Optical fiber coupler and preparation method thereof
By controlling the tapering parameters and heat shrink protection process, the polarization-related loss of the fiber coupler is reduced, solving the problems of high polarization loss and high production cost of the existing fiber coupler, and realizing efficient and low-cost mass production of fiber couplers. .
Patent Information
- Application Number
- CN202410984197.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fiber couplers have high polarization-related losses, which makes it difficult to meet the high performance requirements of laser radar technology for fiber couplers. In addition, the grinding efficiency is low and the cost is high during the production process, making it difficult to achieve mass production.
By setting the tapering parameters and preheating, including oxygen flow and hydrogen flow, remove the optical fiber coating and clean it, taper at the preset speed until it reaches the preset shape, fix and take out the tapered fused optical fiber for heat shrinkage For protection, a fiber optic coupler is obtained, and the cross-sectional area of the coupling connection area is within a preset range to reduce polarization-dependent losses.
It achieves low polarization-related loss of the optical fiber coupler, reduces production costs, improves production efficiency, and facilitates mass production.
Smart Images

Figure CN118732169A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optical fiber couplers, and in particular to an optical fiber coupler and a preparation method thereof. Background Art
[0002] Fiber coupler is a transmission device used in fiber optic communication networks. It has the function of redistributing the optical power or wavelength of the input signal and is widely used in optical communications, EDFA, automobiles and other fields. The PDL (polarization dependent loss) of existing technologies can only reach a level of 0.1dB, and some are even 0.15dB, which can meet the general use of optical communications. With the continuous development of lidar technology, higher and higher requirements are placed on the performance of fiber couplers. Polarization characteristics are an important characteristic of fiber couplers. High-performance systems need to be composed of low-PDL devices, so the existing taper process needs to be optimized to meet development requirements.
[0003] The technical solution described in the patent document with application number 201110456358.1 is to grind two optical fibers separately, then merge the two grinded surfaces together, fuse them together with a high-temperature heating source, and finally accurately control the splitting ratio of the coupler by continuing the melting process or taper. Before the formal fusion, it is necessary to ensure that the two grinded surfaces are close to each other. In actual production, it is difficult to merge the two grinded surfaces together, and it is also difficult to ensure the grinding accuracy. In addition, the grinding efficiency is low and cannot meet the supply of the taper process. Therefore, the cost is high and it is not suitable for mass production. Summary of the invention
[0004] In view of this, in order to solve one of the above problems, an embodiment of the present invention aims to provide a fiber coupler and a preparation method thereof, wherein the fiber coupler has low polarization-dependent loss, can reduce production costs, and is convenient for mass production.
[0005] On the one hand, an embodiment of the present invention provides a fiber coupler, comprising a first optical fiber and a second optical fiber, wherein the first optical fiber is coupled to the second optical fiber, and the cross-sectional area of the coupling connection region is within a preset range, and the preset range is determined based on the first end face area of the first optical fiber and the second end face area of the second optical fiber.
[0006] Optionally, the cross-section has a circular or elliptical shape.
[0007] The implementation of the embodiment of the present invention includes the following beneficial effects: the first optical fiber is coupled to the second optical fiber in the optical fiber coupler, and the cross-sectional area of the coupling connection region is within a preset range, and the preset range is determined based on the first end face area of the first optical fiber and the second end face area of the second optical fiber, that is, the coupling connection region of the first optical fiber and the second optical fiber is within the preset range, thereby reducing the polarization-related loss of the optical fiber coupler.
[0008] On the other hand, an embodiment of the present invention provides a method for preparing an optical fiber coupler, comprising:
[0009] Setting the taper parameters and preheating, wherein the taper parameters include oxygen flow rate and hydrogen flow rate;
[0010] Removing the coating layer of the first optical fiber and cleaning it, placing it in a fixture, and completing the pre-drawing operation;
[0011] removing the coating layer of the second optical fiber and cleaning it, placing it in the fixture, and performing tapering at a preset speed until a preset taper shape is achieved;
[0012] The tapered fused optical fiber is fixed and taken out, and heat-shrinked for protection to obtain an optical fiber coupler.
