Outdoor high-weather-resistance leather cloth and preparation method thereof

The weather-resistant hydrophobic layer is prepared by combining materials such as modified polymethylphenylsiloxane resin and nano-titanium dioxide, which solves the problems of weather resistance and cleanability of traditional leather fabrics in outdoor environments, and achieves efficient hydrophobicity and UV resistance. Extended service life and reduced maintenance costs.

CN118727461APending Publication Date: 2024-10-01DONGGUAN YINGSHENG FIBER PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936700.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional leather fabrics are easily affected by bad weather in outdoor environments. The color fades, the texture becomes hard, the waterproof performance is weakened, and cleaning is difficult, affecting the service life and aesthetics.

Method used

A weather-resistant hydrophobic layer is prepared using a combination of modified polymethylphenylsiloxane resin, modified nano-titanium dioxide, side-containing hydrogen silicone oil, precipitated barium sulfate, coupling agent and catalyst to improve the weather resistance, hydrophobicity and UV resistance of leather cloth. And the self-cleaning function is enhanced by modified nano-titanium dioxide.

Benefits of technology

It achieves long-term weather resistance and hydrophobicity of leather cloth in outdoor environments, reduces maintenance costs, extends service life, and has a self-cleaning function.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of synthetic leather cloth, in particular to outdoor high-weather-resistance leather cloth and a preparation method thereof. The outdoor high-weather-resistance leather cloth comprises a leather cloth layer and a weather-resistant hydrophobic layer, and the weather-resistant hydrophobic layer comprises, by mass, 20-30 parts of a leather cloth layer, 20-30 parts of a weather-resistant hydrophobic layer, 20-30 parts of a waterproof layer, and 20-30 parts of a waterproof layer. Comprising the following preparation raw materials: 30 to 35 parts of modified polymethylphenylsiloxane resin, 15 to 20 parts of modified nano titanium dioxide, 30 to 32 parts of side hydrogen-containing silicone oil, 10 to 12 parts of precipitated barium sulfate, 1 to 1.5 parts of a coupling agent, 0.8 to 1.2 parts of an ultraviolet absorbent and 0.08 to 0.12 part of a catalyst. The outdoor high-weather-resistance leather cloth has the advantages of self-cleaning, high stability, long service life, environmental protection, safety and the like while the weather resistance, hydrophobicity and water resistance are improved, is very suitable for outdoor application occasions, and has a wide market application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of synthetic leather cloth, and in particular to a leather cloth with strong weather resistance for outdoor use and a preparation method thereof. Background Art

[0002] In outdoor environments, leather fabrics are often exposed to various adverse weather conditions, such as strong sunlight, rain, and wind. These conditions can cause the color of leather fabrics to fade, the texture to become hard, and even cracks to appear, seriously affecting their service life and aesthetics. Therefore, it is very important to develop a leather fabric with excellent weather resistance.

[0003] Traditional leather fabrics usually have only certain water resistance, but after long-term outdoor use, their water resistance will gradually weaken, resulting in reduced weather resistance of leather fabrics. In addition, traditional leather fabrics are also difficult to clean because their surfaces easily absorb dust and dirt and are difficult to clean. Summary of the invention

[0004] The purpose of the present application is to provide a weather-resistant leather cloth for outdoor use and a preparation method thereof in view of the deficiencies of the current technology. The novel weather-resistant leather cloth for outdoor use of the present application has excellent weather resistance, hydrophobicity and water resistance, so that it can maintain a good state for a long time in an outdoor environment. At the same time, since the bonding force between the weather-resistant hydrophobic layer and the leather cloth layer is very high, the performance of the leather cloth is very stable and not easy to fall off, thereby greatly improving its service life. In addition, the leather cloth also has a self-cleaning function, making it more convenient to clean.

