Preparation method of knittable perovskite quantum dot luminescent fiber

The batch preparation of perovskite quantum dot fluorescent fibers through the melting method solves the problems of organic solvent waste disposal and low spinning efficiency, achieves efficient, stable, and low-cost production of perovskite fluorescent fibers, and promotes its application in wearable devices. Applications in the fields of flexible display and anti-counterfeiting.

CN118727174APending Publication Date: 2024-10-01ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957296.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing perovskite fluorescent fiber preparation process has problems with organic solvent waste liquid treatment and low spinning efficiency, which limits its industrial application and promotion.

Method used

Perovskite quantum dot fluorescent fibers are prepared in batches using a melting method. Through melt extrusion and melt spinning of polymer perovskite quantum dot pellets, perovskite quantum dots with uniform color, no impurities, and high stability are obtained. Fluorescent fiber requires no solvent in the entire process, achieving 100% raw material utilization.

Benefits of technology

It has achieved high efficiency and batch preparation of high-quality perovskite quantum dot fluorescent fibers. It has high stability and will not show obvious fluorescence performance degradation for more than 200 days, reducing production costs. The process is all solid-state, low-cost, green and environmentally friendly. Suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727174A_ABST
    Figure CN118727174A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of semiconductor luminescent materials, and particularly relates to a preparation method of a knittable perovskite quantum dot luminescent fiber. Polymer perovskite quantum dot fluorescent powder is sequentially subjected to melt extrusion, water-cooling solidification and cutting, and polymer perovskite quantum dot granules are obtained; and carrying out melt spinning on the polymer perovskite quantum dot granules to obtain the perovskite quantum dot fluorescent fiber. The perovskite quantum dot fluorescent fiber prepared by adopting a melting method in a batch and high-efficiency manner is uniform in color, free of impurities and high in stability, obvious fluorescence property degradation does not occur after the perovskite quantum dot fluorescent fiber is stored for 200 days or above in an air environment, inert gas protection and solvent purification are not needed in the preparation process, loss is reduced, the raw material utilization rate can be 100%, and the preparation method is suitable for industrial production. No organic solvent waste is generated, and the method is an all-solid-state, low-cost, high-yield, green and environment-friendly method for preparing the perovskite quantum dot fluorescent fiber on a large scale, and has great development value and commercial prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor light-emitting materials, and in particular relates to a method for preparing a braidable perovskite quantum dot light-emitting fiber. Background Art

[0002] Light-emitting electronic devices have gradually evolved from rigid to flexible. Smart light-emitting devices that fit the human body will become an important human-machine interface in the new generation of flexible electronic devices. Since the organism is soft, complex and dynamic, the mechanical properties of these light-emitting devices must match those of the human body. In order to meet this demand, it is necessary to vigorously develop the preparation technology of high-quality light-emitting fibers. Metal halide perovskite quantum dot materials have become the representative of the new generation of high-quality semiconductor light-emitting materials due to their high fluorescence quantum efficiency, full visible spectrum adjustment range, and easy preparation. They have great potential in the preparation of high-quality fluorescent fibers. At present, the processes for preparing perovskite fluorescent fibers mainly include microfluidic electrospinning technology (R.Cheng, Z.B.Liang, H.Shen, et al., In-situ synthesis of stable perovskite quantum dots in core-shell nanofibers via microfluidic electrospinning, Chin.Chem.Lett.2023,34(3),107384) and microfluidic nano-air jet spinning technology (Cheng, R.; Liang, Z.B.; Zhu, L.; Li, H.; Zhang, Y.; Wang, CF; Chen, S.Fibrous Nanoreactors from Microfluidic Blow Spinning for Mass Production of Highly Stable Ligand-Free Perovskite Quantum Dots.Angew.Chem.Int.Ed.2022,61,e202204371), these technologies can realize the continuous preparation of fluorescent fibers, but they will face the problems of waste liquid treatment of organic solvents and low spinning efficiency during industrial production, which limits their application and promotion in industrialization. Summary of the invention

[0003] In view of this, the object of the present invention is to provide a method for preparing a braidable perovskite quantum dot luminescent fiber, which can efficiently and batch-produce perovskite quantum dot fluorescent fibers with uniform color, no impurities and high stability. The raw materials used in this method are all solid, no solvent is used, and no organic waste liquid is generated.

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing a braidable perovskite quantum dot luminescent fiber, comprising the following steps:

[0006] The polymer perovskite quantum dot phosphor powder is sequentially melt-extruded, water-cooled solidified and cut to obtain polymer perovskite quantum dot pellets;

[0007] The polymer perovskite quantum dot pellets are melt-spun to obtain perovskite quantum dot fluorescent fibers.

