Method for testing content of metal in original silicon wafer

Through the method of dilute hydrofluoric acid or nitric acid extraction and ICP-MS detection, the difference between the metal content on the surface of the original silicon wafer and the body is calculated, which solves the problem of inaccurate detection in the existing technology and realizes the detection of the metal content in the body of the original silicon wafer. Accurate measurement ensures the quality and efficiency of solar cells.

CN118731144APending Publication Date: 2024-10-01SANY SILICON ENERGY (ZHUZHOU) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410740003.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology cannot effectively detect the content of various metal elements in the original silicon wafer, which affects the quality and efficiency of the solar cells. In particular, it cannot distinguish between surface and internal metal contamination, resulting in inaccurate detection results.

Method used

By mixing raw silicon wafer fragments with dilute hydrofluoric acid or nitric acid solution, metal ions are extracted, and ICP-MS is used to test the metal ion concentration. The difference between the surface and body metal content is calculated through the formula to obtain the body metal content. Dry reconstitution method to improve assay stability and repeatability.

Benefits of technology

It achieves accurate detection of metal content in the original silicon wafer, avoids the introduction of contamination during the corrosion process, improves the stability and repeatability of detection, and ensures the quality and efficiency of the battery wafer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of silicon wafer processing, in particular to a method for testing the metal content in an original silicon wafer body. The method for testing the metal content in the original silicon wafer comprises the following steps: respectively detecting the metal content on the surface of the original silicon wafer and the metal content on the surface of the original silicon wafer, and subtracting the metal content on the surface of the original silicon wafer from the metal content on the surface of the original silicon wafer to obtain the metal content in the original silicon wafer. According to the method for testing the metal content in the original silicon wafer, provided by the invention, the stable method for testing the metal content in the original silicon wafer can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon wafer processing, and in particular to a method for testing the metal content in an original silicon wafer. Background Art

[0002] At present, solar crystalline silicon cells are the mainstream products in the photovoltaic industry. The raw silicon wafers used to produce solar cells usually have a silicon content of 99.999% to 99.9999%, and the remaining trace components are carbon, oxygen and metal impurities. Metal contamination is easily introduced during the production and transportation of raw silicon wafers. Excessive metal contamination, especially contamination inside the raw silicon wafers, will affect the quality of the product cells. Surface contamination of the raw silicon wafers will seriously affect the subsequent passivation process of the cell.

[0003] In the prior art, the introduction of metal contamination in raw silicon wafers is mostly determined by observing the appearance of the raw silicon wafers to determine whether there is surface trace impurity element contamination, and testing the minority carrier lifetime of the raw silicon wafers to determine whether there is abnormal metal contamination in the body, but it is impossible to detect the content of each metal element.

[0004] The main inspection items for raw silicon wafers before leaving the factory are: appearance, size, carbon content, oxygen content, minority carrier lifetime, resistivity, and conductivity type. There is a lack of quantitative detection of metal content on the surface and inside of raw silicon wafers. However, excessive content of different metal elements leads to different defects in semiconductor structure devices. For example, alkali metals and alkaline earth metals (Na, K, Ca, Mg, Ba, etc.) will cause the breakdown voltage of the device to decrease; transition metals and heavy metals (Fe, Cr, Cu, Mn, Pb, Ni, etc.) will affect the service life of the device and increase the dark current when the device is working.

[0005] Therefore, monitoring the content of various metal elements in the original silicon wafer plays an important role in our analysis of the efficiency loss of the finished solar cells.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The present invention provides a method for testing the metal content in an original silicon wafer, so as to realize a stable method for testing the metal content in an original silicon wafer.

[0008] The present invention provides a method for testing the metal content in an original silicon wafer, comprising: respectively detecting the metal content on the surface of the original silicon wafer and the metal content on the surface of the original silicon wafer, and subtracting the metal content on the surface of the original silicon wafer from the metal content on the surface of the original silicon wafer to obtain the metal content in the original silicon wafer.

[0009] According to the testing method for the metal content in the original silicon wafer provided by the present invention, the testing method for the metal content on the surface of the original silicon wafer comprises: S1: mixing m1 grams of original silicon wafer fragments with v1 liter of the first acidic solution, and when the surface of the original silicon wafer fragments is hydrophilic, taking out the original silicon wafer fragments and collecting the first extract; S2: heating and evaporating the first extract, and then using the second acidic solution to redissolve and fix the volume to v1 liter to obtain a first sample solution; S3: using ICP-MS to test the metal ion concentration in the first sample solution to be a1 micrograms / liter; S4: calculating the metal content on the surface of the original silicon wafer by the following formula: ω 表 =(a1×v1×10 -6 ) / m1×100%.

