A high-strength para-aramid fiber and preparation method thereof

Through calcium chloride pretreatment and titanate modification, combined with hot and cold alternating water washing and drafting, the problem of insufficient mechanical properties of para-aramid fibers is solved, and high-strength and high-stability fiber preparation is achieved, simplifying the production process .

CN118727433BActive Publication Date: 2024-11-22TAYHO ADVANCED MATERIALS GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222991.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The prior art is difficult to stabilize the production of high-strength para-aramid fibers, and the preparation methods are complicated and they fail to effectively improve their mechanical properties.

Method used

The para-aramid fibers are treated with calcium chloride pretreatment and titanate modification, and the alternating methods of hot water washing and cold water washing are promoted to promote more orderly molecular orientation and structural denseness, and improve grain orientation.

Benefits of technology

High-strength para-aramid fiber with excellent mechanical properties was obtained, with tensile strength ≥24.00cN/dtex, elongation of break of 3.5%-3.8%, and the preparation process was simplified, which was suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727433B_ABST
    Figure CN118727433B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of chemical fiber production, and specifically to a high-strength para-aramid fiber and a preparation method thereof, wherein the preparation method comprises the following steps: S1, placing the washed para-aramid fiber in a calcium chloride ethanol solution, and heating it for pretreatment; S2, placing the para-aramid fiber pretreated in step S1 in a titanate ethanol solution, and performing a sufficient reaction. After the reaction is completed, washing is performed to obtain the modified para-aramid fiber; S3, the para-aramid fiber modified in step S2 is sequentially subjected to hot water washing and cold water washing and stretching, and finally drying to obtain the high-strength para-aramid fiber. The preparation method can promote the molecular orientation of the para-aramid fiber to be more orderly, the structure to be more compact, and the degree of grain orientation to be improved, and finally obtain the high-strength para-aramid fiber with excellent mechanical properties, and the preparation method of the high-strength para-aramid fiber is simple and more suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-strength para-aramid fiber and a preparation method thereof, belonging to the technical field of chemical fiber production. Background Art

[0002] Para-aramid fiber, also known as poly(p-phenylene terephthalamide) fiber or aramid 1414, is a high-performance synthetic fiber. Para-aramid is obtained by polycondensing para-phenylenediamine and terephthaloyl chloride through low-temperature solution to obtain PPTA polymer, which is then dissolved in concentrated sulfuric acid and spun into para-aramid fiber by dry-jet wet spinning. Since the molecular chain of para-aramid fiber is rigid and lyotropic liquid crystal, para-aramid fiber is known for its high strength, high modulus, heat resistance, chemical corrosion resistance, high insulation and low density, and is widely used in a wide range of applications, including but not limited to bulletproof materials, tire cords, insulation paper, optical cables, composite materials, friction sealing materials, etc.

[0003] Chinese patent application CN109183177A discloses a high-strength and high-modulus para-aramid fiber and its preparation method and application. The para-aramid fiber is obtained by compounding sodium pyruvate, ferric acetylacetonate and sodium tripolyphosphate, and then modifying the para-aramid fiber. However, the preparation method requires the treated para-aramid fiber to be dissolved in concentrated sulfuric acid again and spun again, and the preparation process is relatively complicated. In addition, there is currently a technical blockade and embargo on KM2-grade high-strength para-aramid fiber abroad, and my country does not have the ability to stably produce high-strength para-aramid fibers. Therefore, there is an urgent need to develop a stable preparation method for high-strength para-aramid fibers. Summary of the invention

[0004] The present invention aims at the deficiencies in the prior art and provides a high-strength para-aramid fiber and a preparation method thereof. The preparation method can promote the molecular orientation of the para-aramid fiber to be more orderly, the structure to be more compact, and the grain orientation to be improved, thereby finally obtaining a high-strength para-aramid fiber with excellent mechanical properties.

[0005] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing high-strength para-aramid fiber, the preparation method comprising:

[0006] S1, placing the cleaned para-aramid fiber in a calcium chloride ethanol solution and heating it for pretreatment;

[0007] S2, placing the para-aramid fiber pretreated in step S1 in a titanate ethanol solution for sufficient reaction, and after the reaction is completed, washing to obtain the modified para-aramid fiber;

[0008] S3, washing and stretching the para-aramid fiber modified in step S2 with hot water and cold water in sequence, and finally drying to obtain the high-strength para-aramid fiber.