[0013] Optionally, the ratio of the oxygen flow rate to the hydrogen flow rate is in the range of 0.7 to 0.9.
[0014] Optionally, the oxygen flow rate ranges from 100 to 200 sccm, and the hydrogen flow rate ranges from 160 to 240 sccm.
[0015] Optionally, the distance between the oxygen outlet and the hydrogen outlet is in the range of 6 to 12 mm.
[0016] Optionally, the oxygen outlet includes an oxygen pocket, the oxygen pocket includes uniform outlet holes, and the density of the outlet holes meets preset requirements.
[0017] Optionally, the preset speed ranges from 30-220 um / sec.
[0018] Optionally, during the preparation process, heating is performed by a burner, wherein the material of the burner comprises ceramic or glass.
[0019] Optionally, during the preparation process, the flame heating temperature ranges from 2500 to 3000°C.
[0020] The implementation of the embodiment of the present invention includes the following beneficial effects: first, setting the taper parameters and preheating, the taper parameters including oxygen flow rate and hydrogen flow rate; then, removing the coating layer of the first optical fiber and cleaning it, placing it in a fixture, and completing the pre-drawing operation; then, removing the coating layer of the second optical fiber and cleaning it, placing it in a fixture, and tapering it at a preset speed until a preset taper shape is reached; finally, fixing and taking out the fused optical fiber after tapering, performing heat shrinking protection, and obtaining an optical fiber coupler; during the preparation process, controlling the taper parameters, placing the two optical fibers in the same fixture one after another, and performing tapering and heat shrinking protection according to preset requirements to obtain an optical fiber coupler, and no grinding and alignment are required during the preparation process, which reduces the process difficulty and cost, improves production efficiency, and facilitates mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a schematic structural diagram of a cross section of a coupling connection region of an optical fiber coupler provided by an embodiment of the present invention;
[0022] Figure 2 is a schematic diagram of a device for preparing an optical fiber coupler provided in an embodiment of the present invention;
[0023] Figure 3 It is a schematic flow chart of the steps of a method for preparing an optical fiber coupler provided by an embodiment of the present invention;
[0024] Figure 4 is a structural schematic diagram of a clamp provided by an embodiment of the present invention;
[0025] Figure 5 is a normal distribution diagram of polarization-dependent loss of an optical fiber coupler with a splitting ratio of 1 / 99 and a wavelength of 1550 nm provided in an embodiment of the present invention;
[0026] Figure 6 is a normal distribution diagram of polarization-dependent loss of an optical fiber coupler with a splitting ratio of 50 / 50 and a wavelength of 1550 nm provided in an embodiment of the present invention;
[0027] Figure 7 It is a normal distribution diagram of polarization-dependent loss of an optical fiber coupler with a splitting ratio of 50 / 50 and a wavelength of 980 nm provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The step numbers in the following embodiments are only provided for the convenience of explanation and description, and the order between the steps is not limited in any way. The execution order of each step in the embodiment can be adaptively adjusted according to the understanding of those skilled in the art.
[0029] Polarization Dependent Loss (PDL): also known as polarization-dependent sensitivity, refers to the maximum change in the output optical power of each output port when the polarization state of the transmission signal changes 360° (for single-mode devices). The unit is dB and the mathematical expression is:
[0030]
[0031] Among them, PDL i Refers to the polarization-dependent loss of output port i; MinP outi Refers to the minimum output optical power of output port i when the polarization state of the transmission signal changes 360°; MaxP outiRefers to the maximum output optical power at output port i when the polarization state of the transmitted signal changes 360°.