[0010] According to the method for testing the metal content in the original silicon wafer provided by the present invention, the first acidic solution is a dilute hydrofluoric acid solution; and / or the second acidic solution is a nitric acid solution.

[0011] According to the method for testing the metal content in the original silicon wafer provided by the present invention, the concentration of the first acidic solution and the concentration of the second acidic solution are independently, the same or different and are 2wt% to 5wt%.

[0012] According to the method for testing the metal content in the original silicon wafer provided by the present invention, in S1, m1 is 0.3 g to 0.6 g; v1 is 20 ml to 40 ml.

[0013] According to the method for testing the metal content in the original silicon wafer provided by the present invention, in S1, the mixing time is 2 minutes to 10 minutes.

[0014] According to the method for testing the metal content in the original silicon wafer provided by the present invention, the method for testing the metal content on the surface of the original silicon wafer comprises: S1': m2 grams of original silicon wafer fragments are mixed with v2 liters of mixed acid solution, and a second extract is obtained after the reaction is completed; S2': the second extract is heated and evaporated, and then the second acid solution is used to redissolve and dilute to v1 liter to obtain a second sample solution; S3': the metal ion concentration in the second sample solution is tested by ICP-MS and is a2 micrograms / liter; S4': the metal content of the original silicon wafer surface is calculated by the following formula: ω 总 =(a2×v1×10 -6 ) / m2×100%.

[0015] According to the method for testing the metal content in the original silicon wafer provided by the present invention, the mixed acid solution comprises nitric acid and hydrofluoric acid in a mass ratio of 4 to 6:1, and the concentration of the nitric acid in the mixed acid solution is 20 to 50 wt%.

[0016] According to the method for testing the metal content in the original silicon wafer provided by the present invention, in S1', m2 is 0.4 g to 0.6 g; v2 is 20 ml to 40 ml.

[0017] According to the method for testing the metal content in the original silicon wafer provided by the present invention, in S1', v2 liters of the mixed acid solution are added to m2 grams of the original silicon wafer fragments in batches at 30 to 60 degrees Celsius.

[0018] The method for testing the metal content in the original silicon wafer provided by the present invention can realize a stable method for testing the metal content in the original silicon wafer. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the prior art, when testing the metal content in the original silicon wafer, the surface of the original silicon wafer is first corroded, and then the remaining silicon material in the body is digested and extracted for testing. However, during the surface corrosion process, the pollution introduced by the corrosive chemicals themselves and the instability of the corrosion process lead to different corrosion amounts in each sample preparation, resulting in poor experimental repeatability.

[0021] In this regard, the present invention first proposes a new method for testing the metal content in the original silicon wafer, which respectively detects the metal content on the surface of the original silicon wafer and the metal content on the surface of the original silicon wafer, and subtracts the metal content on the surface of the original silicon wafer from the metal content on the surface of the original silicon wafer to obtain the metal content in the original silicon wafer.

[0022] According to a preferred embodiment provided by the present invention, the method for testing the metal content on the surface of the original silicon wafer includes: S1: mixing m1 grams of original silicon wafer fragments with v1 liter of a first acidic solution, and when the surface of the original silicon wafer fragments becomes hydrophilic, taking out the original silicon wafer fragments and collecting a first extract; S2: heating and evaporating the first extract, and then re-dissolving it with a second acidic solution and fixing the volume to v1 liter to obtain a first sample solution; S3: using ICP-MS to test the metal ion concentration in the first sample solution to be a1 micrograms / liter; S4: calculating the metal content on the surface of the original silicon wafer by the following formula: ω 表 =(a1×v1×10 -6 ) / m1×100%.

[0023] The present invention finds that directly detecting the metal ion concentration in the first extract results in a high detection result; subsequent studies have found that the above problem can be avoided by using a method of evaporating the first extract and then re-dissolving and fixing the volume with a second acidic solution.

[0024] Preferably, the first acidic solution is a dilute hydrofluoric acid solution.

