened and polished, the corresponding indentations will be much larger, so that larger ridges and raised portions will exist in the similar or similar surface of the low-density conventional polycrystalline SiC. In other words, the indentations 122 of the flattened and polished second surface 104 of the substrate 100 will be more similar to or similar to the indentations present at the similar or similar surface of the flattened and polished high-density conventional polycrystalline SiC substrate, while at the same time, the manufacturing of the substrate 100 is cheaper than the high-density conventional polycrystalline SiC substrate. In other words, the substrate 100 has both the lower manufacturing cost of a low-density conventional polycrystalline SiC substrate and the better surface finish of a high-density conventional polycrystalline SiC substrate.
[0044] Figure 2A 1 is a side perspective view of a single crystal layer 124 coupled to and on an embodiment of a second surface 104 of a substrate 100. The single crystal layer 124 may be silicon carbide (SiC). The single crystal layer 124 is coupled or bonded to the second surface 104 of the substrate 100 at a coupling or bonding region 128 located between the single crystal layer 124 and the substrate 100. The single crystal layer 124 has a surface 128 facing away from the second surface 104 of the substrate 100 and facing away from the substrate 100. The single crystal layer 124 has a second thickness 130 extending from the second surface 104 of the substrate 100 to the surface 128 of the single crystal layer 124. The second surface 104 of the substrate 100 is covered by the single crystal layer 124, and the single crystal layer 124 includes a second sidewall 132 that is transverse to the surface 128 and the second surface 104, the second sidewall 132 extending from the second surface 104 to the surface 128, and is coplanar and flush with the first sidewall 106 of the substrate 100.
[0045] The second thickness 130 may be less than or equal to 1 micrometer (μm). In some embodiments, the second thickness 130 may be greater than 1 micrometer (μm).
[0046] Figure 2B yes Figure 2A An enlarged and enhanced view of the circled section 2B-2B. Figure 2B As shown in FIG. 1 , at the bonding region, one or more cavities 134 are located between the single crystal layer 124 and the substrate 100. When the single crystal layer 124 is formed on, coupled to, or bonded to the second surface 104 of the substrate 100, due to the presence of the indentation 122 at the second surface 104 of the substrate 100, one or more cavities 134 exist between the second surface 104 and the single crystal layer 124. In some embodiments, when the single crystal layer 124 is formed on, coupled to, or bonded to the second surface 104 of the substrate 100, the one or more cavities 134 may not exist at all, because the indentation 122 may not exist at all or the indentation 122 may be small enough so that the single crystal layer 124 fills the small indentation 122 at the second surface 104 of the substrate 100.
[0047] Even when one or more cavities 134 exist due to the small indentations 122 at the second surface 104 of the substrate 100 after planarization and polishing, the one or more cavities 134 are small enough so that the one or more cavities 134 have little effect on the impedance of the corresponding electrical signal passing through the substrate 100 and the single crystal layer 124. Even when one or more cavities 134 exist due to the small indentations 122 at the second surface 104 of the substrate 100 after planarization and polishing, there may be only a small number of one or more cavities so that the one or more cavities have little effect on the impedance of the corresponding electrical signal passing through the substrate 100 and the single crystal layer 124.
[0048] Figure 5 Is manufactured as Figure 1A-Figure 1D Flowchart 200 of a method of an embodiment of substrate 100 shown in FIG. Flowchart 200 includes a first step 202 , a second step 204 , and a third step 206 .
[0049] In the first step 202, a polycrystalline silicon carbide (SiC) base substrate 208 is formed, which may be referred to as the base substrate 208. For example, the base substrate 208 may be formed by sintering a mixture of powdered silicon (Si) and powdered carbon (C) forming the base substrate 208 together using a furnace or sintering powdered silicon carbide (SiC) forming the base substrate 208 together using a furnace. In other words, the base substrate 208 may be formed using a sintering process known in the silicon carbide (SiC) substrate forming industry. After formation, the base substrate 208 includes a first surface 210 corresponding to the first surface 102 and a second surface 212 corresponding to the second surface 104 and opposite to the first surface 210. The base substrate 208 includes a sidewall 214 extending from the first surface 210 to the second surface 212 and transverse to the first surface 210 and the second surface 212.