[0005] In the first aspect, the present application provides a leather cloth with strong weather resistance for outdoor use, which adopts the following technical solution: A highly weather-resistant leather cloth for outdoor use comprises a leather cloth layer and a weather-resistant hydrophobic layer. The weather-resistant hydrophobic layer comprises the following raw materials by weight: 30-35 parts of modified polymethylphenylsiloxane resin, 15-20 parts of modified nano titanium dioxide, 30-32 parts of side hydrogenated silicone oil, 10-12 parts of precipitated barium sulfate, 1-1.5 parts of coupling agent, 0.8-1.2 parts of ultraviolet absorber and 0.08-0.12 parts of catalyst.

[0006] By adopting the above technical scheme, the modified polymethylphenylsiloxane resin is the main film-forming material of the weather-resistant hydrophobic layer and has certain hydrophobic properties. It mainly plays a role in increasing the surface smoothness and hydrophobic properties of the leather cloth. The role of the modified nano titanium dioxide is to significantly improve the weather resistance, hydrophobicity and water resistance of the leather cloth, and at the same time has a self-cleaning function. The side hydrogen-containing silicone oil and coupling agent play a role in enhancing the film-forming performance and increasing the weather resistance in the weather-resistant hydrophobic layer. Precipitated barium sulfate and ultraviolet absorber mainly play a role in improving the UV resistance and durability of the leather cloth. The catalyst is an important auxiliary component for accelerating the curing of the weather-resistant hydrophobic layer. When these raw materials are used in combination, they work synergistically with each other, so that the weather-resistant leather cloth has excellent performance. By adding modified nano titanium dioxide, the performance of the entire weather-resistant hydrophobic layer can be improved, and the dispersibility and compatibility of nano titanium dioxide with the matrix can be improved by modification, so that it has better stability and service life. Through the combined action of these components and the synergistic effect between them, the obtained outdoor weather-resistant leather cloth not only has excellent weather resistance, hydrophobicity and water resistance, but also has a self-cleaning function, and is very suitable for applications where it is used outdoors for a long time.

[0007] Preferably, the preparation method of the modified polymethylphenylsiloxane resin is as follows: methylphenyldichlorosilane, dimethyldichlorosilane and methyltrichlorosilane are added into a reactor with a separatory funnel, condensation reflux and vacuum in a substance ratio of 2:7:1 respectively, and a mixed diluent and isopropyl titanate catalyst are added under heating and magnetic stirring, and deionized water is added dropwise slowly after sufficient stirring, and the reaction is stirred at room temperature for 4 hours, and then the temperature is raised to 70-75°C and refluxed for 2-3 hours; finally, the low-boiling substances are removed under reduced pressure at 70°C and 1 kPa for 2-3 hours to obtain the modified polymethylphenylsiloxane resin.

[0008] By adopting the above technical scheme, the modified polymethylphenylsiloxane resin has good hydrophobic properties because its chemical structure contains hydrophobic methyl and phenyl groups. When used as a film-forming material for the weather-resistant hydrophobic layer, this resin can effectively prevent moisture penetration and keep the leather cloth dry. The structure of the resin provides good UV resistance, which can protect the leather cloth from degradation caused by ultraviolet radiation and extend the service life of the material. As a basic film-forming material, the modified polymethylphenylsiloxane resin forms a continuous film layer in the coating, providing a uniform and tight protective layer for the leather cloth. There is good adhesion between the resin and the leather cloth layer, which helps to improve the bonding strength between the weather-resistant hydrophobic layer and the leather cloth layer, ensuring that the coating will not fall off easily. The modified polymethylphenylsiloxane resin works together with modified nano titanium dioxide and other ingredients such as side hydrogen silicone oil to improve the overall performance of the coating. For example, combined with the hydrophobic properties of the side hydrogen silicone oil, the hydrophobicity and self-cleaning ability of the material are further improved. In summary, the modified polymethylphenylsiloxane resin prepared by the above method not only serves as the basic film-forming material of the weather-resistant hydrophobic layer, but also synergizes with other ingredients to jointly endow the leather cloth with excellent weather resistance, hydrophobicity, water resistance and self-cleaning functions.