[0025] The present invention finds that the hydrofluoric acid of the above concentration only corrodes the surface of silicon oxide, and the silicon corrosion speed is extremely slow. When corroding the sample, no over-corrosion will occur, and the detection stability and repeatability are good.

[0026] And / or, the second acidic solution is a nitric acid solution.

[0027] According to a preferred embodiment provided by the present invention, the concentration of the first acidic solution and the concentration of the second acidic solution are independently, the same or different and are 2 wt % to 5 wt %.

[0028] According to a preferred embodiment provided by the present invention, in S1, m1 is 0.3 g to 0.6 g; v1 is 20 ml to 40 ml.

[0029] According to a preferred embodiment provided by the present invention, in S1, the mixing time is 2 minutes to 10 minutes.

[0030] According to a preferred embodiment provided by the present invention, the testing method of the metal content on the surface of the original silicon wafer includes: S1': mixing m2 grams of original silicon wafer fragments with v2 liters of mixed acid solution, and obtaining a second extract after the reaction is completed; S2': heating and evaporating the second extract, and then using the second acid solution to redissolve and fix the volume to v2 liters to obtain a second sample solution; S3': using ICP-MS to test the metal ion concentration in the second sample solution to be a2 micrograms / liter; S4': calculating the metal content on the surface of the original silicon wafer by the following formula: ω 总 =(a2×v1×10 -6 ) / m2×100%.

[0031] The present invention finds that directly detecting the metal ion concentration in the second extract results in a high detection result; subsequent studies have found that the above problem can be avoided by evaporating the second extract and then re-dissolving and fixing the volume with a second acidic solution.

[0032] According to a preferred embodiment provided by the present invention, the mixed acid solution comprises nitric acid and hydrofluoric acid in a mass ratio of 4 to 6:1, and the concentration of the nitric acid in the mixed acid solution is 30 to 45 wt %.

[0033] According to a preferred embodiment provided by the present invention, in S1', m2 is 0.4 g to 0.6 g; v1 is 20 ml to 40 ml.

[0034] According to a preferred embodiment provided by the present invention, in S1', v2 liters of the mixed acid solution are added to m2 grams of original silicon wafer fragments in batches at 30-60 degrees Celsius.

[0035] According to a preferred embodiment provided by the present invention, the method for testing the metal content in the original silicon wafer includes: respectively detecting the metal content in the body of the original silicon wafer and the metal content on the surface of the original silicon wafer, and subtracting the metal content on the surface of the original silicon wafer from the metal content on the surface of the original silicon wafer to obtain the metal content.

[0036] The testing method for the metal content on the surface of the original silicon wafer includes: S1: mixing m1 grams of original silicon wafer fragments with v1 liter of 2wt% to 5wt% dilute hydrofluoric acid, and when the surface of the original silicon wafer fragments becomes hydrophilic, taking out the original silicon wafer fragments and collecting the first extract; S2: heating and evaporating the first extract, and then re-dissolving it with 2wt% to 5wt% nitric acid solution and fixing the volume to v1 liter to obtain a first sample solution; S3: using ICP-MS to test the metal ion concentration in the first sample solution to be a1 micrograms / liter; S4: calculating the metal content on the surface of the original silicon wafer by the following formula: ω 表 =(a1×v1×10 -6 ) / m1×100%.

[0037] In S1 of the present invention, when m1 gram of original silicon wafer fragments are mixed with v1 liter of dilute hydrofluoric acid, the method includes: adding dilute hydrofluoric acid to a fluorine-proof beaker for weighing samples until the silicon wafer is covered, reacting for 10 to 20 minutes, clamping the silicon wafer with fluorine-proof tweezers, and rinsing the front and back surfaces of the silicon wafer two to three times with an acidic solution, collecting the rinsing liquid and the soaking liquid together in a beaker, and the rinsing liquid and the soaking liquid together account for v1 liter.

[0038] The testing method for the metal content on the surface of the original silicon wafer includes: S1': mixing m2 grams of original silicon wafer fragments with v2 liters of mixed acid solution, and obtaining a second extract after the reaction is completed; S2': heating and evaporating the second extract, and then re-dissolving it with 2wt% to 5wt% nitric acid solution and fixing the volume to v2 liters to obtain a second sample solution; S3': using ICP-MS to test the metal ion concentration in the second sample solution to be a2 micrograms / liter; S4': calculating the metal content on the surface of the original silicon wafer by the following formula: ω 总 =(a2×v1×10 -6 ) / m2×100%.

