Experimental device and method for testing forming limit and resilience of high-strength steel
By designing an experimental device for testing the forming limit and springback of high-strength steel, and using low-frequency vibration and digital image correlation methods, the problem of inaccurate evaluation of the forming limit and springback in the existing technology has been solved, and the forming performance of high-strength steel has been achieved. scientific, accurate assessment and process optimization.
Patent Information
- Application Number
- CN202310310342.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology lacks devices and methods specifically designed to evaluate the forming limits and springback conditions of high-strength steel under low-frequency vibration-assisted forming, resulting in inaccurate evaluation of forming performance and affecting product design and process development.
An experimental device for forming limit and springback testing of high-strength steel was designed, including an upper platen, a pillar, a concave mold, a blank holder, a nitrogen gas spring, a lower platen, a punch and an excitation cylinder. Through low-frequency oscillation and digital image correlation methods Record the strain in real time and measure the forming limit and springback phenomenon.
The device can accurately evaluate the forming limit and springback conditions of high-strength steel under low-frequency vibration fields, provide real and accurate data to guide the low-frequency vibration process window, improve forming performance and reduce springback phenomena, and simplify the testing process.
Smart Images

Figure CN118730769A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a vibration-assisted forming technology in sheet metal forming manufacturing, and more specifically to an experimental device and method for high-strength steel forming limit and springback testing. Background Art
[0002] Lightweighting of automobiles has become an inevitable trend of development. High-strength steel has become the preferred material for car body materials due to its high strength, light weight and low cost. However, high-strength steel has insufficient forming performance due to its poor plasticity, and the release of residual stress after forming will cause large springback, complex torsion and other problems, which seriously affect the dimensional accuracy of the formed parts and create extremely high manufacturing difficulty. This has become the main problem restricting the use of high-strength steel.
[0003] The vibration-assisted forming process is a new forming technology that superimposes a vibration field of a certain amplitude and frequency during the forming process to reduce the material's deformation resistance, improve contact conditions, and thus enhance the product's forming performance and surface quality. According to the size of the superimposed vibration frequency, it can be divided into ultrasonic vibration-assisted forming and low-frequency vibration-assisted forming. There are significant differences in the excitation source and vibration application mechanism of the two. Since ultrasonic vibration sources are easy to obtain and implement, ultrasonic vibration-assisted forming has been studied earlier and has been widely used, but the ultrasonic vibration excitation force is small. It is usually used for the forming of parts with low material strength and small geometric dimensions, and is difficult to use for the forming of high-strength and large parts. In contrast, the excitation force generated by low-frequency vibration is larger and can be used for the forming of high-strength and large-size parts. It is rarely reported and has not been widely used.
[0004] From the existing research results, low-frequency vibration-assisted forming technology can promote material flow and improve the forming limit on the one hand; on the other hand, the material vibrates up and down during forming to continuously release residual stress and reduce unloading springback. This is consistent with the forming characteristics of high-strength steel, and provides a theoretical possibility for combining vibration-assisted forming with high-strength steel to improve the forming performance of high-strength steel. At present, most of the research on low-frequency vibration-assisted forming only stays on low-strength materials such as low-carbon steel, aluminum and copper, and has not yet involved high-strength steel materials such as QP steel. There are still blank experimental devices and test methods for low-frequency vibration-assisted high-strength steel forming.
[0005] At present, there is no device or method specifically used to evaluate the forming limit of materials under low-frequency vibration-assisted forming. The existing evaluation of the forming performance of steel materials, including high-strength steel, mostly adopts the deep drawing process, and judges the forming ability of the material by the limit drawing ratio of the formed part or by the standard FLC test. This type of method can only measure the forming limit of the material under the condition of no vibration based on the macroscopic measurement, and cannot accurately reflect the true limit strain capacity of the material under vibration conditions. It will cause errors and losses in evaluating the forming ability of the vibration forming process and guiding product design, process design and mold development. Summary of the invention
[0006] In view of the defects existing in the prior art, the purpose of the present invention is to provide an experimental device and method for testing the forming limit and springback of high-strength steel, which can test the forming limit and springback of the material under a low-frequency vibration field, so as to clarify the forming limit value of high-strength steel under low-frequency vibration and obtain the optimal low-frequency vibration process window, thereby providing real and accurate guidance data for low-frequency vibration part design, process development, and process window selection.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] The first aspect of the present invention provides an experimental device for high-strength steel forming limit and springback testing, comprising an upper mold plate, a support, a concave mold, a blank holder, a spring, a lower mold plate, a punch and an exciting cylinder;
[0009] The upper template is arranged on the crossbeam of the testing machine;
[0010] The upper end of the pillar is connected to the upper mold plate, and the lower end is connected to the concave mold;
[0011] The upper end of the spring is connected to the blank holder, and the lower end is connected to the lower mold plate. The blank holder corresponds to the concave mold.
