Photosensitive resin composition, dry film, cured product, and printed wiring board
By using a photosensitive resin composition of inorganic fillers, acryloyl or methacryloyl compounds, photopolymerization initiators and inorganic colloids in the solder resist of printed wiring boards, the solder resist has solved the problem of high thermal expansion rate, poor burying ability and durability. The problem of insufficient crack resistance improves the insulation reliability and stability of electronic components.
Patent Information
- Application Number
- CN202410349940.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-01
AI Technical Summary
The solder resist of existing printed wiring boards has problems in electronic components such as high thermal expansion rate, poor buryability and insufficient crack resistance, resulting in reduced insulation reliability and stability of electronic components.
A photosensitive resin composition containing an inorganic filler, an acryloyl or methacryloyl compound, a photopolymerization initiator and an inorganic colloid is used. By adjusting the composition proportions and processing methods, a dry resin composition with low thermal expansion rate and high landfillability is formed. Film used to prepare solder resist for printed wiring boards.
It reduces the thermal expansion rate of the solder resist, improves the filling property and crack resistance, and enhances the insulation reliability and stability of electronic components.
Smart Images

Figure BDA0004759625550000251 
Figure BDA0004759625550000261 
Figure BDA0004759625550000291
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition and further to a dry film, a cured product and a printed wiring board using the photosensitive resin composition. Background Art
[0002] In recent years, with the demand for miniaturization and high performance of electronic components, semiconductor chips mounted on electronic components are also being densified and highly functionalized. Along with this, printed wiring boards on which semiconductor chips are mounted are also required to be miniaturized and densified. In order to manufacture printed wiring boards with high integration, insulating materials (e.g., solder resists, insulating films, etc.) with high definition and reliability are being developed.
[0003] As electronic components are miniaturized, printed wiring boards on which semiconductor chips are mounted are required to have higher smoothness. This is because when electronic components are mounted on printed wiring boards, if there is a height deviation on the surface of the printed wiring board, the connection between the electronic components and the printed wiring board becomes unstable and reliability decreases. Therefore, the solder resist for the outermost layer of the printed wiring board is preferably a dry film type solder resist with high surface smoothness (for example, Patent Document 1).
[0004] Dry film type solder resist is formed by heating and pressing on a printed wiring board using a vacuum laminator or other device. At this time, if the solder resist is not properly buried between wirings of the printed wiring board, the insulation reliability of the electronic components will be significantly reduced. Therefore, in order to allow the solder resist to be properly buried even in difficult-to-access areas such as between wirings, improvements such as improving fluidity have been made.
[0005] However, with the recent miniaturization of electronic components, the wiring of printed wiring boards has become even finer, and dry film type solder resists are required to have high filling properties.
[0006] In addition, the heat generated by electronic components has increased due to the performance improvement. As a result, the volume change caused by heating and cooling of insulating materials such as solder resist constituting electronic components has increased, and the stress generated has also increased. The solder resist cannot withstand the increased stress and cracks are generated, causing failure of electronic components. Therefore, it is required to improve the crack resistance of the solder resist.
[0007] In order to improve the crack resistance of solder resist, it is necessary to suppress the stress caused by volume change due to heating / cooling. To this end, it is widely known that suppressing the volume change of solder resist or making its thermal expansion coefficient consistent with the various constituent materials in contact with the solder resist is an effective method.
[0008] In this case, the solder resist preferably has a low thermal expansion coefficient. In order to reduce the thermal expansion coefficient, high filling of inorganic fillers is effective, but if the filling amount of the inorganic filler is increased, there is a problem that the melt viscosity increases and the filling property decreases.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2011-13486. Summary of the invention
[0012] Therefore, the object of the present invention is to provide a photosensitive resin composition that can form a cured product with a low thermal expansion coefficient and suppress the increase in melt viscosity to improve the embedding property. In addition, the object of the present invention is to provide a dry film having a resin layer composed of a dry coating film of the resin composition, a cured product of the resin layer of the resin composition or the dry film, and a printed wiring board having the cured product.