[0039] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 .

[0040] In S1' of the present invention, at 30 to 60 degrees Celsius, a small amount of mixed acid is dripped into a fluorine-proof beaker containing m2 grams of original silicon wafer fragments for multiple times; specifically, when the mixed acid is dripped, violent yellow smoke emerges, and the container is covered in time. When the reaction is no longer violent, the mixed acid is continued to be added, and the acid is stopped when the single amount is repeatedly added. After dissolving for 0.5 to 1.5 hours, the reaction is completed when the yellow smoke no longer emerges.

[0041] In the present invention, the container used when the original silicon wafer fragments are mixed with the acid may be made of PP material, or may be an acid-resistant container that does not contain metal impurities, which is not limited here.

[0042] In the following examples, the original silicon wafer is wrapped in a dust-free cloth, and the surface of the original silicon wafer is gently tapped using a tool that does not contain metal components to obtain original silicon wafer fragments.

[0043] In the following examples, "%" represents mass percentage unless otherwise specified.

[0044] Example 1

[0045] This embodiment provides a method for testing the nickel content in an original silicon wafer (the resistivity of the original silicon wafer is 0.3 to 0.7 ohm / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.35 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.32 g of original silicon wafer fragments are obtained.

[0046] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.02 L to obtain a first sample solution.

[0047] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution, it is 0.23 μg / L.

[0048] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω 表 =(0.23×0.02×10 -6 ) / 0.35×100%=0.00000131%.

[0049] Test of metal content on the surface of original silicon wafer: S1': 0.37 g of original silicon wafer fragments were mixed with 0.02 liter of mixed acid solution to obtain a second extract.

[0050] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0051] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 0.24 μg / L.

[0052] S4': Calculate the metal content of the original silicon wafer surface by the following formula: ω 总 =(0.24×0.05×10 -6 ) / 0.37×100%=0.00000320%.

[0053] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 =0.00000189%.

[0054] Example 2

[0055] This embodiment provides a method for testing the nickel content in an original silicon wafer (the resistivity of the original silicon wafer is 1.2 to 1.7 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.35 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.32 g of original silicon wafer fragments are obtained.

[0056] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.02 L to obtain a first sample solution.

[0057] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution, it is 0.34 μg / L.

[0058] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω 表 =(0.34×0.02×10 -6 ) / 0.35×100%=0.00000194%.

[0059] Test of metal content on the surface of original silicon wafer: S1': 0.4 g of original silicon wafer fragments are mixed with 0.02 liter of mixed acid solution to obtain a second extract.

[0060] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0061] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 0.22 μg / L.

[0062] S4': Calculate the metal content of the original silicon wafer surface by the following formula: ω 总 =(0.22×0.05×10 -6 ) / 0.4×100%=0.00000303%.

[0063] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 =0.00000109%.

[0064] Example 3

[0065] This embodiment provides a method for testing the nickel content in an original silicon wafer (the resistivity of the original silicon wafer is 0.7 to 1.2 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.35 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.32 g of original silicon wafer fragments are obtained.

[0066] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.02 L to obtain a first sample solution.

[0067] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution is 0.33 μg / L.

[0068] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω 表 =(0.33×0.02×10 -6 ) / 0.35×100%=0.00000189%.

[0069] Test of metal content on the surface of original silicon wafer: S1': 0.41 g of original silicon wafer fragments were mixed with 0.02 liters of mixed acid solution to obtain a second extract.

[0070] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0071] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 0.23 μg / L.

[0072] S4': Calculate the metal content of the original silicon wafer surface by the following formula: ω 总=(0.23×0.05×10 -6 ) / 0.41×100%=0.00000316%.

[0073] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 =0.00000127%.

[0074] Example 4

[0075] This embodiment provides a method for testing the nickel content in an original silicon wafer (the resistivity of the original silicon wafer is 0.7 to 1.2 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.35 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.32 g of original silicon wafer fragments are obtained.

[0076] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.02 L to obtain a first sample solution.

[0077] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution is 0.30 μg / L.

[0078] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω 表 =(0.30×0.02×10 -6 ) / 0.35×100%=0.00000143%.

[0079] Test of metal content on the surface of original silicon wafer: S1': 0.41 g of original silicon wafer fragments were mixed with 0.02 liters of mixed acid solution to obtain a second extract.