[0009] Furthermore, before the pretreatment, the para-aramid fiber is firstly cleaned, and the cleaning process is as follows: the para-aramid fiber is extracted in acetone to remove dirt on the fiber surface, washed with distilled water, and dried to obtain cleaned para-aramid fiber.

[0010] Furthermore, in step S1, the mass concentration of calcium chloride in the calcium chloride ethanol solution is 1-10%.

[0011] Furthermore, in step S1, the heating temperature of the pretreatment is 70-80°C, and the heating time of the pretreatment is 3-6 hours.

[0012] Furthermore, in step S2, the mass concentration of phthalate in the titanate ethanol solution is 2-20%.

[0013] Preferably, the phthalate in the titanate ethanol solution is neoalkoxy tris(dioctyl phosphate acyloxy) titanate, and the mass concentration of neoalkoxy tris(dioctyl phosphate acyloxy) titanate in the titanate ethanol solution is 3%.

[0014] Furthermore, the reaction time of step S2 is 1-6 hours. After the reaction is completed, ethanol and deionized water are used for washing to obtain the modified para-aramid fiber.

[0015] Further, in step S3, the temperature of the hot water drawing is 30-60°C, and the drawing ratio of the hot water drawing is 2.5-3.5; the temperature of the cold water drawing is 10-30°C, and the drawing ratio of the cold water drawing is 0.98-1.35;

[0016] The temperature difference between the hot water washing and drawing and the cold water washing and drawing is not less than 15°C.

[0017] Furthermore, the drying temperature of step S3 is 200-350°C.

[0018] The present invention discloses a high-strength para-aramid fiber. The high-strength para-aramid fiber is prepared by the preparation method of the present invention. The tensile strength of the high-strength para-aramid fiber is ≥24.00 cN / dtex and the elongation at break is 3.5%-3.8%.

[0019] The beneficial effects of the present invention are:

[0020] The preparation method of the present invention first pre-treats the p-aramid fiber with calcium chloride, then modifies the surface of the p-aramid fiber with titanate, and then uses hot and cold alternating drafting and water washing to promote more orderly molecular orientation, more compact structure, and improve grain orientation, and finally obtain high-strength p-aramid fiber with excellent mechanical properties. The tensile strength of the high-strength p-aramid fiber is ≥24.00 cN / dtex, and the elongation at break is 3.5%-3.8%.

[0021] The preparation method of the high-strength para-aramid fiber of the present invention is simple and does not require re-spinning. The high-strength para-aramid fiber can be obtained by pretreating the para-aramid fiber, modifying its surface, and stretching and washing it in an alternating hot and cold manner. There is no need to change the conventional para-aramid fiber spinning process method, which is more conducive to industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a process flow chart of the method for preparing high-strength para-aramid fiber of the present invention;

[0023] Figure 2 This is a comparison chart of the tensile strength of the high-strength para-aramid fiber obtained in Examples 1-5 and the para-aramid fiber raw material in Comparative Example 1. DETAILED DESCRIPTION

[0024] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.

[0026] like Figure 1 As shown, a method for preparing high-strength para-aramid fiber, the preparation method is:

[0027] S1, placing the cleaned para-aramid fiber in a calcium chloride ethanol solution and heating it for pretreatment;

[0028] S2, placing the para-aramid fiber pretreated in step S1 in a titanate ethanol solution for sufficient reaction, and after the reaction is completed, washing to obtain the modified para-aramid fiber;

[0029] S3, washing and stretching the para-aramid fiber modified in step S2 with hot water and cold water in sequence, and finally drying to obtain the high-strength para-aramid fiber.

[0030] Specifically, before the pretreatment, the para-aramid fiber is firstly cleaned, and the cleaning process is as follows: the para-aramid fiber is extracted in acetone to remove dirt on the fiber surface, washed with distilled water, and dried to obtain the cleaned para-aramid fiber.

[0031] More specifically, the para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber.

[0032] More specifically, the para-aramid fiber used in the embodiment of the present invention is Tayho.

[0033] Specifically, in step S1, the mass concentration of calcium chloride in the calcium chloride ethanol solution is 1-10%.

[0034] Specifically, in step S1, the heating temperature of the pretreatment is 70-80° C., and the heating time of the pretreatment is 3-6 hours.

[0035] Preferably, the heating temperature of the pretreatment is 80° C. At 80° C., the calcium chloride ethanol solution will boil, and boiling can replace mechanical stirring to promote the pretreatment reaction.