[0013] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that by adding an inorganic filler, a compound having at least one acryloyl group or methacryloyl group in one molecule, a photopolymerization initiator and an inorganic colloid to a photosensitive resin composition, a photosensitive resin composition can be obtained that can form a cured product with a low thermal expansion coefficient, suppress an increase in melt viscosity, and improve embedding properties.
[0014] That is, according to the present invention, the following inventions are provided.
[0015] [1] A photosensitive resin composition comprising (A) an inorganic filler, (B) a compound having at least one acryloyl group or methacryloyl group in one molecule, (C) a photopolymerization initiator, and (D) an inorganic colloid, wherein the total amount of the (A) inorganic filler and the (D) inorganic colloid is 30.0% by mass or more based on solid content relative to the total amount of the photosensitive resin composition, and the amount of the (D) inorganic colloid is 2.0% by mass or more based on solid content relative to the total amount of the photosensitive resin composition, and the melt viscosity of the photosensitive resin composition at 100° C. is less than 1000 dPa·s.
[0016] [2] The photosensitive resin composition according to [1], wherein the surface area of the inorganic colloid (D) is 100 m 2 / g or above.
[0017] [3] The photosensitive resin composition according to [1] or [2], wherein the (D) inorganic colloid is colloidal silica having an average particle size of 30 nm or less and subjected to a silane coupling treatment on the surface.
[0018] [4] The photosensitive resin composition according to [3], wherein the colloidal silica is colloidal silica to which an acryloyl group or a methacryloyl group is added in a portion less than 50% of the total surface area.
[0019] [5] The photosensitive resin composition according to [3] or [4], wherein the colloidal silica is colloidal silica derived from sodium silicate.
[0020] [6] The photosensitive resin composition according to any one of [3] to [5], wherein the density of the colloidal silica is 1.9 to 2.2.
[0021] [7] The photosensitive resin composition according to any one of [1] to [6], wherein the average particle size of the (A) inorganic filler is 200 nm or more and less than 1000 nm.
[0022] [8] The photosensitive resin composition according to any one of [1] to [7], wherein the (A) inorganic filler is silica having an acryloyl group or a methacryloyl group added to the surface by a silane coupling treatment.
[0023] [9] The photosensitive resin composition according to any one of [1] to [8], wherein the (A) inorganic filler and the (D) inorganic colloid are spherical.
[0024]
[10] The photosensitive resin composition according to any one of [1] to [9], wherein the ratio of the average particle size of the (A) inorganic filler to the average particle size of the (D) inorganic colloid is 8 or more.
[0025]
[11] The photosensitive resin composition according to any one of [1] to
[10] , further comprising (E) a carboxyl group-containing resin.
[0026]
[12] A dry film comprising a first film and a resin layer formed on the first film and composed of a dry coating film of the photosensitive resin composition according to any one of [1] to
[11] .
[0027]
[13] A cured product, characterized in that the cured product is obtained by curing the photosensitive resin composition according to any one of [1] to
[11] .
[0028]
[14] A cured product, characterized in that the cured product is obtained by curing the resin layer of the dry film described in
[12] .
[0029]
[15] A printed wiring board, characterized in that the printed wiring board comprises the cured product described in
[13] .
[0030]
[16] A printed wiring board, characterized in that the printed wiring board comprises the cured product described in
[14] .