[0080] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0081] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 0.20 μg / L.

[0082] S4': Calculate the metal content of the original silicon wafer surface by the following formula: ω 总 =(0.20×0.05×10 -6 ) / 0.41×100%=0.00000276%.

[0083] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 =0.00000133%.

[0084] Example 5

[0085] This embodiment provides a method for testing the nickel content in an original silicon wafer (the resistivity of the original silicon wafer is 0.7 to 1.2 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.34 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.31 g of original silicon wafer fragments are obtained.

[0086] S2: Collect the first extract to obtain a first sample solution.

[0087] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution, it is 20.03 μg / L.

[0088] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω 表 =(20.03×0.02×10 -6 ) / 0.34×100%=0.00011782%.

[0089] Test of metal content on the surface of original silicon wafer: S1': 0.37 g of the original silicon wafer fragments were mixed with 0.02 liters of mixed acid solution to obtain a second extract, and after the reaction was completed, the mixed acid solution was added to 0.05 liters to obtain a second sample solution.

[0090] S2': The nickel metal ion concentration in the second sample solution was measured by ICP-MS and found to be 0.47 μg / L.

[0091] S3': Calculate the metal content of the original silicon wafer surface by the following formula: ω 总 =(0.47×0.05×10 -6 ) / 0.37×100%=0.00000636%.

[0092] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 =-0.00011146%.

[0093] Example 6

[0094] This embodiment provides a method for testing the magnesium content in an original silicon wafer (the resistivity of the original silicon wafer is 0.3 to 0.7 ohm / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.37 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.35 g of original silicon wafer fragments are obtained.

[0095] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.03 L to obtain a first sample solution.

[0096] S3: Using ICP-MS to measure the nickel metal ion concentration in the first sample solution, it is 1.36 μg / L.

[0097] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω 表 =(1.36×0.03×10 -6 ) / 0.37×100%=0.00001103%.

[0098] Test of metal content on the surface of original silicon wafer: S1': 0.42 g of original silicon wafer fragments were mixed with 0.02 liter of mixed acid solution to obtain a second extract.

[0099] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0100] S3': The nickel metal ion concentration in the second sample solution is measured by ICP-MS and is 8.17 μg / L.

[0101] S4': Calculate the metal content of the original silicon wafer surface by the following formula: ω 总 =(8.17×0.05×10 -6 ) / 0.42×100%=0.000097%.

[0102] The metal content in the original silicon wafer is: 体 =ω 总 -ω 表 =0.00008623%.

[0103] Example 7

[0104] This embodiment provides a method for testing the magnesium content in an original silicon wafer (the resistivity of the original silicon wafer is 0.7 to 1.2 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.34 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.32 g of original silicon wafer fragments are obtained.

[0105] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.03 L to obtain a first sample solution.

[0106] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution is 0.99 μg / L.

[0107] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω table = (0.99 × 0.03 × 10 -6 ) / 0.34×100%=0.00000874%.

[0108] Test of metal content on the surface of original silicon wafer: S1': 0.46 g of original silicon wafer fragments were mixed with 0.02 liter of mixed acid solution to obtain a second extract.

[0109] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0110] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 2.88 μg / L.

[0111] S4': The metal content of the original silicon wafer is calculated by the following formula: ωtotal = (2.88 × 0.05 × 10 -6 ) / 0.46×100%=0.000031%.

[0112] The metal content in the original silicon wafer is: ω body = ω total - ω surface = 0.00002257%.

[0113] Example 8

[0114] This embodiment provides a method for testing the magnesium content in an original silicon wafer (the resistivity of the original silicon wafer is 1.2 to 1.7 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.38 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.36 g of original silicon wafer fragments are obtained.

[0115] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.03 L to obtain a first sample solution.

[0116] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution is 0.02 μg / L.

[0117] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω table = (0.02 × 0.03 × 10 -6 ) / 0.38×100%=0.00000016%.

[0118] Test of metal content on the surface of original silicon wafer: S1': 0.34 g of original silicon wafer fragments were mixed with 0.02 liters of mixed acid solution to obtain a second extract.

[0119] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0120] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 1.01 μg / L.

[0121] S4': The metal content of the original silicon wafer is calculated by the following formula: ωtotal = (1.01 × 0.05 × 10 -6 ) / 0.34×100%=0.000015%.