[0032] An embodiment of the present invention provides an optical fiber coupler, including a first optical fiber and a second optical fiber, wherein the first optical fiber is coupled to the second optical fiber, and the cross-sectional area of the coupling connection region is within a preset range, and the preset range is determined based on the first end face area of the first optical fiber and the second end face area of the second optical fiber.
[0033] See also Figure 1 There are many possible cross-sections of the coupling connection region between the first optical fiber and the second optical fiber, such as Figure 1 As shown in (a), the cross-section of the coupling connection area between the first optical fiber and the second optical fiber is larger, that is, the overlap area between the first optical fiber and the second optical fiber is smaller, and the polarization-dependent loss is higher; Figure 1 As shown in (b), the cross-section of the coupling connection area between the first optical fiber and the second optical fiber is smaller, that is, the overlap area between the first optical fiber and the second optical fiber is larger, and the polarization-dependent loss is smaller; Figure 1 As shown in (c), the cross-section of the coupling connection region between the first optical fiber and the second optical fiber is smaller, that is, the first optical fiber and the second optical fiber completely overlap, and the polarization-dependent loss is smaller.
[0034] It should be noted that the first end face area of the first optical fiber and the second end face area of the second optical fiber may be the same or different. When the first optical fiber is the same as the second optical fiber, the first end face area of the first optical fiber and the second end face area of the second optical fiber are the same. Specifically, a total area is determined based on the sum of the first end face area and the second end face area, and a preset range can be determined based on the total area and the preset area ratio.
[0035] Optionally, the cross-sectional shape comprises a circle or an ellipse.
[0036] The shape of the cross section can reflect the cross-sectional area of the coupling connection region between the first optical fiber and the second optical fiber. The shape of the cross section is circular or elliptical, which indicates that there are more overlapping areas corresponding to the coupling connection region between the first optical fiber and the second optical fiber, and the polarization-related loss is smaller.
[0037] The implementation of the embodiment of the present invention includes the following beneficial effects: the first optical fiber is coupled to the second optical fiber in the optical fiber coupler, and the cross-sectional area of the coupling connection region is within a preset range, and the preset range is determined based on the first end face area of the first optical fiber and the second end face area of the second optical fiber, that is, the coupling connection region of the first optical fiber and the second optical fiber is within the preset range, thereby reducing the polarization-related loss of the optical fiber coupler.
[0038] See also Figure 2During the preparation of the optical fiber coupler, the equipment used includes but is not limited to the oxygen outlet 1-1, the hydrogen outlet 1-2 and the fire head 1-3. The oxygen flow rate is controlled by the oxygen outlet 1-1, the hydrogen flow rate is controlled by the hydrogen outlet 1-2, and the fire head is used to provide a fire source.
[0039] See also Figure 3 , an embodiment of the present invention provides a method for preparing an optical fiber coupler, comprising:
[0040] S100, setting the taper parameters and preheating, the taper parameters including oxygen flow rate and hydrogen flow rate.
[0041] It should be noted that the taper parameters include but are not limited to oxygen flow rate and hydrogen flow rate. The oxygen flow rate and hydrogen flow rate are determined according to actual applications and are not specifically limited in this embodiment.
[0042] The set taper drawing parameters are dynamically controlled, such as hydrogen flow rate and oxygen flow rate. After high oxygen preheating, the taper is drawn according to normal parameters.
[0043] Optionally, the ratio of the oxygen flow rate to the hydrogen flow rate is in the range of 0.7 to 0.9.
[0044] Optionally, the oxygen flow rate ranges from 100 to 200 sccm, and the hydrogen flow rate ranges from 160 to 240 sccm.
[0045] It should be noted that the ratio of oxygen flow rate to hydrogen flow rate is determined according to actual application, and is not specifically limited in this embodiment, such as 0.85. When the oxygen flow rate and the hydrogen flow rate satisfy the proportional relationship, a specific value can be determined within the above range.
[0046] Optionally, the distance between the oxygen outlet and the hydrogen outlet is in the range of 6 to 12 mm.