[0050] After the first step 202 of forming the base substrate 208, a second step 204 of forming or generating a density gradient within the base substrate 208 is performed. The density gradient is formed or generated within the base substrate 208 by applying a first temperature 214 to the first surface 210 and a second temperature 216 to the second surface 212. The first temperature 214 is different from the second temperature 216. For example, the first temperature 214 is greater than the second temperature 216. The first temperature 214 may be greater than or equal to 2000 degrees Celsius and the second temperature 216 may be less than or equal to 2000 degrees Celsius. In some embodiments, the first temperature 214 may be greater than or equal to 2200 degrees Celsius and the second temperature 216 may be less than or equal to 2000 degrees Celsius. Applying the first temperature 214 to the first surface 210 and applying the second temperature 216 to the second surface 212 occurs simultaneously, causing atoms and particles of the base substrate to move or be transported in a mass transport direction represented by arrow 218. The mass transport direction 218 is directed away from the first surface and toward the second surface 212. As the atoms and particles move in the mass transport direction 218, the first density at the first surface 210 decreases and the second density at the second surface 212 increases. In other words, the second density at the second surface 212 becomes greater than the first density at the first surface 210. After the first temperature 214 has been applied to the first surface 210 and the second temperature 216 has been applied to the second surface 212 for a period of time, the base substrate 208 is allowed to cool. As the base substrate 208 cools down from being previously heated by the first temperature 214 and the second temperature 216, the first density at the first surface 210, the second density at the second surface 212, and the density gradient between the first surface 210 and the second surface 212 of the base substrate 208 solidify. After the base substrate 208 is allowed to cool for a period of time, the base substrate 208 has a density gradient that increases along the substrate in the mass transport direction 218, wherein the second density at the second surface 212 is the maximum density of the base substrate 208, and the first density at the first surface 210 is the lowest density of the base substrate 208. The density of the substrate between the first surface 210 and the second surface 212 is an intermediate density that is greater than the first density at the first surface 210 and less than the second density at the second surface 212 .
[0051] In an alternative embodiment, the density gradient in the base substrate 208 between the first surface 210 and the second surface 212 may be formed using a chemical vapor deposition (CVD) process instead of applying the first temperature 214 to the first surface 210 and the second temperature 216 to the second surface 212. When using a CVD process instead of applying the first temperature 214 and the second temperature 216 to the base substrate 208, additional silicon carbide (SiC) or silicon (Si) and carbon (C) particles or atoms are introduced to the second surface 212 of the base substrate such that the additional SiC or Si and C particles and atoms impregnate the base substrate 208 at the second surface 212, resulting in the formation of a density gradient within the base substrate 208 such that the second density at the second surface 212 is greater than the first density at the first surface 210 and the intermediate density between the first surface 210 and the second surface 212 is greater than the first density and less than the second density. When utilizing a CVD process, additional SiC or Si and C particles and atoms may impregnate the base substrate 208, thereby filling the voids 114 at the second surface or within the base substrate at a depth less than a third thickness 220 of the base substrate extending from the first surface 210 to the second surface 212, respectively. The third thickness 220 of the base substrate 208 may be greater than the first thickness 110 of the substrate 100.
[0052] In view of the above, in at least one embodiment, when performing the CVD process, a porous polycrystalline SiC substrate is placed in a furnace. A hydrogen flow is introduced into the furnace. In the hydrogen flow, silane and ethylene are introduced into the hydrogen flow. Alternatively, propane can be introduced into the hydrogen flow as a carbon source. In other words, some carbon sources and some silicon sources are introduced into the hydrogen flow so that carbon and silicon are present in the hydrogen flow. By introducing silane and ethylene into the hydrogen flow, free silicon and free carbon are formed. These free silicon and free carbon are then deposited on the porous substrate as silicon carbide. When the free silicon and free carbon are deposited on the porous substrate, the temperature of the furnace is substantially equal to 1600 degrees Celsius. This causes the free silicon and free carbon to be deposited on the porous substrate in the form of silicon carbide (SiC). Furthermore, since the substrate is porous (i.e., the porosity ranges from 7% to 20%, or is equal to the upper and lower limits of the range), the silicon carbide (SiC) deposited onto the porous substrate actually impregnates the porous substrate, thereby filling the voids within the porous substrate located at or adjacent to the second surface 212 of the base substrate 208. This results in the base substrate 208 being impregnated with silicon carbide, so that a density gradient is formed between the first surface 210 and the second surface 212 of the base substrate 208.