[0009] Preferably, the mixed diluent is prepared by mixing tetraethoxysilane, butyl acetate and anhydrous ethanol in a molar ratio of 2:2:1.

[0010] Preferably, the usage ratio of the methyltrichlorosilane, the mixed diluent, the isopropyl titanate catalyst and the deionized water is 1 mol:6L:0.1 mol:(3-4) mol.

[0011] Preferably, the preparation method of the modified nano titanium dioxide comprises the following steps: S51. Fully mix hexamethyldisilazane, 3-aminopropyltrimethoxysilane, tetraethoxysilane and anhydrous ethanol according to their weight fractions to prepare a mixed modifier; S52. According to the mass proportions, 100 parts of nano titanium dioxide with a particle size of 20 nm and 200 parts of mixed modifier are fully mixed at room temperature for 30-40 minutes, ultrasonicated at room temperature for 1-2 hours, and then transferred into a vacuum mixer. The mixture is heated to 70-80°C and stirred under reflux conditions of -0.3 to -0.2 MPa for 4-5 hours. Finally, ethanol is removed under reduced pressure and the modified nano titanium dioxide is obtained after drying.

[0012] By adopting the above technical scheme, nano titanium dioxide is an effective ultraviolet absorber, which can absorb ultraviolet rays and reduce the photodegradation of leather cloth caused by UV, thereby improving the weather resistance of the material. Through the reaction with substances such as hexamethyldisilazane, 3-aminopropyltrimethoxysilane and tetraethoxysilane, the surface of nano titanium dioxide is modified to make it more hydrophobic. This helps the formation and rolling of water droplets on the surface of the leather cloth, thereby taking away dust and dirt. Due to the presence of modified nano titanium dioxide, the contact angle formed by water droplets on the surface of the material increases (more than 138.0°), making the leather cloth have a self-cleaning function. Rainwater scouring can easily remove surface pollution and reduce maintenance costs. Through surface modification, the compatibility and dispersibility of nano titanium dioxide in the weather-resistant hydrophobic layer are improved, thereby enhancing the stability and durability of the coating. The modified nano titanium dioxide can better combine with polymethylphenylsiloxane resin to form a uniform and continuous protective layer, improving the overall weather resistance and hydrophobicity. Nano-sized titanium dioxide particles are filled in the coating, which can effectively cover the leather surface, reduce fine cracks and pores, and further improve weather resistance and water resistance. Together with the UV absorber, the modified nano titanium dioxide can absorb ultraviolet rays more comprehensively and protect the leather cloth from light damage. The presence of the coupling agent can further improve the adhesion of nano titanium dioxide to the base material, ensuring that the weather-resistant hydrophobic layer will not fall off easily. In summary, the modified nano titanium dioxide not only has weather resistance and hydrophobic properties itself, but also through the synergistic effect with other raw materials, it together forms a high-efficiency weather-resistant hydrophobic layer, which significantly improves the overall performance of outdoor leather cloth.

[0013] Preferably, the mass ratio of hexamethyldisilazane, 3-aminopropyltrimethoxysilane, tetraethoxysilane and anhydrous ethanol is 1:1:1:5.

[0014] Preferably, the coupling agent is prepared by mixing 3-(isomethacryloyloxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:2.