[0047] It should be noted that the distance between the oxygen outlet and the hydrogen outlet is determined according to actual application, and this embodiment does not impose any specific limitation. For example, the distance between the oxygen outlet and the hydrogen outlet is 8 mm. The distance between the oxygen outlet and the hydrogen outlet is within a suitable range, which can promote the full combustion of hydrogen and provide the required temperature for taper pulling.
[0048] Optionally, the oxygen outlet includes an oxygen pocket, the oxygen pocket includes uniform outlet holes, and the density of the outlet holes meets preset requirements.
[0049] See also Figure 2 The gas outlet is an oxygen pocket, which includes uniform gas outlet holes. The density of the gas outlet holes meets the preset requirements to ensure that the oxygen output is uniform and stable to provide sufficient oxygen, further promote the full combustion of hydrogen, and provide the temperature required for cone pulling.
[0050] S200, removing the coating layer of the first optical fiber and cleaning it, placing it in a fixture, and completing the pre-drawing operation.
[0051] See also Figure 4 , the clamp 1-4 can fix the two ends of the optical fiber 1-5. Specifically, the coating layer can be stripped by a stripping method, and during the stripping process, it is important not to lose the internal structure of the optical fiber. Cleaning can be performed by wiping or the like.
[0052] S300, removing the coating layer of the second optical fiber and cleaning it, placing it in a fixture, and performing tapering at a preset speed until a preset taper shape is achieved.
[0053] The same method as above can be used to remove the coating layer of the second optical fiber and clean it, and the cleaned second optical fiber is placed in the above fixture, and tapers at a preset speed until a preset taper shape is achieved. The preset taper shape includes but is not limited to a circle or an ellipse.
[0054] Optionally, the preset speed ranges from 30-220 um / sec.
[0055] It should be noted that the preset speed is determined according to actual application, and this embodiment does not impose any specific limitation. If the preset speed is controlled within a suitable range, the melting degree of the first optical fiber and the second optical fiber can be improved.
[0056] Optionally, during the preparation process, the flame heating temperature ranges from 2500 to 3000°C.
[0057] Optionally, during the preparation process, heating is performed by a burner, and the material of the burner includes ceramic or glass.
[0058] It should be noted that the flame heating temperature range affects the quality of the optical fiber taper, and the flame heating temperature is determined according to the actual application, and this embodiment does not impose any specific restrictions. Since the flame heating temperature is relatively high, the material of the flame head is selected to be a heat-resistant material, including but not limited to ceramics or glass.
[0059] S400, fix and take out the tapered fused optical fiber, perform heat shrink protection, and obtain an optical fiber coupler.
[0060] The tapered fused optical fiber is fixed on a quartz substrate, such as by dispensing glue, so as to characterize the tapered fused optical fiber, and then the tapered fused optical fiber is taken out, heat-shrink protected, and the tapered fused optical fiber is packaged, such as in a metal tube with multiple layers of sealing at both ends, to obtain a fiber optic coupler.
[0061] In a specific embodiment, a fiber coupler is obtained by the preparation method of the embodiment of the present invention, and the fiber coupler is tested. The test results are shown in Table 1 and Figure 5-7shown. Figure 5 It represents the normal distribution diagram of polarization-dependent loss of an optical fiber coupler with a splitting ratio of 1 / 99 and a wavelength of 1550 nm, wherein the low PDL process refers to the preparation method of an embodiment of the present invention, and the conventional parameter process refers to a conventional method for preparing an optical fiber coupler. Figure 6 It represents the normal distribution diagram of polarization-dependent loss of an optical fiber coupler with a splitting ratio of 50 / 50 and a wavelength of 1550 nm, wherein the low PDL process refers to the preparation method of an embodiment of the present invention, and the conventional parameter process refers to a conventional method for preparing an optical fiber coupler. Figure 7 It represents the normal distribution diagram of polarization-dependent loss of an optical fiber coupler with a splitting ratio of 50 / 50 and a wavelength of 980 nm, wherein the low PDL process refers to the preparation method of an embodiment of the present invention, and the conventional parameter process refers to a conventional method for preparing an optical fiber coupler.