[0122] The metal content in the original silicon wafer is: ω body = ω total - ω surface = 0.00001470%.

[0123] Example 9

[0124] This embodiment provides a method for testing the iron content in an original silicon wafer (the resistivity of the original silicon wafer is 0.3-0.7 ohm / m2), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.37 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.35 g of original silicon wafer fragments are obtained.

[0125] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.03 L to obtain a first sample solution.

[0126] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution, it is 3.74 μg / L.

[0127] S4: Calculate the nickel element metal content of the original silicon wafer by the following formula: ω table = (3.74 × 0.03 × 10 -6 ) / 0.37×100%=0.00003032%.

[0128] Test of metal content on the surface of original silicon wafer: S1': 0.42 g of original silicon wafer fragments were mixed with 0.02 liter of mixed acid solution to obtain a second extract.

[0129] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0130] S3': The nickel metal ion concentration in the second sample solution is measured by ICP-MS and is 15.52 μg / L.

[0131] S4': The metal content of the original silicon wafer is calculated by the following formula: ωtotal = (15.52 × 0.05 × 10 -6 ) / 0.42×100%=0.000185%

[0132] The metal content in the original silicon wafer is: ω body = ω total - ω surface = 0.00015444%.

[0133] Example 10

[0134] This embodiment provides a method for testing the iron content in an original silicon wafer (the resistivity of the original silicon wafer is 0.7 to 1.2 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.34 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.32 g of original silicon wafer fragments are obtained.

[0135] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.03 L to obtain a first sample solution.

[0136] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution, it is 4.79 μg / L.

[0137] S4: Calculate the nickel metal content of the original silicon wafer by the following formula: ω table = (4.79 × 0.03 × 10 -6) / 0.34×100%=0.00004226%.

[0138] Test of metal content on the surface of original silicon wafer: S1': 0.46 g of original silicon wafer fragments were mixed with 0.02 liter of mixed acid solution to obtain a second extract.

[0139] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0140] S3': The nickel metal ion concentration in the second sample solution is measured by ICP-MS and is 14.16 μg / L.

[0141] S4': The metal content of the original silicon wafer is calculated by the following formula: ωtotal = (14.16 × 0.05 × 10 -6 ) / 0.46×100%=0.000154%

[0142] The metal content in the original silicon wafer is: ω body = ω total - ω surface = 0.00011165%.

[0143] Embodiment 11

[0144] This embodiment provides a method for testing the iron content in an original silicon wafer (the resistivity of the original silicon wafer is 1.2 to 1.7 ohms / square meter), comprising the following steps: Test of metal content on the original silicon wafer surface: S1: 0.38 g of original silicon wafer fragments are mixed with 0.02 liters of 2 wt% dilute hydrofluoric acid. When the surface of the original silicon wafer fragments becomes hydrophilic, the original silicon wafer fragments are taken out and the first extract is collected. After drying, 0.36 g of original silicon wafer fragments are obtained.

[0145] S2: The first extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.03 L to obtain a first sample solution.

[0146] S3: Using ICP-MS to test the nickel metal ion concentration in the first sample solution, it is 4.15 μg / L.

[0147] S4: Calculate the nickel metal content of the original silicon wafer by the following formula: ω table = (4.15 × 0.03 × 10 -6 ) / 0.38×100%=0.00003276%.

[0148] Test of metal content on the surface of original silicon wafer: S1': 0.34 g of original silicon wafer fragments were mixed with 0.02 liters of mixed acid solution to obtain a second extract.

[0149] S2': The second extract is heated and evaporated, and then redissolved with a 5 wt % nitric acid solution and fixed to 0.05 L to obtain a second sample solution.

[0150] S3': Using ICP-MS to measure the nickel metal ion concentration in the second sample solution, it is 6.08 μg / L.

[0151] S4': The metal content of the original silicon wafer is calculated by the following formula: ωtotal = (6.08 × 0.05 × 10 6 ) / 0.34×100%=0.000089%

[0152] The metal content in the original silicon wafer is: ω body = ω total - ω surface = 0.00005665%.

[0153] Test example

[0154] The present invention further verifies the accuracy of the detection method provided in the above embodiment, and the results are shown in Table 1.