[0015] By adopting the above technical scheme, the main function of the coupling agent in this application is to improve the bonding force between the weather-resistant hydrophobic layer and the leather cloth layer, enhance the adhesion of the coating, and make it difficult to fall off in an outdoor environment. At the same time, the coupling agent can also improve the hydrophobicity and water resistance of the coating, and further improve the weather resistance of the leather cloth. 3-(isobutylene acyloxy) propyl trimethoxy silane and methyl trimethoxy silane form a stable chemical bond with the leather cloth layer and the weather-resistant hydrophobic layer through chemical bonding, thereby improving the adhesion of the coating. 3-(isobutylene acyloxy) propyl trimethoxy silane and methyl trimethoxy silane form a hydrophobic group in the coating, so that the coating surface has excellent hydrophobic properties, and improves the water resistance of the leather cloth. 3-(isobutylene acyloxy) propyl trimethoxy silane and methyl trimethoxy silane form a stable chemical structure in the coating, which can resist the erosion of natural environmental factors such as ultraviolet rays and oxidation, thereby improving the weather resistance of the leather cloth. 3-(Isomethacryloyloxy)propyltrimethoxysilane and methyltrimethoxysilane form a uniform cross-linked network structure in the coating, which improves the stability and service life of the coating. In summary, the coupling agent in the present application is prepared by mixing 3-(Isomethacryloyloxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:2, which can effectively improve the weather resistance, hydrophobicity and water resistance of the leather cloth, so that it has a longer service life in outdoor environments.

[0016] Preferably, the viscosity of the hydrogenated silicone oil is 100 mPa·s, and the active hydrogen content is 0.1%.

[0017] Preferably, the catalyst is a platinum catalyst, and the content of the platinum catalyst is 15ppm-18ppm based on the mass of platinum.

[0018] In a second aspect, the present application provides a method for preparing a weather-resistant leather cloth for outdoor use, which adopts the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned outdoor weather-resistant leather cloth, comprising the following steps: S101, respectively add modified polymethylphenylsiloxane resin, precipitated barium sulfate, two-thirds of the side hydrogenated silicone oil and coupling agent into a preheated vacuum mixer according to their mass fractions, stir for 2-3 hours at a temperature of 110-120°C and -0.1MPa, and grind after cooling to room temperature until the fineness is ≤50μm; S102, adding the qualified material of fineness into a high-speed mixer, and adding modified nano titanium dioxide, ultraviolet absorber, catalyst and remaining side hydrogen silicone oil, stirring for 30-50min at room temperature and -0.09 to -0.1MPa to obtain a weather-resistant hydrophobic coating; S103, coating the surface of the leather cloth layer with a weather-resistant hydrophobic coating, and forming a weather-resistant hydrophobic layer with a thickness of 30-40 microns on the surface of the leather cloth layer after drying, thereby obtaining a leather cloth with strong weather resistance for outdoor use.

[0019] In summary, the beneficial technical effects of this application are: 1. Excellent weather resistance: By using raw materials such as modified polymethylphenylsiloxane resin and modified nano titanium dioxide, the leather cloth's resistance to ultraviolet rays, temperature differences, humidity and other environmental factors is improved, so that it can still maintain good physical properties and appearance after long-term outdoor use.

[0020] 2. Excellent hydrophobic and water-resistant properties: The ingredients in the weather-resistant hydrophobic layer, such as modified nano-titanium dioxide and side hydrogen-containing silicone oil, provide an extremely high water contact angle, making it difficult for water to penetrate, enhancing the waterproof performance of the material. At the same time, hydrophobicity also brings self-cleaning function, reducing maintenance costs.

[0021] 3. Stability and durability: The use of coupling agent enhances the bonding force between the weather-resistant hydrophobic layer and the leather cloth layer, making the coating less likely to fall off, thereby extending the service life of the product.

[0022] 4. Self-cleaning function: Due to the high hydrophobicity, the spherical drops of water formed on the surface of the leather cloth can effectively take away dust and dirt, reducing the frequency and difficulty of cleaning. DETAILED DESCRIPTION

[0023] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0024] Preparation Example 1 Preparation of modified polymethylphenylsiloxane resin The preparation method of the modified polymethylphenylsiloxane resin is as follows: 2 mol of methylphenyldichlorosilane, 7 mol of dimethyldichlorosilane and 1 mol of methyltrichlorosilane are added into a reactor equipped with a separatory funnel, condensation reflux and vacuum respectively; 6L of a mixed diluent and 0.1 mol of isopropyl titanate catalyst are added under heating and magnetic stirring; 3.5 mol of deionized water is added dropwise and fully stirred; after stirring at room temperature for 4 hours, the temperature is raised to 73°C and refluxed for 2.5 hours; finally, the low-boiling point substances are removed under reduced pressure at 70°C and 1 kPa for 2.5 hours to obtain the modified polymethylphenylsiloxane resin, wherein the mixed diluent is prepared by mixing tetraethoxysilane, butyl acetate and anhydrous ethanol in a substance amount ratio of 2:2:1.