[0053] After the second step 204 in which the density gradient has been formed and generated throughout the base substrate 208, a third step 206 is performed in which the second surface 212 of the base substrate 208 is planarized (i.e., flattened) and polished (i.e., smoothed) by a planarization and polishing tool 222, which may be a chemical mechanical planarization tool that rotates to planarize and polish the second surface 212 of the base substrate 208. After the second surface 212 is planarized and polished by the planarization and polishing tool 222, the polycrystalline SiC substrate 100 has been manufactured. The second surface 212 may be polished to have a density of less than or equal to 5 angstroms. The roughness of the second surface 212 is such that the second surface 212 becomes the same or similar to the second surface 104 as previously discussed herein.
[0054] In such Figure 4A During the third step 206 shown in FIG. 2 , due to the densification process in the second step 204 in which a density gradient is formed within the base substrate such that a second density (e.g., high density) at the second surface 212 is greater than a first density (e.g., low density) at the first surface 210, there are fewer voids 114 at, adjacent to, or in close proximity to the second surface 212, so the second surface 212 can be more easily planarized and polished effectively by the planarization and polishing tool 222. In other words, if any dimples 122 exist at the second surface 212 after planarization and polishing by the planarization and polishing tool 222, the dimples 122 are small so that the second surface 212 has a thickness of less than or equal to 20 angstroms. In some embodiments, the indentation is small, so that the second surface 212 has a roughness less than or equal to 5 angstroms. Roughness.
[0055] In such Figure 4B After the third step 206 shown in FIG. , the base substrate 208 has been converted into Figure 1A-Figure 1C The substrate 100 is shown. In other words, after the manufacturing method in the flowchart 200 is completed, the substrate 100 has been manufactured.
[0056] It is cheaper to manufacture a conventional multicrystalline SiC substrate with high density using the manufacturing method in flowchart 200 than through a conventional multicrystalline SiC substrate as a larger amount of material is required to manufacture a conventional multicrystalline SiC substrate with high density through a conventional multicrystalline SiC substrate relative to manufacturing substrate 100. Moreover, it may be cheaper to manufacture a conventional multicrystalline SiC substrate with high density using the manufacturing method in flowchart 200 than through a conventional base substrate to form a conventional base substrate with high density and then use it to form a conventional multicrystalline SiC substrate with high density, because sintering base substrate 208 together may require less energy than forming a conventional base substrate with high density through a conventional base substrate and then using it to form a conventional multicrystalline SiC substrate with high density.
[0057] Although it is cheaper to manufacture the substrate 100 using the manufacturing method in flowchart 200 than to manufacture a high-density conventional polycrystalline SiC substrate, the second density at the second surface 212 of the base substrate 208 is high and similar to the high density of conventional high-density polycrystalline SiC substrates, allowing the second surface 212 of the base substrate 208 to be effectively and consistently planarized and polished to reduce the size of the dimples 122, to reduce the number of dimples 122 that exist after planarization and polishing, or to prevent the dimples 122 from existing at all.
[0058] In view of the above discussion, the method of manufacturing substrate 100 is less expensive than manufacturing a high-density conventional polycrystalline SiC substrate having a high density throughout, while still allowing second surface 212 to be effectively and consistently planarized and polished in a manner similar to when various surfaces of a high-density conventional polycrystalline SiC substrate are planarized and polished.
[0059] After the substrate 100 is manufactured using the processes discussed herein, the substrate 100 can be used to form an electronic component, such as a semiconductor package, a semiconductor die, or some other similar electronic or semiconductor component. For example, after the substrate 100 is manufactured, the substrate 100 can be further refined or processed (e.g., segmented, back-grinded, etc.) to form an electronic component. Alternatively, for example, one or more additional layers can be formed on the second surface 104 of the substrate 100 (e.g., the single crystal layer 124), a semiconductor structure can be formed on the second surface 104 of the substrate 100, or a semiconductor structure can be coupled to the second surface 104 of the substrate 100. For example, in at least one embodiment, the single crystal layer 124 is formed on the second surface 104, which will be referred to below. Figure 5 Discuss in more detail.