[0008] Preferably, the polymer perovskite quantum dot phosphor is obtained by mixing cesium stearate, lead stearate, octylamine, an organic halide salt and a polymer.

[0009] Preferably, the polymer includes one or more of polyethylene, polypropylene, polystyrene, polymethyl methacrylate and polyurethane.

[0010] Preferably, the temperature of the melt extrusion is 160-300°C.

[0011] Preferably, the melt extrusion rate is 5 to 15 mm / s.

[0012] Preferably, the melt spinning temperature is 160-300°C.

[0013] Preferably, the melt spinning rate is 2 to 10 mm / s.

[0014] Preferably, the melt spinning pressure is 25-30 kPa.

[0015] Preferably, the organic halide salt comprises an organic bromide salt and / or an organic chloride salt.

[0016] Preferably, the mixing is carried out under stirring conditions; the stirring rate is 5000-10000 rpm; and the mixing time is 3-5 min.

[0017] The invention provides a method for preparing a braidable perovskite quantum dot luminescent fiber, comprising the following steps: sequentially performing melt extrusion, water cooling solidification and cutting on a polymer perovskite quantum dot phosphor powder to obtain a polymer perovskite quantum dot granule; and performing melt spinning on the polymer perovskite quantum dot granule to obtain a perovskite quantum dot fluorescent fiber.

[0018] The perovskite quantum dot fluorescent fiber prepared in batches and with high efficiency by the present invention has uniform color, is free of impurities, has high stability, is stored in an air environment for more than 200 days without obvious fluorescence performance decay, and does not require inert gas protection or solvent purification during the preparation process. All raw materials used are solid, which reduces losses and can achieve 100% raw material utilization. No organic solvent waste is generated. The present invention is a full-solid-state, low-cost, high-yield, green and environmentally friendly method for large-scale preparation of perovskite quantum dot fluorescent fibers, and has great development value and commercial prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a photo of the polymer perovskite quantum dot pellets prepared in Example 1 under sunlight;

[0020] Figure 2 This is a photo of the polymer perovskite quantum dot pellets prepared in Example 1 under ultraviolet light;

[0021] Figure 3 This is a fluorescence spectrum of the perovskite quantum dot fluorescent fiber prepared in Example 1;

[0022] Figure 4 This is a real photo of the perovskite quantum dot fluorescent fiber prepared in Example 2;

[0023] Figure 5 This is the fluorescence spectrum of the perovskite quantum dot fluorescent fiber prepared in Comparative Example 1;

[0024] Figure 6 The fluorescence spectra of the perovskite quantum dot fluorescent fibers prepared in Example 1 and Comparative Example 2 are shown. DETAILED DESCRIPTION

[0025] The present invention provides a method for preparing a braidable perovskite quantum dot luminescent fiber, comprising the following steps:

[0026] The polymer perovskite quantum dot phosphor powder is sequentially melt-extruded, water-cooled solidified and cut to obtain polymer perovskite quantum dot pellets;

[0027] The polymer perovskite quantum dot pellets are melt-spun to obtain perovskite quantum dot fluorescent fibers.

[0028] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used in the preparation, and commercially available products known to those skilled in the art can be used.

[0029] The present invention sequentially performs melt extrusion, water cooling solidification and cutting on polymer perovskite quantum dot fluorescent powder to obtain polymer perovskite quantum dot granules.

[0030] In the present invention, the polymer perovskite quantum dot phosphor is preferably obtained by mixing cesium stearate, lead stearate, octylamine, an organic halide and a polymer. Octylamine, as a ligand on the surface of quantum dots, can passivate the surface of perovskite quantum dots and improve the luminescence efficiency of quantum dots.

[0031] In the present invention, the polymer preferably includes one or more of polyethylene (PE), polypropylene (PP), polystyrene (PS), polymethyl methacrylate (PMMA) and polyurethane (TPU), and is more preferably polyethylene (PE); the polymer is preferably a polymer powder; the particle size of the polymer powder is preferably 10 to 30 μm, and is more preferably 20 μm; the organic halide salt preferably includes an organic bromide salt and / or an organic chloride salt, and is more preferably an organic bromide salt; the organic bromide salt preferably includes one or more of tetraoctylammonium bromide, tetraphenylphosphonium bromide, oleylamine bromide and pyridinium tribromide, and is more preferably pyridinium tribromide. ; The organic chloride salt preferably includes tetraoctylammonium chloride and / or oleylamine chloride, more preferably oleylamine chloride; the mass ratio of cesium stearate to lead stearate is preferably 1:(1-4), more preferably 1:(1-3); the mass ratio of cesium stearate to octylamine is preferably (7-9):10, more preferably (7-8):10; the mass ratio of cesium stearate to organic halide salt is preferably (5-7):8, more preferably (5-6):8; the mass ratio of cesium stearate to polymer is preferably (0.5-3):(25-100), more preferably (0.5-1):(50-100), and most preferably 0.6:100. When there are multiple types of organic halide salts, the present invention has no special restrictions on the ratio of different types of organic halide salts, and any ratio can be used.