[0012] The excitation cylinder is arranged on the lower template;
[0013] The punch is arranged on the excitation cylinder and is matched with the blank holder;
[0014] The lower template is arranged on the base of the stretching machine.
[0015] Preferably, there are four pillars, which are evenly distributed between the upper mold plate and the concave mold.
[0016] Preferably, the pressure ring is provided with a positioning ring for fixing the sample.
[0017] Preferably, the spring is a nitrogen spring, four of which are provided and evenly distributed between the pressure ring and the lower template.
[0018] Preferably, the excitation cylinder and the lower mold plate, and the punch and the excitation cylinder are connected by bolts.
[0019] Preferably, the punch is a hemispherical punch with a diameter of 100 mm.
[0020] The second aspect of the present invention provides an experimental method for high-strength steel forming limit and springback test, and the forming limit test and springback test of high-strength steel are carried out by using the experimental device for high-strength steel forming limit and springback test provided by the first aspect of the present invention:
[0021] Before the forming limit test, the sample is subjected to a painting treatment;
[0022] When conducting a forming limit test, the excitation cylinder generates low-frequency oscillations, and the punch connected thereto oscillates together. The testing machine moves downward so that the die and the blank holder clamp the sample, and then drives the sample to move downward so that the sample contacts the punch and gradually deforms. At the same time, the digital image correlation method is used to record the strain in real time until the sample breaks. Then, the principal strain and secondary strain of the sample before breaking under different vibration conditions are calculated respectively as evaluation indicators of the forming limit.
[0023] When conducting the rebound test, the starting position and the ending position of the stretching machine are set on the premise that the sample does not break, that is, to ensure that the sample has the same deformation under different vibration fields, and the height of the center position of the sample is measured as an evaluation index of the rebound amount.
[0024] Preferably, the painting process is specifically as follows:
[0025] First, wipe the sample with alcohol to remove the oil on the surface, and then spray a layer of white paint on it. After the white paint is air-dried, spray evenly fine black spots on it.
[0026] Preferably, the digital image correlation method is specifically:
[0027] During the deformation process of the sample, a high-speed camera is used to synchronously collect high-frequency data to obtain a strain image of the sample surface at each loading stage.
[0028] Preferably, the height of the center position of the sample is the distance between the highest point of the semicircle of the sample and the plane when the bent sample is placed on a plane after the rebound test.
[0029] The present invention provides an experimental device and method for forming limit and springback test of high-strength steel, which solves the device problem and experimental method of low-frequency vibration forming limit test and springback test of materials including high-strength steel. Compared with the existing vibration-assisted forming test device (deep drawing, etc.), the device can measure the ultimate principal true strain and secondary true strain under vibration conditions and different stress states, and more accurately judge the influence of the vibration field on the forming limit of high-strength steel. Moreover, the method can complete the two tests of forming limit and springback phenomenon under vibration field using the same device and the same size sample, which is simple and fast to operate, and does not require other sizes of samples and separate bending devices. On the one hand, the present invention aims at the problems of insufficient forming performance and serious springback phenomenon of high-strength steel, superimposes low-frequency vibration field when forming high-strength steel, and calculates the forming limit of high-strength steel under different vibration conditions through equipment such as DIC, thereby ensuring scientificity and accuracy. On the other hand, the method uses the same size sample and the same device to complete the springback test of formed parts under vibration field by changing the loading conditions, which is simple and fast to operate and reduces the workload. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a structural schematic diagram of a high-strength steel forming limit and springback test experimental device of the present invention;
[0031] Figure 2 Schematic diagram of a sample in an embodiment of the high-strength steel forming limit and springback test experimental method of the present invention;
[0032] Figure 3 It is a strain curve diagram of the cross section obtained by DIC recording one frame before the sample breaks in the embodiment of the experimental method of the present invention;
[0033] Figure 4 Schematic diagram of forming limit of QP980 at different vibration amplitudes in the embodiment of the experimental method of the present invention;
[0034] Figure 5 Schematic diagram of forming limit of QP980 at different vibration amplitudes in the embodiment of the experimental method of the present invention;
[0035] Figure 6 1 is a schematic diagram of the height of the center position of the springback test formed part in the embodiment of the experimental method of the present invention;
[0036] Figure 7 Schematic diagram of the center position height and springback reduction rate of the formed part under different vibration amplitudes in the embodiment of the experimental method of the present invention;
[0037] Figure 8 It is a schematic diagram of the center position height and rebound reduction rate of the formed part under different vibration amplitudes in the embodiment of the experimental method of the present invention. DETAILED DESCRIPTION
[0038] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0039] Combination Figure 1 As shown, an experimental device for high-strength steel forming limit and springback test provided by the present invention includes an upper template 1, a support 2, a die 3, a blank holder 5, a nitrogen spring 7, a lower template 9, a punch 6 and an exciting cylinder 8.