[0036] Specifically, in step S2, the mass concentration of phthalate in the titanate ethanol solution is 2-20%.

[0037] Preferably, the phthalate in the titanate ethanol solution is neoalkoxy tris(dioctyl phosphate acyloxy) titanate, and the mass concentration of neoalkoxy tris(dioctyl phosphate acyloxy) titanate in the titanate ethanol solution is 3%.

[0038] Specifically, the reaction time of step S2 is 1-6 hours. After the reaction is completed, ethanol and deionized water are used for washing to obtain the modified para-aramid fiber.

[0039] Specifically, in step S3, the temperature of the hot water drawing is 30-60°C, and the drawing ratio of the hot water drawing is 2.5-3.5; the temperature of the cold water drawing is 10-30°C, and the drawing ratio of the cold water drawing is 0.98-1.35;

[0040] The temperature difference between the hot water washing and drawing and the cold water washing and drawing is not less than 15°C.

[0041] Specifically, the drying temperature of step S3 is 200-350°C.

[0042] A high-strength para-aramid fiber is prepared by adopting the preparation method of the present invention. The high-strength para-aramid fiber has a tensile strength of ≥24.00 cN / dtex and an elongation at break of 3.5%-3.8%.

[0043] Example 1

[0044] Preparation of a high-strength para-aramid fiber:

[0045] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0046] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0047] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0048] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 60°C deionized water with a drawing ratio of 2.70; the cold water washing is 20°C deionized water with a drawing ratio of 1.05; and finally, the fiber is dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0049] Example 2

[0050] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0051] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0052] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 1%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0053] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 60°C deionized water with a drawing ratio of 2.70; the cold water washing is 20°C deionized water with a drawing ratio of 1.05; and finally, the fiber is dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0054] Example 3

[0055] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0056] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0057] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 2%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0058] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 60°C deionized water with a drawing ratio of 2.70; the cold water washing is 20°C deionized water with a drawing ratio of 1.05; and finally, the fiber is dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0059] Example 4

[0060] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0061] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0062] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 4%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0063] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 60°C deionized water with a drawing ratio of 2.70; the cold water washing is 20°C deionized water with a drawing ratio of 1.05; and finally, the fiber is dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0064] Example 5

[0065] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0066] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0067] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 5%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0068] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 60°C deionized water with a drawing ratio of 2.70; the cold water washing is 20°C deionized water with a drawing ratio of 1.05; and finally, the fiber is dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0069] Example 6

[0070] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0071] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 10%, and setting aside; then placing the cleaned para-aramid fiber into the 10% calcium chloride ethanol solution, and heating it in a 75° C. water bath for 3 hours to obtain pretreated para-aramid fiber;

[0072] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 20%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 1 hour, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0073] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 30°C deionized water with a drawing ratio of 2.5; the cold water washing is 10°C deionized water with a drawing ratio of 0.98; and finally, the fiber is dried at a drying temperature of 300°C to obtain high-strength para-aramid fiber.

[0074] Example 7

[0075] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0076] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 1%, and setting aside; then placing the cleaned para-aramid fiber into the 1% calcium chloride ethanol solution, and heating it in a 70° C. water bath for 6 hours to obtain pretreated para-aramid fiber;

[0077] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 10%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 6 hours, and then washing with ethanol and deionized water to obtain modified para-aramid fiber;

[0078] (4) The modified para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 45°C deionized water with a drawing ratio of 3.5; the cold water washing is 30°C deionized water with a drawing ratio of 1.35; and finally, the fiber is dried at a drying temperature of 350°C to obtain high-strength para-aramid fiber.

[0079] Comparative Example 1

[0080] The 1000D para-aramid fiber without modification was tested, that is, the para-aramid fiber raw material used in each example.

[0081] Comparative Example 2

[0082] The high-strength para-aramid fiber was prepared by the same method as in Example 1, except that no pretreatment operation was performed in this comparative example 2, and no hot water washing and drawing and cold water washing and drawing were performed. The specific operation process is as follows:

[0083] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0084] (2) Neoalkoxy tri(dioctylphosphoyl) titanate was dissolved in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, and the cleaned para-aramid fiber was immersed in the titanate ethanol solution for 2 h, then washed with ethanol and deionized water to obtain the modified para-aramid fiber, and finally dried at a drying temperature of 200 °C to obtain a high-strength para-aramid fiber.