[0025] The modified polymethylphenylsiloxane resin prepared above was applied to each example.

[0026] Preparation Example 2 Preparation of modified nano titanium dioxide The preparation method of modified nano titanium dioxide comprises the following steps: S51. According to the mass fractions, 1 kg of hexamethyldisilazane, 1 kg of 3-aminopropyltrimethoxysilane, 1 kg of tetraethoxysilane and 5 kg of anhydrous ethanol were fully mixed to prepare a mixed modifier; S52. According to the mass fractions, 1 kg of nano titanium dioxide with a particle size of 20 nm and 2 kg of mixed modifier were fully mixed at room temperature for 35 minutes, and then ultrasonicated at room temperature for 1.5 hours, and then transferred into a vacuum mixer. The mixture was heated to 75°C and stirred at -0.25 MPa for 4.5 hours under reflux conditions. Finally, the ethanol was removed under reduced pressure and the modified nano titanium dioxide was obtained after drying.

[0027] The modified nano titanium dioxide prepared above is applied to various examples.

[0028] Example 1 A leather cloth with strong weather resistance for outdoor use, comprising a leather cloth layer and a weather-resistant hydrophobic layer, wherein the weather-resistant hydrophobic layer comprises the following raw materials by mass: 3.0 kg of modified polymethylphenylsiloxane resin, 1.5 kg of modified nano titanium dioxide, 3.0 kg of side hydrogen-containing silicone oil (viscosity 100 mPa·s, active hydrogen content 0.1%), 1.0 kg of precipitated barium sulfate, 0.1 kg of coupling agent, 0.08 kg of ultraviolet absorber, and 0.008 kg of catalyst, wherein the coupling agent is prepared by mixing 3-(isomethacryloyloxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:2, and the catalyst is a platinum catalyst, and the content of the platinum catalyst is 15 ppm based on the mass of platinum.

[0029] The method for preparing the above-mentioned outdoor weather-resistant leather cloth comprises the following steps: S101, respectively add modified polymethylphenylsiloxane resin, precipitated barium sulfate, two-thirds of the side hydrogenated silicone oil and coupling agent into a preheated vacuum mixer according to their mass fractions, stir for 3 hours at 110°C and -0.1MPa, and grind after cooling to room temperature until the fineness is ≤50μm; S102, adding the qualified material of fineness into a high-speed mixer, and adding modified nano titanium dioxide, ultraviolet absorber, catalyst and remaining side hydrogen silicone oil, stirring for 30 minutes at room temperature and -0.09MPa to obtain a weather-resistant hydrophobic coating; S103, coating the surface of the leather cloth layer with a weather-resistant hydrophobic coating, and forming a weather-resistant hydrophobic layer with a thickness of 30 microns on the surface of the leather cloth layer after drying, thereby obtaining a leather cloth with strong weather resistance for outdoor use.

[0030] Example 2 A leather cloth with strong weather resistance for outdoor use, comprising a leather cloth layer and a weather-resistant hydrophobic layer, wherein the weather-resistant hydrophobic layer comprises the following raw materials by mass: 3.5 kg of modified polymethylphenylsiloxane resin, 2.0 kg of modified nano titanium dioxide, 3.2 kg of side hydrogen-containing silicone oil (viscosity 100 mPa·s, active hydrogen content 0.1%), 1.2 kg of precipitated barium sulfate, 0.15 kg of coupling agent, 0.12 kg of ultraviolet absorber, and 0.012 kg of catalyst, wherein the coupling agent is prepared by mixing 3-(isobutyleneoxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:2, and the catalyst is a platinum catalyst, and the content of the platinum catalyst is 18 ppm based on the mass of platinum.