[0040] The upper template 1 is connected to the crossbeam of the testing machine at the top and to four pillars 2 at the bottom. The pillars 2 are installed in the die. During the loading process, the crossbeam drives the upper template 1, pillars 2 and die 3 to move downward together. The positioning ring above the blank holder 5 is used to center and fix the sample 4. The four nitrogen springs 7 below are symmetrically distributed in the four directions of the blank holder. The lower template 9 of the device is fixed to the base of the tensile machine. The lower template 9 and the exciting cylinder 8, as well as the upper part of the exciting cylinder 8 and the punch 6 are all connected by bolts. During loading, the die 3 loads the pressing blank ring 5 downward, and moves downward together after pressing the sample 4. The counter-thrust force generated by the loaded compressed nitrogen spring 7 is used as the experimental blank holder force. After contacting the punch 6, the sample 4 is deformed. At this time, the vibration condition is changed by adjusting the vibration amplitude and vibration frequency of the exciting cylinder 8.
[0041] The vibration cylinder 8 changes the vibration amplitude and vibration frequency of the vibration cylinder 8 by changing the oil intake and the reversing frequency through the control station. The vibration cylinder 8 is connected to the punch 6, driving the punch 6 to vibrate and provide a low-frequency vibration field for the forming process.
[0042] Low-frequency vibration means that the exciting cylinder 8 and the punch 6 vibrate together to provide a vibration field with a frequency of 0 to 100 Hz.
[0043] The punch 6 is a hemispherical punch with a diameter of 100 mm.
[0044] Four nitrogen springs 7 of the same specification are symmetrically placed in four directions below the blank holder 5 to ensure uniform force. The testing machine drives the die 3 and the blank holder 5 to move downward, and the compression of the nitrogen spring 7 generates a counter-force on the blank holder 5, which is used as the blank holder force during forming.
[0045] Sample 4 is made of high-strength steel and is cut using an electric spark cutting device to ensure dimensional accuracy. Samples 4 used in the forming limit test and the springback test are of the same size.
[0046] The present invention also provides an experimental method for high-strength steel forming limit and springback test, and the forming limit test and springback test of high-strength steel are realized by using the experimental device for high-strength steel forming limit and springback test of the present invention:
[0047] Before the forming limit test, sample 4 was spray-painted;
[0048] When conducting the forming limit test, the exciting cylinder 8 generates low-frequency oscillation, and the punch 6 connected to it oscillates together. The testing machine moves downward to clamp the sample 4 with the die 3 and the blank holder 5, and then drives the sample 4 to move downward, so that the sample 4 contacts the punch 6 and gradually deforms. At the same time, the digital image correlation method (DIC) is used to record the strain in real time until the sample 4 breaks. Then, the principal strain and secondary strain of the sample 4 before the break under different vibration conditions are calculated respectively as the evaluation index of the forming limit.
[0049] When conducting the rebound test, on the premise that sample 4 does not break, the starting position and the ending position of the stretching machine are set, that is, to ensure that sample 4 has the same deformation under different vibration fields, and the height of the center position of sample 4 is measured as an evaluation index of the rebound amount.