[0062] Table 1
[0063]
[0064] In Table 1, when the splitting ratio is 1 / 99, PDL1 refers to the optical fiber with a splitting ratio of 99%, and PDL2 refers to the optical fiber with a splitting ratio of 1%; when the splitting ratio is 50 / 50, PDL1 refers to the optical fiber with a splitting ratio of 50%, and PDL2 refers to the optical fiber with a splitting ratio of the other 50%.
[0065] From Table 1 and Figure 5-7 It can be seen that the polarization-dependent loss of the optical fiber coupler obtained by the preparation method of the embodiment of the present invention is lower than 0.1, which is much higher than the industry average level, and has better stability.
[0066] The implementation of the embodiment of the present invention includes the following beneficial effects: first, setting the taper parameters and preheating, the taper parameters including oxygen flow rate and hydrogen flow rate; then, removing the coating layer of the first optical fiber and cleaning it, placing it in a fixture, and completing the pre-drawing operation; then, removing the coating layer of the second optical fiber and cleaning it, placing it in a fixture, and tapering it at a preset speed until a preset taper shape is reached; finally, fixing and taking out the fused optical fiber after tapering, performing heat shrink protection, and obtaining an optical fiber coupler; during the preparation process, controlling the taper parameters, placing the two optical fibers in the same fixture one after another, and performing tapering and heat shrink protection according to preset requirements to obtain an optical fiber coupler, and no grinding and alignment are required during the preparation process, which reduces the process difficulty and cost, improves production efficiency, and facilitates mass production.
[0067] The above is a specific description of the preferred implementation of the present invention, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A fiber coupler, characterized in that: The method comprises a first optical fiber and a second optical fiber, wherein the first optical fiber is coupled to the second optical fiber, and the cross-sectional area of the coupling connection region is within a preset range, and the preset range is determined according to the first end face area of the first optical fiber and the second end face area of the second optical fiber.
2. The optical fiber coupler according to claim 1, characterized in that: The cross-sectional shape includes a circle or an ellipse.
3. A method for preparing an optical fiber coupler, characterized in that: include: Setting the taper parameters and preheating, wherein the taper parameters include oxygen flow rate and hydrogen flow rate; Removing the coating layer of the first optical fiber and cleaning it, placing it in a fixture, and completing the pre-drawing operation; removing the coating layer of the second optical fiber and cleaning it, placing it in the fixture, and performing tapering at a preset speed until a preset taper shape is achieved; The tapered fused optical fiber is fixed and taken out, and heat-shrinked for protection to obtain an optical fiber coupler.
4. The preparation method according to claim 3, characterized in that: The ratio of the oxygen flow rate to the hydrogen flow rate is in the range of 0.7 to 0.
9.
5. The preparation method according to claim 3, characterized in that: The oxygen flow rate ranges from 100 to 200 sccm, and the hydrogen flow rate ranges from 160 to 240 sccm.
6. The preparation method according to claim 3, characterized in that: The distance between the oxygen outlet and the hydrogen outlet is in the range of 6 to 12 mm.
7. The preparation method according to claim 6, characterized in that: The oxygen outlet comprises an oxygen pocket, and the oxygen pocket comprises uniform outlet holes, and the density of the outlet holes meets preset requirements.
8. The preparation method according to claim 3, characterized in that: The preset speed ranges from 30 to 220 um / sec.
9. The preparation method according to claim 3, characterized in that: During the preparation process, heating is performed by a burner, the material of which includes ceramic or glass.
10. The preparation method according to claim 3, characterized in that: During the preparation process, the flame heating temperature ranges from 2500 to 3000°C.
Citation Information
Patent Citations
Manufacturing process for optical fiber coupler
CN102520485A