[0031] The method for preparing the above-mentioned outdoor weather-resistant leather cloth comprises the following steps: S101, respectively add modified polymethylphenylsiloxane resin, precipitated barium sulfate, two-thirds of the side hydrogenated silicone oil and coupling agent into a preheated vacuum mixer according to their mass fractions, stir for 2 hours at 120°C and -0.1MPa, and grind after cooling to room temperature until the fineness is ≤50μm; S102, adding the qualified material of fineness into a high-speed mixer, and adding modified nano titanium dioxide, ultraviolet absorber, catalyst and remaining side hydrogen silicone oil, stirring for 50min at room temperature and -0.1MPa to obtain a weather-resistant hydrophobic coating; S103, coating the surface of the leather cloth layer with a weather-resistant hydrophobic coating, and forming a weather-resistant hydrophobic layer with a thickness of 40 microns on the surface of the leather cloth layer after drying, thereby obtaining a leather cloth with strong weather resistance for outdoor use.

[0032] Example 3 A leather cloth with strong weather resistance for outdoor use, comprising a leather cloth layer and a weather-resistant hydrophobic layer, wherein the weather-resistant hydrophobic layer comprises the following raw materials by mass: 3.3 kg of modified polymethylphenylsiloxane resin, 1.7 kg of modified nano titanium dioxide, 3.1 kg of side hydrogen-containing silicone oil (viscosity 100 mPa·s, active hydrogen content 0.1%), 1.1 kg of precipitated barium sulfate, 0.12 kg of coupling agent, 0.1 kg of ultraviolet absorber, and 0.01 kg of catalyst, wherein the coupling agent is prepared by mixing 3-(isomethacryloyloxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:2, and the catalyst is a platinum catalyst, and the content of the platinum catalyst is 17 ppm based on the mass of platinum.

[0033] The method for preparing the above-mentioned outdoor weather-resistant leather cloth comprises the following steps: S101, respectively add modified polymethylphenylsiloxane resin, precipitated barium sulfate, two-thirds of the side hydrogenated silicone oil and coupling agent into a preheated vacuum mixer according to their mass fractions, stir for 2.5 hours at 115°C and -0.1MPa, and grind after cooling to room temperature until the fineness is ≤50μm; S102, adding the qualified material of fineness into a high-speed mixer, and adding modified nano titanium dioxide, ultraviolet absorber, catalyst and remaining side hydrogen silicone oil, stirring for 40 minutes at room temperature and -0.095MPa to obtain a weather-resistant hydrophobic coating; S103, coating the surface of the leather cloth layer with a weather-resistant hydrophobic coating, and forming a weather-resistant hydrophobic layer with a thickness of 35 microns on the surface of the leather cloth layer after drying, thereby obtaining a leather cloth with strong weather resistance for outdoor use.

[0034] Comparative Example 1 The same as Example 3, except that an equal amount of nano titanium dioxide with a particle size of 20 nm is used instead of the modified nano titanium dioxide.

[0035] Comparative Example 2 The same as Example 3, except that the amount of modified nano titanium dioxide added is 0.

[0036] Comparative Example 3 The same as Example 3, except that the coupling agent is 3-(isomethacryloyloxy)propyltrimethoxysilane.

[0037] Comparative Example 4 The same as Example 3, except that the coupling agent is methyltrimethoxysilane.