[0060] Figure 5 3 is a flow chart 300 of a method for fabricating a single crystal layer 124 on the second surface 104 of the substrate 100. Figure 5As shown in , the first step 202, the second step 204, and the third step 206 in the flowchart 200 of the method of manufacturing the substrate 100 are performed as previously discussed herein. After the substrate 100 is formed, the fourth step 302 is performed, in which the single crystal layer 124 is formed on, coupled to, or bonded to the second surface 104 of the substrate 100. For example, the single crystal layer 124 can be a wafer thinner than the substrate 100, which is bonded to, coupled to, or adhered to the second surface 104 of the substrate 100. Alternatively, the single crystal layer 124 can be deposited on the second surface 104 of the substrate 100 by a deposition technique, so that the single crystal layer 124 is formed on, bonded to, or coupled to the second surface 104 of the substrate 100. For example, such a deposition technique can be a sputtering technique, a vapor deposition technique, a crystal growth technique, or some other technique for forming the single crystal layer 124 on the second surface 104 of the substrate 100 or bonding or coupling the single crystal layer 124 to the second surface 104 of the substrate 100.
[0061] In at least one embodiment, in the fourth step 302, the single crystal layer 124 is directly and physically coupled to the second surface 212. For example, the single crystal layer 124 may be formed by first coupling a single crystal substrate (not shown) to the second surface 212 by exposing the second surface 212 to bombardment of argon (Ar) ions or neutral atoms (e.g., a particle beam that may be argon (Ar), may be neutral atoms, or may be some other similar or like type of particles or atoms that may be suitable) in an ultra-high vacuum to clean and activate the second surface 104 of the substrate 100 through a SAB (surface activated bonding) technique. Once the second surface 104 has been cleaned and activated by the SAB technique, the single crystal substrate 124 is applied to the second surface 104, resulting in the single crystal substrate being physically and directly coupled to the second surface 104. Once the single crystal substrate has been directly and physically coupled to the second surface 104, a portion of the single crystal substrate is removed so that the single crystal layer 124 remains present on the second surface 212, which corresponds to the second surface 104 of the substrate 100. Before the second surface 212 is exposed to the bombardment of argon (Ar) ions or neutral atoms, the second surface 212 may be planarized or polished.
[0062] In at least one alternative embodiment, a first conductive layer (not shown) is formed on the second surface 212, and a second conductive layer (not shown) is formed on the surface of the single crystal substrate to be coupled to the second surface 212. The first conductive layer and the second conductive layer can be formed by a sputtering technique. Once the first conductive layer and the second conductive layer are formed, the first and second layers can be cleaned and activated using the SAB technique as described above, and then the corresponding surface of the single crystal substrate is applied to the second surface 212. After the single crystal substrate has been directly and physically coupled to the second surface 212, a portion of the single crystal substrate is removed so that the single crystal layer 124 remains present on the second surface 104 of the substrate. The first conductive layer and the second conductive layer can be planarized and polished before being exposed to bombardment by argon (Ar) ions or neutral atoms.
[0063] If at least some of the indentations 122 exist at the second surface 104 of the substrate 100 when the single crystal layer 124 is formed on, bonded to, or coupled to the second surface 104 (which corresponds to the second surface 212) of the substrate 100, then one or more cavities 134 may be formed and exist between the single crystal layer 124 and the substrate 100. However, since these one or more cavities 134 are small, the one or more cavities provide little impedance to the electrical signal when the electrical signal passes through the substrate 100 and the single crystal layer 124. Alternatively, the indentations 122 may not exist, so that one or more cavities do not exist between the single crystal layer 124 and the substrate 100. Alternatively, the indentations 122 may be completely filled when the single crystal layer 124 is formed on the second surface 104 of the substrate 100 or bonded to or coupled to the second surface 104 of the substrate 100. By keeping one or more cavities 134 small or by avoiding them altogether, there is little impedance to the electrical signals as they pass through the substrate 100 and the single crystal layer 124 , thereby resulting in more efficient and accurate devices in which the substrate 100 and the single crystal layer 124 are incorporated.