[0155] Table 1 Table Metal Content Surface metal content Body metal content Example 1 0.00000131% 0.000003209% 0.00000189% Example 2 0.00000194% 0.00000303% 0.00000109% Example 3 0.00000189% 0.00000316% 0.00000127% Example 4 0.00000143% 0.00000276% 0.00000133% Example 5 0.00011782% 0.00000636% -0.00011146% Example 6 0.00001103% 0.000097% 0.00008623% Example 7 0.00000874% 0.000031% 0.00002257% Example 8 0.00000016% 0.000015% 0.000014709% Example 9 0.00003032% 0.000185% 0.00015444% Example 10 0.00004226% 0.000154% 0.00011165% Embodiment 11 0.00003276% 0.000089% 0.00005665%

[0156] The results show that when the evaporation and re-dissolution operations are omitted and the concentration of metal ions in the extract is directly detected, the detection results of the metal content on the surface of the original silicon wafer and the metal content on the surface of the original silicon wafer will be higher to varying degrees, and ultimately the detection results of the metal content in the original silicon wafer will be inaccurate. At the same time, it can be seen that the test results are in line with the rule that the higher the resistivity of the original silicon wafer, the lower the metal content in the body, and the detection accuracy is relatively high.

[0157] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for testing the metal content in an original silicon wafer, characterized in that: include: The metal content of the original silicon wafer body and the metal content on the surface of the original silicon wafer are detected respectively, and the metal content in the original silicon wafer body is subtracted from the metal content on the surface of the original silicon wafer to obtain the metal content in the original silicon wafer body.

2. The method for testing the metal content in the original silicon wafer according to claim 1, characterized in that: The testing method for the metal content on the surface of the original silicon wafer includes: S1: mixing m1 grams of original silicon wafer fragments with v1 liter of the first acidic solution, and when the surface of the original silicon wafer fragments is hydrophilic, taking out the original silicon wafer fragments and collecting the first extract; S2: heating and evaporating the first extract, and then using the second acidic solution to redissolve and fix the volume to v1 liter to obtain a first sample solution; S3: using ICP-MS to test the metal ion concentration in the first sample solution to be a1 micrograms / liter; S4: calculating the metal content on the surface of the original silicon wafer by the following formula: ω 表 =(a1×v1×10 -6 ) / m1×100%.

3. The method for testing the metal content in the original silicon wafer according to claim 2, characterized in that: The first acidic solution is a dilute hydrofluoric acid solution; and / or the second acidic solution is a nitric acid solution.

4. The method for testing the metal content in the original silicon wafer according to claim 3, characterized in that: The concentration of the first acidic solution and the concentration of the second acidic solution are independently, the same or different from each other and are 2 wt % to 5 wt %.

5. The method for testing the metal content in the original silicon wafer according to claim 2, characterized in that: In S1, m1 is 0.3 g to 0.6 g; v1 is 20 ml to 40 ml.

6. The method for testing the metal content in the original silicon wafer according to claim 2, characterized in that: In S1, the mixing time is 2 minutes to 10 minutes.

7. The method for testing the metal content in the original silicon wafer according to claim 1, characterized in that: The testing method for the metal content of the original silicon wafer surface comprises: S1': mixing m2 grams of original silicon wafer fragments with v1 liter of mixed acid solution, and obtaining a second extract after the reaction is completed; S2': heating and evaporating the second extract, and then re-dissolving it with the second acid solution and fixing the volume to v2 liters to obtain a second sample solution; S3': using ICP-MS to test that the metal ion concentration in the second sample solution is a2 micrograms / liter; S4': calculating the metal content of the original silicon wafer surface by the following formula: ω 总 =(a2×v2×10 -6 ) / m2×100%.

8. The method for testing the metal content in the original silicon wafer according to claim 7, characterized in that: The mixed acid solution comprises nitric acid and hydrofluoric acid in a mass ratio of 4 to 6:1, and the concentration of the nitric acid in the mixed acid solution is 30 to 45 wt %.

9. The method for testing the metal content in the original silicon wafer according to claim 7, characterized in that: In S1', m2 is 0.4 g to 0.6 g; v1 is 20 ml to 40 ml.

10. The method for testing the metal content in the original silicon wafer according to claim 7, characterized in that: In S1', v2 liters of the mixed acid solution are added to m2 grams of original silicon wafer fragments in portions at 30-60 degrees Celsius.

Citation Information

Cited By

  • Electronic-grade polycrystalline silicon surface metal detection method by scanning appearance

    CN121364235A