[0032] In the present invention, the mixing is preferably carried out under stirring conditions; the stirring rate is preferably 5000-10000 rpm, more preferably 6000-9000 rpm; the mixing time is preferably 3-5 min, more preferably 4-5 min; the mixing is preferably carried out in an atmospheric environment; the equipment used for the mixing is preferably a mixer.

[0033] The present invention uses polymer particles as a dispersion carrier of the perovskite material, and an ultra-high-speed mechanical stirring rotor provides a driving force for the reaction, thereby successfully synthesizing a perovskite quantum dot phosphor with uniform morphology and high-efficiency luminescence.

[0034] In the present invention, the temperature of the melt extrusion is preferably 160-300°C, more preferably 200-280°C; the rate of the melt extrusion is preferably 5-15 mm / s, more preferably 7-10 mm / s; the melt extrusion is preferably carried out in an atmospheric environment at a first room temperature; the first room temperature is preferably 10-30°C, more preferably 20-25°C; the melt extrusion equipment is preferably a melt extruder.

[0035] After obtaining the polymer perovskite quantum dot granules, the present invention performs melt spinning on the polymer perovskite quantum dot granules to obtain perovskite quantum dot fluorescent fibers.

[0036] In the present invention, the temperature of the melt spinning is preferably 160-300°C, more preferably 200-270°C; the rate of the melt spinning is preferably 2-10 mm / s, more preferably 4-6 mm / s; the pressure of the melt spinning is preferably 25-30 kPa, more preferably 25-28 kPa; the melt spinning is preferably carried out in an atmospheric environment at a second room temperature; the second room temperature is preferably 10-20°C, more preferably 15-20°C.

[0037] In the present invention, the diameter of the perovskite quantum dot fluorescent fiber is preferably 30 to 80 μm, and more preferably 50 to 60 μm.

[0038] The present invention utilizes melt extrusion for granulation, and then utilizes melt spinning equipment to further process the polymer perovskite quantum dot pellets into fluorescent fibers that can be used for textiles, and utilizes the rich surface environment of the polymer to ensure the uniform dispersion of the perovskite quantum dots in the solid phase, effectively avoiding fluorescence quenching caused by aggregation; and utilizes melt spinning technology to prepare multiple strands of fluorescent fibers at one time, which can effectively avoid the use of organic solvents. The present invention does not produce any organic solvent waste, and can quickly prepare highly luminous perovskite quantum dot fluorescent fibers in large quantities. It is an all-solid-state, low-cost, room temperature, large-scale, high-efficiency, green and environmentally friendly preparation method, which can promote the application of perovskite quantum dot materials in the fields of wearable flexible display, anti-counterfeiting, etc. This method can realize the preparation of fluorescent fibers in the red, green and blue bands by regulating the composition of halogens in polymer perovskite quantum dot phosphors, and has a high prospect for commercial application.

[0039] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.

[0040] Example 1

[0041] 0.6 g of cesium stearate, 2.0 g of lead stearate, 0.78 g of octylamine, 0.85 g of an organic halide salt (specifically pyridinium tribromide), and 100 g of polyethylene (PE) powder were stirred in an atmospheric environment at 10,000 rpm for 5 min by a mixer, and fully mixed to obtain a polymer perovskite (CsPbBr3) quantum dot phosphor.

[0042] In an atmospheric environment at room temperature of 20° C., the perovskite quantum dot phosphor is added into a melt extruder, and melt extruded at 160° C. at a rate of 10 mm / s, and then the extruded polymer perovskite composite material is solidified by water cooling, and finally cut into polymer perovskite quantum dot pellets;

[0043] The polymer perovskite quantum dot pellets were added to a melt spinning device, the device temperature was controlled to be 160°C, the melt spinning pressure was 25 kPa, the atmospheric temperature was adjusted to be 20°C, and melt spinning was performed at a rate of 6 mm / s to obtain perovskite quantum dot fluorescent fibers (with a diameter of 50 μm).