[0064] When one or more cavities exist between the substrate 100 and the single crystal layer 124 , the size of the one or more cavities is less than or equal to 10 micrometers (μm).
[0065] In view of the above discussion, the substrate 100 is cheaper to manufacture, similar to manufacturing a low-density conventional polycrystalline SiC substrate having a low density overall, while the substrate 100 has less roughness at the second surface when planarized and polished, similar to planarizing or polishing a corresponding surface of a high-density conventional polycrystalline SiC substrate.
[0066] After the single crystal layer 124 has been formed on or coupled to the second surface 104 of the substrate 100, the single crystal layer 124 may be further refined or processed (e.g., polished, thinned, etc.) to form an electronic component. Alternatively, for example, one or more additional layers may be formed on the single crystal layer 124, a semiconductor structure may be formed on the single crystal layer 124, or a semiconductor structure may be coupled to the single crystal layer 124 (e.g., a dielectric layer, a conductive layer, a non-conductive layer, etc.).
[0067] After the single crystal layer 124 has been formed on or coupled to the second surface 104 of the substrate 100, the substrate 100 and the single crystal layer 124, one or more additional layers (e.g., dielectric layers, semiconductor layers, conductive layers, non-conductive layers, etc.) may be formed on the substrate 100 and the single crystal layer 124. Once these one or more additional layers are formed, the substrate 100, the single crystal layer 124, and the one or more additional layers may be singulated into individual dies or may be singulated into individual stacked layer assemblies, which may be further processed to form various semiconductor dies, semiconductor packages, semiconductor components, or other similar electronic components. The semiconductor dies, semiconductor packages, semiconductor components, or other similar electronic components may be positioned within a phone, a tablet, a computer, or some other similar electronic device.
[0068] The individual dies singulated from the substrate 100, the single crystal layer 124, and one or more additional layers may then be encapsulated in a molding compound, epoxy, resin, or similar material to form a corresponding semiconductor package, semiconductor component, or other similar electronic component. The semiconductor package may be positioned within a phone, tablet, computer, or some other similar electronic device.
[0069] The first density at the first surface 102 of the substrate 100 may have a lower density than that of a single crystal silicon carbide (SiC) substrate, and the second density at the second surface 104 of the substrate 100 may have a density similar to that of a single crystal silicon carbide (SiC) substrate. However, manufacturing the substrate 100 may be cheaper than manufacturing a high density polycrystalline SiC substrate and than manufacturing a single crystal SiC substrate.
[0070] The substrate 100 may have a resistivity of less than or equal to 20 milliohm-cm at the second surface 104 of the substrate 100. In some embodiments, the substrate 100 may have a resistivity of less than or equal to 5 milliohm-cm at the second surface 104 of the substrate 100.
[0071] When the single crystal layer 124 exists on the substrate 100 having a density gradient, the resistivity of the single crystal layer 124 can be less than or equal to a resistivity less than or equal to 25 mohm-cm or preferably less than or equal to 18 mohm-cm or in the range of 15-20 mohm-cm or equal to the upper and lower limits of this range.
[0072] At least one embodiment of the apparatus of the present disclosure can be summarized as including: a polycrystalline silicon carbide (SiC) wafer including a first side and a second side opposite to the first side; a first density at the first side of the polycrystalline silicon carbide (SiC) wafer; a second density at the second side of the polycrystalline silicon carbide (SiC) wafer, the second density being greater than the first density; and a density gradient between the first side and the second side, the density gradient increasing in a density gradient direction pointing from the first side of the polycrystalline silicon carbide (SiC) wafer to the second side.
[0073] The polycrystalline silicon carbide (SiC) wafer may also include a second side having a thickness of less than 5 angstroms. The roughness of the surface.
[0074] The resistivity at the second side of the polycrystalline silicon carbide (SiC) wafer may be less than or equal to 20 milliohm centimeters (mohm-cm).
[0075] The resistivity at the second side of the polycrystalline silicon carbide (SiC) wafer may be less than 5 milliohm-cm.
[0076] A thickness extending from a first side to a second side of a polycrystalline silicon carbide (SiC) wafer and may be less than or equal to 800 micrometers (μm).
[0077] The device may also include a single crystal silicon carbide (SiC) layer that may be coupled to the second side of the polycrystalline silicon carbide (SiC) wafer.