[0038] Performance Testing The outdoor weather-resistant leather fabrics prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were sampled and subjected to the following performance tests. The test results are shown in Table 1. Water resistance: Determine according to the provisions of GB / T1733-1933, test time is 600 hours, and judge whether there is delamination; Water contact angle: analyzed by JY-PHB contact angle meter from Chengde Jinhe Instrument Manufacturing Co., Ltd. Peeling test: Use a tensile testing machine to test the outdoor weather-resistant leather fabrics prepared in Examples 1 to 3 and Comparative Examples 1 to 4. Cut the fabrics into samples with a length of 125 mm and a width of 50 mm. Then place the samples stably on the test board of the tensile testing machine. The tensile testing machine performs peeling at 300 mm / min. Resistance to artificial weathering: Determined in accordance with the provisions of GB / T1865-2009.

[0039] Table 1 Performance test project Water contact angle / ° Peel test / KN / m Weather resistance / h Water resistance Example 1 138.3 8.2 1800 No stratification Example 2 141.1 7.9 1800 No stratification Example 3 139.7 8.1 1800 No stratification Comparative Example 1 109.3 6.3 900 Layering Comparative Example 2 107.2 7.8 700 No stratification Comparative Example 3 131.2 7.1 1500 Layering Comparative Example 4 130.1 6.9 1450 Layering Analyzing the data in Table 1, we can see that: 1) The weather-resistant leather cloth for outdoor use prepared in Examples 1 to 3 has excellent weather resistance, hydrophobicity and water resistance, so that it can maintain a good state for a long time in an outdoor environment. At the same time, since the bonding force between the weather-resistant hydrophobic layer and the leather cloth layer is very high, the performance of the leather cloth is very stable and not easy to fall off, thereby greatly improving its service life.

[0040] 2) The performance comparison analysis of the outdoor weather-resistant leather cloth prepared in combination with Example 3 and Comparative Examples 1-2 shows that the modified nano titanium dioxide prepared by the present application is modified by reacting with substances such as hexamethyldisilazane, 3-aminopropyltrimethoxysilane and tetraethoxysilane, so that the surface of the nano titanium dioxide is modified to have stronger hydrophobic properties. This helps the formation and rolling of water droplets on the surface of the leather cloth, thereby taking away dust and dirt. Due to the presence of the modified nano titanium dioxide, the contact angle formed by the water droplets on the surface of the material increases (more than 138.0°), so that the leather cloth has a self-cleaning function. Rainwater scouring can easily remove surface pollution and reduce maintenance costs. Through surface modification, the compatibility and dispersibility of nano titanium dioxide in the weather-resistant hydrophobic layer are improved, thereby enhancing the stability and durability of the coating. The modified nano titanium dioxide can be better combined with the polymethylphenylsiloxane resin to form a uniform and continuous protective layer, improving the overall weather resistance and hydrophobicity. Nano-sized titanium dioxide particles are filled in the coating, which can effectively cover the leather surface, reduce micro cracks and pores, and further improve weather resistance and water resistance.

[0041] 3) The performance comparison analysis of the outdoor weather-resistant leather cloth prepared in combination with Example 3 and Comparative Examples 3-4 shows that the coupling agent is prepared by mixing 3-(isobutylene acyloxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:2, and the synergistic effect between them is utilized to improve the bonding force between the weather-resistant hydrophobic layer and the leather cloth layer, enhance the adhesion of the coating, and make it difficult to fall off in the outdoor environment. At the same time, the coupling agent can also improve the hydrophobicity and water resistance of the coating, further improve the weather resistance of the leather cloth, and make it have a longer service life in the outdoor environment.

[0042] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A weather-resistant leather cloth for outdoor use, characterized in that: The weather-resistant leather cloth for outdoor use comprises a leather cloth layer and a weather-resistant hydrophobic layer. The weather-resistant hydrophobic layer comprises the following preparation raw materials by weight: 30-35 parts of modified polymethylphenylsiloxane resin, 15-20 parts of modified nano titanium dioxide, 30-32 parts of side hydrogen-containing silicone oil, 10-12 parts of precipitated barium sulfate, 1-1.5 parts of coupling agent, 0.8-1.2 parts of ultraviolet absorber, and 0.08-0.12 parts of catalyst.