[0085] Comparative Example 3

[0086] The high-strength para-aramid fiber was prepared by the same method as in Example 1, except that no hot water washing and drawing and cold water washing and drawing were performed in this comparative example 3. The specific operation process is as follows:

[0087] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0088] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0089] (3) Dissolve neoalkoxy tri(dioctylphosphoyl) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, soak the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, then wash with ethanol and deionized water to obtain the modified para-aramid fiber; finally, dry the fiber at a temperature of 200 °C to obtain a high-strength para-aramid fiber.

[0090] Comparative Example 4

[0091] The high-strength para-aramid fiber was prepared by the same method as in Example 1, except that: in step (3) of this comparative example 4, only one normal temperature water washing and drawing was performed. The specific operation process is as follows:

[0092] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0093] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0094] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0095] (4) The modified para-aramid fiber is washed with water at room temperature and stretched at the same time, with a stretching ratio of 1.50, and finally dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0096] Comparative Example 5

[0097] The high-strength para-aramid fiber was prepared by the same method as in Example 1, except that: in step (3) of this comparative example 4, only one hot water washing and drawing was performed. The specific operation process is as follows:

[0098] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0099] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0100] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0101] (4) The modified para-aramid fiber is washed and stretched by hot water, wherein the hot water is deionized water at 60°C and the stretching ratio is 2.70; finally, the fiber is dried at a drying temperature of 200°C to obtain a high-strength para-aramid fiber.

[0102] Comparative Example 6

[0103] The high-strength para-aramid fiber was prepared by the same method as in Example 1, except that no pretreatment operation was performed in this comparative example 6. The specific operation process is as follows:

[0104] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0105] (2) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, soaking the washed para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain a modified para-aramid fiber;

[0106] (3) The modified para-aramid fiber was sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing was performed with deionized water at 60°C and the drawing ratio was 2.70; the cold water washing was performed with deionized water at 20°C and the drawing ratio was 1.05; and finally, the fiber was dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0107] Comparative Example 7

[0108] The high-strength para-aramid fiber was prepared by the same method as in Example 1, except that no titanate modification operation was performed in this comparative example 7. The specific operation process is as follows:

[0109] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0110] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0111] (3) The pretreated para-aramid fiber is sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing is 60°C deionized water with a drawing ratio of 2.70; the cold water washing is 20°C deionized water with a drawing ratio of 1.05; and finally, the fiber is dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0112] Comparative Example 8

[0113] High-strength para-aramid fiber was prepared by the same method as in Example 1, except that: in this comparative example 8, the hot water drawing temperature was 30°C, the cold water drawing temperature was 25°C, and the temperature difference between the hot water drawing and the cold water drawing was 5°C (less than 15°C).

[0114] (1) The para-aramid fiber is extracted in acetone for 8 hours to remove dirt on the fiber surface, washed with distilled water, and dried at 60° C. to obtain washed para-aramid fiber;

[0115] (2) dissolving calcium chloride in ethanol to obtain a calcium chloride ethanol solution with a mass concentration of 5%, and setting aside; then placing the cleaned para-aramid fiber into the 5% calcium chloride ethanol solution, and heating it in a water bath at 80° C. for 4 hours to obtain pretreated para-aramid fiber;

[0116] (3) dissolving neoalkoxy tri(dioctylphosphoyloxy) titanate in ethanol to obtain a titanate ethanol solution with a mass concentration of 3%, soaking the pretreated para-aramid fiber in the titanate ethanol solution for 2 h, and then washing with ethanol and deionized water to obtain the modified para-aramid fiber;

[0117] (4) The modified para-aramid fiber was sequentially subjected to hot water washing and drawing and cold water washing and drawing, wherein the hot water washing was performed with deionized water at 30°C and the drawing ratio was 2.70; the cold water washing was performed with deionized water at 25°C and the drawing ratio was 1.05; and finally, the fiber was dried at a drying temperature of 200°C to obtain high-strength para-aramid fiber.

[0118] The performance of the para-aramid fibers obtained in the above examples and comparative examples was tested using GB / T 14344-2008 “Test method for tensile properties of chemical fiber filaments”. The results are shown in Table 1.

[0119] Table 1 Performance test results

[0120]

[0121] Note: The CV in Table 1 stands for coefficient of variation, which indicates the degree of dispersion.