[0078] The polycrystalline silicon carbide (SiC) wafer may have a first thickness extending from the first side to the second side; and the single crystal silicon carbide (SiC) layer may include: a surface facing away from the polycrystalline silicon carbide (SiC) wafer; and a second thickness extending from the second side to the surface of the single crystal silicon carbide (SiC) layer, and the second thickness may be less than the first thickness.
[0079] The second thickness may be less than or equal to 1 micrometer (μm).
[0080] The first thickness may be less than or equal to 800 micrometers (μm).
[0081] At least one embodiment of the method of the present disclosure can be summarized as comprising: forming a polycrystalline silicon carbide (SiC) substrate; after forming the polycrystalline silicon carbide (SiC) substrate, generating a density gradient between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite to the first side by stimulating mass transport directed in a mass transport direction from a first side of the polycrystalline silicon carbide base substrate to a second side opposite to the first side, wherein stimulating mass transport comprises: exposing the first side of the polycrystalline silicon carbide (SiC) substrate to a mass transport direction directed from a first side of the polycrystalline silicon carbide (SiC) base ... exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a second temperature that transfers mass toward the second side of the polycrystalline silicon carbide (SiC) substrate, the second temperature being less than the first temperature; and cooling the polycrystalline silicon carbide (SiC) substrate to generate a first density on the first side of the polycrystalline silicon carbide (SiC) substrate, a second density greater than the first density on the second side of the polycrystalline silicon carbide (SiC) substrate, and a density gradient between the first side and the second side of the polycrystalline silicon carbide (SiC) substrate.
[0082] Forming a polycrystalline silicon carbide (SiC) substrate may include sintering at least one of: silicon carbide (SiC) powder; and a powdered mixture of silicon (Si) and carbon (C).
[0083] The second temperature may be greater than or equal to 2000 degrees Celsius.
[0084] The first temperature may be less than or equal to 2000 degrees Celsius.
[0085] The first temperature may be equal to 2000 degrees Celsius and the second temperature may be greater than or equal to 2100 degrees Celsius.
[0086] The method may also include coupling a single crystal silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) base substrate.
[0087] The density gradient may increase in a mass transport direction from a first side toward a second side of the polycrystalline silicon carbide (SiC) substrate.
[0088] At least one embodiment of the method of the present disclosure can be summarized as including: generating a density gradient between a first side of a polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite to the first side, generating the density gradient between the first side and the second side including: exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a chemical vapor deposition process, thereby infusing silicon (Si) and carbon (C) into the second side of the polycrystalline silicon carbide (SiC) substrate.
[0089] The method may also include coupling a single crystal silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) substrate.
[0090] The method may also include, before generating a density gradient between the first side of the polycrystalline silicon carbide (SiC) substrate and the second side of the polycrystalline silicon carbide (SiC) substrate, forming the polycrystalline silicon carbide (SiC) substrate by sintering at least one of the following: silicon carbide (SiC) powder; and a powdered mixture of silicon (Si) and carbon (C).
[0091] The density gradient may increase in a density gradient direction away from the first side of the polycrystalline silicon carbide (SiC) substrate and toward the second side of the polycrystalline silicon carbide (SiC) substrate.
[0092] The various embodiments described above can be combined to provide further embodiments. Aspects of the embodiments can be modified, if necessary to employ concepts of the various patents, applications and publications to provide further embodiments.
[0093] These and other changes can be made to the embodiments in light of the above detailed description. In general, in the appended claims, the terms used should not be interpreted as limiting the claims to the specific embodiments disclosed in the specification and claims, but should be interpreted to include all possible embodiments and the full range of equivalents to which such claims are entitled. Therefore, the claims are not limited by the present disclosure.
Claims
1. A device comprising: a polycrystalline silicon carbide (SiC) wafer comprising a first side and a second side opposite the first side; a first density at a first side of the polycrystalline silicon carbide (SiC) wafer; a second density at a second side of the polycrystalline silicon carbide (SiC) wafer, the second density being greater than the first density; and A density gradient between the first side and the second side increases in density in a density gradient direction pointing from the first side to the second side of the polycrystalline silicon carbide (SiC) wafer.