2. The weather-resistant leather cloth for outdoor use according to claim 1, characterized in that: The preparation method of the modified polymethylphenylsiloxane resin is as follows: methylphenyldichlorosilane, dimethyldichlorosilane and methyltrichlorosilane are added into a reactor equipped with a separatory funnel, condensation reflux and vacuum according to a substance molar ratio of 2:7:1 respectively; a mixed diluent and isopropyl titanate catalyst are added under heating and magnetic stirring; deionized water is added dropwise and fully stirred; after stirring at room temperature for 4 hours, the temperature is raised to 70-75°C and refluxed for 2-3 hours; and finally, low-boiling substances are removed under reduced pressure at 70°C and 1 kPa for 2-3 hours to obtain the modified polymethylphenylsiloxane resin.

3. The weather-resistant leather cloth for outdoor use according to claim 2, characterized in that: The mixed diluent is prepared by mixing tetraethoxysilane, butyl acetate and anhydrous ethanol in a substance amount ratio of 2:2:

1.

4. The weather-resistant leather cloth for outdoor use according to claim 2, characterized in that: The dosage ratio of the methyltrichlorosilane, the mixed diluent, the isopropyl titanate catalyst and the deionized water is 1 mol:6L:0.1 mol:(3-4) mol.

5. The weather-resistant leather cloth for outdoor use according to claim 1, characterized in that: The preparation method of the modified nano titanium dioxide comprises the following steps: S51. Fully mix hexamethyldisilazane, 3-aminopropyltrimethoxysilane, tetraethoxysilane and anhydrous ethanol according to their weight fractions to prepare a mixed modifier; S52. According to the mass proportions, 100 parts of nano titanium dioxide with a particle size of 20 nm and 200 parts of mixed modifier are fully mixed at room temperature for 30-40 minutes, ultrasonicated at room temperature for 1-2 hours, and then transferred into a vacuum mixer. The mixture is heated to 70-80°C and stirred under reflux conditions of -0.3 to -0.2 MPa for 4-5 hours. Finally, ethanol is removed under reduced pressure and the modified nano titanium dioxide is obtained after drying.

6. The weather-resistant leather cloth for outdoor use according to claim 5, characterized in that: The mass ratio of the hexamethyldisilazane, 3-aminopropyltrimethoxysilane, tetraethoxysilane and anhydrous ethanol is 1:1:1:

5.

7. The weather-resistant leather cloth for outdoor use according to claim 1, characterized in that: The coupling agent is prepared by mixing 3-(isomethacryloyloxy)propyltrimethoxysilane and methyltrimethoxysilane in a mass ratio of 5:

2.

8. The weather-resistant leather cloth for outdoor use according to claim 1, characterized in that: The viscosity of the hydrogen-containing silicone oil is 100 mPa·s, and the active hydrogen content is 0.1%.

9. The weather-resistant leather cloth for outdoor use according to claim 1, characterized in that: The catalyst is a platinum catalyst, and the content of the platinum catalyst is 15ppm-18ppm based on the mass of platinum.

10. A method for preparing a weather-resistant leather cloth for outdoor use according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101, respectively add modified polymethylphenylsiloxane resin, precipitated barium sulfate, two-thirds of the side hydrogenated silicone oil and coupling agent into a preheated vacuum mixer according to their mass fractions, stir for 2-3 hours at a temperature of 110-120°C and -0.1MPa, and grind after cooling to room temperature until the fineness is ≤50μm; S102, adding the qualified material into a high-speed mixer, and adding modified nano titanium dioxide, ultraviolet absorber, catalyst and remaining side hydrogen silicone oil, stirring for 30-50 minutes at room temperature and -0.09 to -0.1MPa to obtain a weather-resistant hydrophobic coating; S103, coating the surface of the leather cloth layer with a weather-resistant hydrophobic coating, and forming a weather-resistant hydrophobic layer with a thickness of 30-40 microns on the surface of the leather cloth layer after drying, thereby obtaining a leather cloth with strong weather resistance for outdoor use.