[0122] From the above data, it can be seen that the para-aramid fibers prepared by the preparation method of the present invention in Examples 1-7 are compared with the performance test results of Comparative Example 1. It can be seen that the para-aramid fibers prepared by the preparation method of the present invention have stable performance, and the tensile strength of the para-aramid fibers is effectively improved, and the tensile strength is not less than 24.00 cN / dtex, which meets the requirements of high-strength para-aramid fibers for fiber strength. The present invention uses calcium chloride to pretreat para-aramid fibers, uses titanate to modify para-aramid fibers, and adopts a hot water washing and drawing and cold water washing and drawing alternately to obtain a high-strength para-aramid multifilament fiber.

[0123] From the data comparison of Comparative Example 1 and Comparative Examples 2-3, it can be seen that after calcium chloride pretreatment, chlorine atoms can provide more sites as a bridge between titanate and the surface of aramid fiber, thereby improving the modification effect of titanate, better improving the interface bonding strength between titanate and aramid fiber, and the breaking strength of 1110D para-aramid fiber is improved.

[0124] From the comparison of the data of Comparative Examples 4-5 and Example 1, it can be seen that the treatment method of alternating hot water washing and stretching and cold water washing and stretching is more conducive to improving the strength performance of the para-aramid fiber.

[0125] From the comparison of the data of Comparative Examples 6-7 and Example 1, it can be seen that if the calcium chloride pretreatment operation or the titanate modification operation is not performed during the preparation process, the strength performance of the para-aramid fiber will not be able to meet the index requirement of 24.00 cN / dtex high-strength para-aramid fiber. Therefore, the synergistic combination of calcium chloride pretreatment and titanate modification and the use of appropriate water washing and stretching operations are more conducive to obtaining high-strength para-aramid fibers.

[0126] From the data comparison between Comparative Example 8 and Example 1, it can be seen that if the temperature difference between hot water washing and drawing and cold water washing and drawing is too small, it is not conducive to improving the strength performance of the para-aramid fiber. Therefore, the hot water washing and drawing and cold water washing and drawing conditions specified in the present invention are more conducive to improving the performance of the para-aramid fiber.

[0127] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0128] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.

Claims

1. A method for preparing high-strength para-aramid fiber, characterized in that: The preparation method is: S1, placing the cleaned para-aramid fiber in a calcium chloride ethanol solution and heating it for pretreatment; S2, placing the para-aramid fiber pretreated in step S1 in a titanate ethanol solution for sufficient reaction, and after the reaction is completed, washing to obtain the modified para-aramid fiber; S3, sequentially washing and stretching the para-aramid fiber modified in step S2 with hot water and cold water, and finally drying to obtain the high-strength para-aramid fiber; The phthalate in the titanate ethanol solution is neoalkoxy tris(dioctylphosphoyloxy) titanate; In step S3, the temperature of the hot water drawing is 30-60°C, and the drawing ratio of the hot water drawing is 2.5-3.5; the temperature of the cold water drawing is 10-30°C, and the drawing ratio of the cold water drawing is 0.98-1.35; The temperature difference between the hot water washing and drawing and the cold water washing and drawing is not less than 15°C.

2. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: Before the pretreatment, the para-aramid fiber is firstly cleaned, and the cleaning process is as follows: the para-aramid fiber is extracted in acetone to remove dirt on the fiber surface, washed with distilled water, and dried to obtain the cleaned para-aramid fiber.

3. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: In step S1, the mass concentration of calcium chloride in the calcium chloride ethanol solution is 1-10%.

4. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: In step S1, the heating temperature of the pretreatment is 70-80°C, and the heating time of the pretreatment is 3-6 hours.

5. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: In step S2, the mass concentration of phthalate in the titanate ethanol solution is 2-20%.

6. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: The mass concentration of neoalkoxy tris(dioctylphosphoyloxy) titanate in the titanate ethanol solution is 3%.

7. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: The reaction time of step S2 is 1-6 hours. After the reaction is completed, ethanol and deionized water are used for washing to obtain the modified para-aramid fiber.

8. The method for preparing high-strength para-aramid fiber according to claim 1, characterized in that: The drying temperature of step S3 is 200-350°C.

9. A high-strength para-aramid fiber, characterized in that: The high-strength para-aramid fiber is prepared by the preparation method according to any one of claims 1 to 8, and the tensile strength of the high-strength para-aramid fiber is ≥24.00 cN / dtex, and the elongation at break is 3.5%-3.8%.