[0050] The specific painting process is as follows:
[0051] First, wipe the sample 4 with alcohol to remove the oil on the surface, and then spray it with a layer of white paint. After the white paint is dried, spray it with evenly distributed and fine black specks to ensure that DIC can clearly capture and identify it.
[0052] The digital image correlation method is specifically:
[0053] During the deformation process of sample 4, a high-speed camera was used to synchronously collect high-frequency data to obtain the strain image of the surface of sample 4 at each loading stage. In the forming limit test, the entire process from the start of the experiment to the fracture of sample 4 was recorded by DIC equipment.
[0054] The principal strain and the secondary strain are the limit strain in the length direction and the limit strain in the width direction before the fracture of sample 4. The photo of the frame before the fracture was recorded by DIC photography, and the cross-section line was inserted in the direction perpendicular to the crack to obtain the forming limit strain, and then the principal true strain and the secondary true strain under different stress states and vibration conditions were obtained by fitting.
[0055] The forming limit refers to the maximum strain that a material can produce without failure. In this experiment, it is represented by principal strain and secondary strain. The larger the absolute value, the greater the forming limit under this stress state and the better the forming performance.
[0056] The height of the center position of the sample 4 is the distance between the highest point of the semicircle of the sample 4 and the plane when the bent sample is placed on the plane after the rebound test.
[0057] Springback refers to the change in shape caused by the release of elastic stress in the deformed body after the deformation constraint is removed, which affects the dimensional accuracy of the specimen 4. The greater the deviation between the actual size and the ideal size, the more serious the springback phenomenon.
[0058] Example
[0059] The forming limit test and springback test device in this embodiment is manufactured and installed as described above. The material of the template 1, support 2 and blank holder 5 on the device is 45 steel, and the material of the die 3 and punch 6 is Cr12MoV die steel. The material of the experimental sample is 1.0mm thick QP980 high-strength steel, and the wire cutting process is used to process the size as follows Figure 2 As shown in the figure, the initial total load of the four nitrogen springs is 96 kN, and the maximum total load is 153.2 kN as the blank holding force, and the blank holding force increases with the increase of the downward pressure.
[0060] Both vibration amplitude and vibration frequency will affect the forming limit and springback phenomenon of high-strength steel. To explore the influence of vibration amplitude, the vibration frequency was fixed at 30 Hz, and the amplitudes were selected as 0.062 mm, 0.078 mm, and 0.125 mm; to explore the influence of vibration frequency, the amplitude was fixed at 0.125 mm, and the vibration frequencies were selected as 10 Hz, 20 Hz, and 30 Hz.
[0061] In this embodiment, spray painting is required before the forming limit test. After wiping the oil stains on the surface of the sample 4 with alcohol, a layer of white paint is sprayed on it, and after air drying, fine black speckles are evenly sprayed on it. A plane mirror is placed above the die 3 to clearly reflect the sample. The speckles on the surface of the sample 4 are identified by adjusting the position and angle of the DIC device camera to ensure that the DIC system can clearly capture and record the strain of the sample 4 during the loading process.
[0062] After painting, the sample 4 is fixed in the positioning ring above the blank holder 5, and lubricating oil is applied to the punch 6 as the lubrication condition of the experiment. Then the position of the die 3 is adjusted downward so that the sample 4 is close to the punch 6, and this position is determined as the starting position for loading. The displacement of the testing machine is reset here to ensure that the position of each loading is the same. The initial blank holder force at this time is 106.3kN. The testing machine drives the die 3 to move downward at 2mm / min as the loading speed. At the beginning of loading, the DIC device is turned on to take pictures and record and apply vibrations under different conditions until the sample breaks. The shooting speed is 10 frames per second.
[0063] According to the photos taken by the DIC device, the frame before the fracture of sample 4 is selected, and the section perpendicular to the fracture is inserted to obtain the main true strain and secondary true strain curves on the section, as shown in Figure 3 The exported data were fitted with a parabola using Matlab software to obtain the principal strain and secondary strain before fracture, which represent the forming limit of QP980 under different vibration conditions.
[0064] During loading, the sample 4 is in a uniaxial tensile stress state, the principal strain is the strain in the length direction of the sample, and the secondary true strain is the strain in the width direction of the sample, so the principal strain value is positive and the secondary strain value is negative. The larger the absolute value of the principal strain and the secondary strain, the greater the deformation, indicating that the forming limit is greater.