2. The apparatus of claim 1, wherein the polycrystalline silicon carbide (SiC) wafer further comprises a silicon carbide layer having a thickness of less than 5 angstroms at the second side. The roughness of the surface.
3. The apparatus of claim 1, wherein the resistivity at the second side of the polycrystalline silicon carbide (SiC) wafer is less than or equal to 20 milliohm centimeters (mohm-cm).
4. The apparatus of claim 1, wherein the resistivity at the second side of the polycrystalline silicon carbide (SiC) wafer is less than 20 milliohm centimeters (mohm-cm).
5. The apparatus of claim 1, further comprising a thickness extending from the first side to the second side of the polycrystalline silicon carbide (SiC) wafer, and the thickness is less than or equal to 800 micrometers (μm).
6. The apparatus of claim 1, further comprising a single crystal silicon carbide (SiC) layer coupled to the second side of the polycrystalline silicon carbide (SiC) wafer.
7. The apparatus of claim 6, wherein: The polycrystalline silicon carbide (SiC) wafer has a first thickness extending from the first side to the second side; as well as The single crystal silicon carbide (SiC) layer comprises: a surface facing away from the polycrystalline silicon carbide (SiC) wafer; as well as A second thickness extends from the second side to a surface of the single crystal silicon carbide (SiC) layer, and the second thickness is less than the first thickness.
8. The device of claim 7, wherein the second thickness is less than or equal to 1 micrometer (μm).
9. The apparatus of claim 8, wherein the first thickness is less than or equal to 800 micrometers (μm).
10. A method comprising: forming a polycrystalline silicon carbide (SiC) substrate; After forming the polycrystalline silicon carbide (SiC) substrate, generating a density gradient between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite to the first side by stimulating mass transport directed in a mass transport direction directed from a first side of the polycrystalline silicon carbide base substrate toward a second side opposite to the first side, the stimulating mass transport comprising: exposing the first side of the polycrystalline silicon carbide (SiC) substrate to a first temperature that transports mass away from the first side of the polycrystalline silicon carbide (SiC) substrate; exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a second temperature that transfers mass toward the second side of the polycrystalline silicon carbide (SiC) substrate, the second temperature being less than the first temperature; and The polycrystalline silicon carbide (SiC) substrate is cooled to generate a first density on a first side of the polycrystalline silicon carbide (SiC) substrate, a second density greater than the first density on a second side of the polycrystalline silicon carbide (SiC) substrate, and a density gradient between the first side and the second side of the polycrystalline silicon carbide (SiC) substrate.
11. The method of claim 10, wherein forming the polycrystalline silicon carbide (SiC) substrate comprises sintering at least one of: Silicon carbide (SiC) powder; and A powdered mixture of silicon (Si) and carbon (C).
12. The method of claim 10, wherein the second temperature is greater than or equal to 2000 degrees Celsius.
13. The method of claim 12, wherein the first temperature is less than or equal to 2000 degrees Celsius.
14. The method of claim 10, wherein the first temperature is equal to 2000 degrees Celsius and the second temperature is greater than or equal to 2100 degrees Celsius.
15. The method of claim 10, further comprising coupling a single crystal silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) base substrate.
16. The method of claim 10, wherein the density gradient increases in a mass transport direction directed from the first side to the second side of the polycrystalline silicon carbide (SiC) substrate.
17. A method comprising: Generating a density gradient between a first side of a polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side, generating a density gradient between the first side and the second side comprising: The second side of the polycrystalline silicon carbide (SiC) substrate is exposed to a chemical vapor deposition process to infuse silicon (Si) and carbon (C) into the second side of the polycrystalline silicon carbide (SiC) substrate.
18. The method of claim 17, further comprising coupling a single crystal silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) substrate.
19. The method of claim 17, further comprising: Before generating a density gradient between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate, the polycrystalline silicon carbide (SiC) substrate is formed by sintering at least one of: Silicon carbide (SiC) powder; and A powdered mixture of silicon (Si) and carbon (C).
20. The method of claim 17, wherein the density gradient increases in a density gradient direction away from a first side of the polycrystalline silicon carbide (SiC) substrate and toward a second side of the polycrystalline silicon carbide (SiC) substrate.