[0044] Example 2

[0045] The difference from Example 1 is that the polyethylene (PE) powder in Example 1 is replaced by polypropylene (PP) powder.

[0046] Example 3

[0047] The difference from Example 1 is that the polyethylene (PE) powder in Example 1 is replaced by polystyrene (PS) powder.

[0048] Example 4

[0049] The difference from Example 1 is that the organic halide salt in Example 1 is replaced by a mixture of oleylamine bromide and oleylamine chloride in a mass ratio of 1:1.

[0050] Comparative Example 1

[0051] The difference from Example 1 is that the polyethylene (PE) powder in Example 1 is not used.

[0052] Comparative Example 2

[0053] The difference from Example 1 is that the pyridinium tribromide in Example 1 is replaced by didodecyl dimethyl ammonium bromide.

[0054] Performance Testing

[0055] Figure 1 This is a photo of the polymer perovskite quantum dot granules prepared in Example 1 under sunlight. Figure 1 It can be seen that the composite material of perovskite quantum dots and polymer prepared in the present invention has uniform color and is free of impurities, which is mainly attributed to the fact that the perovskite quantum dots can be well dispersed on the surface of the polymer medium, significantly reducing the occurrence of quantum dot agglomeration.

[0056] Figure 2 This is a photo of the polymer perovskite quantum dot granules prepared in Example 1 under ultraviolet light. As can be seen from the figure, the composite material of the perovskite quantum dots and the polymer prepared in the present invention exhibits bright green fluorescence.

[0057] Figure 3 This is a fluorescence spectrum of the perovskite quantum dot fluorescent fiber prepared in Example 1. As can be seen from the figure, the wavelength of the perovskite quantum dot fluorescent fiber prepared in the present invention is 525nm, with a narrow emission half-peak width.

[0058] Figure 4 This is a real photo of the perovskite quantum dot fluorescent fiber prepared in Example 2. As can be seen from the figure, the present invention can realize the batch preparation of perovskite quantum dot fluorescent fibers, proving that the invention has considerable industrial prospects.

[0059] Figure 5 This is a fluorescence spectrum of the perovskite quantum dot fluorescent fiber prepared in Comparative Example 1. It can be seen from the figure that the emission peak of the perovskite quantum dot fluorescent fiber prepared without using polyethylene (PE) powder is asymmetric, and the perovskite quantum dot fluorescent fiber cannot be formed.

[0060] Figure 6 The fluorescence spectra of the perovskite quantum dot fluorescent fibers prepared in Example 1 and Comparative Example 2 are shown in FIG. As can be seen from the figure, compared with Example 1, the luminescence spectrum of the perovskite quantum dot fluorescent fibers prepared in Comparative Example 2 is blue-shifted, and the emission intensity is lower. In the subsequent spinning process, the sample of Comparative Example 2 is unstable and loses fluorescence after heating, so the formed perovskite quantum dot fibers do not have fluorescent properties.

[0061] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a braidable perovskite quantum dot luminescent fiber, characterized in that: The following steps are involved: The polymer perovskite quantum dot phosphor powder is sequentially melt-extruded, water-cooled solidified and cut to obtain polymer perovskite quantum dot pellets; The polymer perovskite quantum dot pellets are melt-spun to obtain perovskite quantum dot fluorescent fibers.

2. The preparation method according to claim 1, characterized in that: The polymer perovskite quantum dot fluorescent powder is obtained by mixing cesium stearate, lead stearate, octylamine, organic halogen salt and polymer.

3. The preparation method according to claim 2, characterized in that: The polymer includes one or more of polyethylene, polypropylene, polystyrene, polymethyl methacrylate and polyurethane.

4. The preparation method according to claim 1, characterized in that: The temperature of the melt extrusion is 160-300°C.

5. The preparation method according to claim 1, characterized in that: The melt extrusion rate is 5 to 15 mm / s.

6. The preparation method according to claim 1, characterized in that: The temperature of the melt spinning is 160-300°C.

7. The preparation method according to claim 1, characterized in that: The melt spinning rate is 2-10 mm / s.

8. The preparation method according to claim 1, characterized in that: The melt spinning pressure is 25-30 kPa.

9. The preparation method according to claim 2, characterized in that: The organic halide salt includes an organic bromide salt and / or an organic chloride salt.

10. The preparation method according to claim 2, characterized in that: The mixing is carried out under stirring conditions; the stirring rate is 5000-10000 rpm; and the mixing time is 3-5 min.