[0065] Figure 4 The figure shows the forming limit of QP980 under different amplitudes. The principal strain of the specimen is 0.2305 and the secondary strain is -0.0938 without vibration. After superimposing low-frequency vibrations of different amplitudes, different degrees of improvement occur. At a frequency of 30Hz and an amplitude of 0.062mm, the principal strain of the specimen increases to 0.2622, and the secondary strain increases to -0.1198. The principal strain of the 0.078mm amplitude is 0.273, which is further improved year-on-year. The secondary strain is -0.107, which is still higher than the case without vibration. At a large amplitude of 0.125mm, the maximum principal strain and secondary strain are 0.3487 and -0.135, respectively.
[0066] Figure 5 The figure shows the forming limit of QP980 under different vibration frequencies. The forming limit of 0.125mm amplitude and 10Hz vibration frequency increases significantly, with the principal strain of 0.3211 and the secondary strain of -0.114. When the vibration frequency is 20Hz, the principal strain increases to 0.3390, and the secondary strain decreases slightly to -0.1066, which is still higher than the case without vibration. The forming limit is the largest at 30Hz.
[0067] Superimposing low-frequency vibration fields with different amplitudes and frequencies during loading can improve the forming limit of QP980 high-strength steel.
[0068] The rebound test of this embodiment does not require pre-painting and DIC equipment to record strain. The experimental setting is the same as the starting position of the forming limit test machine, that is, the sample is close to the punch, the same size of sample is used and the same loading speed is set. The difference is that the forming limit test stops until the sample breaks, while the displacement of the rebound test tensile machine is set to 20mm. After the displacement is reached, the test machine automatically stops loading, and the excitation cylinder stops vibrating, unloading and removing the formed part, placing it on the plane to measure the distance H between the highest point of the center position and the table, as shown in Figure 6 As shown. At the beginning of the experiment, the center of the sample was close to the top of the punch, so the height of the center of the formed part without springback was 20mm of the punch stroke. Since the springback phenomenon of QP980 is more serious, this height is often less than 20mm. This test defines the difference between the center height H and 20mm as the springback amount.
[0069] Figure 7The center height and springback reduction rate of the formed parts under different amplitudes. In the absence of vibration, the center height H of the formed part is 18.49mm, and the springback is 1.51mm. After superimposing the vibration field with a frequency of 30Hz and an amplitude of 0.062mm, H increases to 18.89mm, and the springback is 1.11mm, which is 0.4mm less than before. With an amplitude of 0.078mm, the height is further increased to 19.04mm, and the springback is 0.96mm, which is 36.4% less than the springback without vibration. The springback of the formed part with a larger amplitude of 0.125mm is the smallest, only 0.36mm, and the reduction ratio reaches 76.2%.
[0070] The reduction rate of the center height and springback of the formed part under different vibration frequencies is as follows Figure 8 As shown in the figure, the center height of the formed part is 19.19mm under the condition of 0.125mm amplitude and 10Hz vibration frequency, and the springback is reduced by 0.62mm compared with the condition without vibration, a year-on-year decrease of 46.4%. When the amplitude is increased to 20Hz, the springback is reduced to 0.51mm compared with 10Hz, and the reduction rate is 66.2%. The springback phenomenon is further reduced at the vibration frequency of 30Hz.
[0071] The springback phenomenon is caused by the release of residual stress in the formed part after unloading. The repeated up and down vibration of the formed part during the stress process under the low-frequency vibration field is conducive to the release of residual stress. The springback phenomenon after unloading is weakened compared with ordinary forming, further ensuring the dimensional accuracy of the formed part.
[0072] The above low-frequency vibration-assisted high-strength steel forming limit test and springback test experimental device and method are original to the present invention. Different from the existing inventions, the device can more accurately obtain the forming limit of high-strength steel under different stress states and different vibration conditions. In addition, the method uses the same set of equipment, the same size specimen and the same vibration loading method to complete the forming limit test and springback test for the two major problems of poor forming performance and severe springback phenomenon of high-strength steel, and more comprehensively reflects the changes in the forming performance of high-strength steel under the vibration field.
[0073] After specific experimental implementation, low-frequency vibration fields with different frequencies and amplitudes were superimposed during the forming process of QP980 high-strength steel, and the main true strain and secondary true strain before the specimen fracture were obtained by DIC equipment photography and calculation processing. After superimposing low-frequency vibration, the main true strain and secondary true strain increased to varying degrees, and the forming limit was improved. After the rebound test vibration forming, the center height of the formed part is closer to the punch displacement than that of ordinary forming, the rebound amount is reduced, and the rebound phenomenon is weakened. Therefore, superimposing low-frequency vibration during the forming process of high-strength steel is beneficial to improving the forming limit and reducing springback.
[0074] Compared with the prior art, the present invention is improved in that: on the one hand, the experimental device generates a low-frequency vibration field when the high-strength steel is deformed by the vibration of the punch, and cooperates with equipment such as DIC to more accurately obtain the forming limit of high-strength steel under different stress states and different vibration conditions, so as to judge the change in the forming performance of high-strength steel under the low-frequency vibration field. On the other hand, the experimental method completes the forming limit test and the rebound test through the same device and the same size specimen, improving the cumbersome process of using different devices and different size specimens for the forming limit test and the rebound test. In comparison, the method described in the present invention is more convenient and accurate.
[0075] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. An experimental device for high-strength steel forming limit and springback testing, characterized in that: It includes an upper mold plate, a support, a concave mold, a blank holder, a spring, a lower mold plate, a punch and an exciting cylinder; The upper template is arranged on the crossbeam of the testing machine; The upper end of the pillar is connected to the upper mold plate, and the lower end is connected to the concave mold; The upper end of the spring is connected to the blank holder, and the lower end is connected to the lower mold plate. The blank holder corresponds to the concave mold. The excitation cylinder is arranged on the lower template; The punch is arranged on the excitation cylinder and is matched with the blank holder; The lower template is arranged on the base of the stretching machine.
2. The experimental device for high-strength steel forming limit and springback test according to claim 1, characterized in that: The pillars are provided with four and are evenly distributed between the upper mold plate and the concave mold.
3. The experimental device for high-strength steel forming limit and springback test according to claim 1, characterized in that: The pressure ring is provided with a positioning ring for fixing the sample.
4. The experimental device for high-strength steel forming limit and springback test according to claim 1, characterized in that: The spring is a nitrogen spring, 4 of which are provided and evenly distributed between the blank holder and the lower template.
5. The experimental device for high-strength steel forming limit and springback test according to claim 1, characterized in that: The excitation cylinder and the lower mold plate, and the punch and the excitation cylinder are connected by bolts.
6. The experimental device for high-strength steel forming limit and springback test according to claim 1, characterized in that: The punch is a hemispherical punch with a diameter of 100 mm.
7. An experimental method for high-strength steel forming limit and springback testing, characterized in that: The forming limit test and springback test of high-strength steel are carried out by using the experimental device for the forming limit and springback test of high-strength steel as described in any one of claims 1 to 6: Before the forming limit test, the sample is subjected to a painting treatment; When conducting a forming limit test, the excitation cylinder generates low-frequency oscillations, and the punch connected thereto oscillates together. The testing machine moves downward so that the die and the blank holder clamp the sample, and then drives the sample to move downward so that the sample contacts the punch and gradually deforms. At the same time, the digital image correlation method is used to record the strain in real time until the sample breaks. Then, the principal strain and secondary strain of the sample before breaking under different vibration conditions are calculated respectively as evaluation indicators of the forming limit. When conducting the rebound test, the starting position and the ending position of the stretching machine are set on the premise that the sample does not break, that is, to ensure that the sample has the same deformation under different vibration fields, and the height of the center position of the sample is measured as an evaluation index of the rebound amount.
8. The experimental method for high-strength steel forming limit and springback test according to claim 7, characterized in that: The spray painting process is specifically as follows: First, wipe the sample with alcohol to remove the oil on the surface, and then spray a layer of white paint on it. After the white paint is air-dried, spray evenly fine black spots on it.
9. The experimental method for high-strength steel forming limit and springback test according to claim 7, characterized in that: The digital image correlation method is specifically: During the deformation process of the sample, a high-speed camera is used to synchronously collect high-frequency data to obtain a strain image of the sample surface at each loading stage.
10. The experimental method for high-strength steel forming limit and springback test according to claim 7, characterized in that: The center height of the sample is the distance between the highest point of the semicircle of the sample and the plane when the bent sample is placed on a plane after the rebound test.