[0031] According to the present invention, it is possible to provide a photosensitive resin composition that can form a cured product with a low thermal expansion coefficient, suppress the increase in melt viscosity, and improve the embedding property. Furthermore, according to the photosensitive resin composition of the present invention, it is also possible to reduce the thermal expansion coefficient. In addition, according to the present invention, it is possible to provide a dry film having a resin layer composed of a dry coating film of the resin composition, a cured product of the resin layer of the resin composition or the dry film, and a printed wiring board having the cured product. DETAILED DESCRIPTION
[0032] [Photosensitive resin composition]
[0033] The photosensitive resin composition according to the present invention contains at least (A) an inorganic filler, (B) a compound having at least one acryloyl group or methacryloyl group in one molecule, (C) a photopolymerization initiator, and (D) an inorganic colloid. The photosensitive resin composition according to the present invention may also contain (E) a carboxyl-containing resin, a thermosetting component, a cation trapping agent, a colorant, an organic solvent, and other additives. The following describes the components constituting the photosensitive resin composition of the present invention.
[0034] The melt viscosity of the photosensitive composition at 100° C. is less than 1000 dPa·s, preferably less than 900 dPa·s, and more preferably less than 700 dPa·s.
[0035] When the melt viscosity of the photosensitive composition at 100° C. is less than 1000 dPa·s, the embedding property in the circuit can be improved.
[0036] In the present invention, the melt viscosity of the photosensitive composition at 100° C. is a value measured under the following conditions using a vacuum laminator CVP-300 manufactured by Nikko Materials Co., Ltd., by laminating dry films at a lamination temperature of 30 to 40° C. to produce a resin layer having a thickness of 300 μm and a width of 20 mm, and using a rheometer MARS40.
[0037] (Measuring conditions of melt viscosity)
[0038] Heating rate: 5℃ / min.
[0039] Frequency: 1Hz.
[0040] Pressure: 3Pa.
[0041] ((A) Inorganic filler)
[0042] The average particle size of the inorganic filler is preferably 200 nm or more and less than 1000 nm, more preferably 250 nm or more and 900 nm or less, and 300 nm or more and 800 nm or less.
[0043] The photosensitive resin composition has good embedding properties by containing the inorganic filler having the above-mentioned average particle diameter.
[0044] In addition, the ratio of the average particle size of the inorganic filler to the average particle size of the inorganic colloid (average particle size of the inorganic filler / average particle size of the inorganic colloid) is preferably 8 or more, more preferably 8 or more and 100 or less, and further preferably 8 or more and 50 or less. If the ratio of the average particle size of the inorganic colloid to the average particle size of the inorganic filler is within the above numerical range, the landfilling property is good.
[0045] In the present invention, the average particle size of the inorganic filler is a volume average particle size (D50 volume %) measured by a dynamic light scattering method using a laser diffraction measuring device.
[0046] Specifically, the average particle size of the inorganic filler can be measured by the following method.
[0047] Particle size distribution meter: Microtrac MT3300EX manufactured by Nikkiso Co., Ltd.
[0048] Circulation device: ASVR manufactured by Nikkiso Co., Ltd.
[0049] First, enter the measurement conditions according to the following steps. Start the software ("Particle Size Distribution Measurement") that comes with Microtrac, enter from the SET UP screen, and set the time from the measurement condition setting options. Set the start time (Set zero) to 30 sec., the measurement to 30 sec., and the number of measurements to 2 times. Then, enter the analysis conditions. In the analysis information, set the particle refractive index to 1.81 (fixed value: the average value of the refractive index of all inorganic substances), in the particle characteristics, set the transmittance to transparent, and set the shape to non-spherical. In addition, in the solvent information, select PMA (propylene glycol monomethyl ether acetate) and set the solvent refractive index to 1.4. Then, enter the scale setting. In the particle size range, set the minimum particle size to 0.021μm and the maximum particle size to 704μm. Then, enter the sampling system. Set the number of washes of ASVR to 4 times, the flow rate to 50%, the ultrasonic output to 40W, and the ultrasonic time to 300sec. After entering all measurement conditions, press Save and Close in the Measurement Conditions Settings.
[0050] Next, adjust the sample according to the following steps. As a sample, an inorganic filler before being mixed with the photosensitive resin composition is used. In the case of mixing an inorganic filler with a powder, the powder is used as a sample. In the case of dispersing an inorganic filler in a solvent or the like and mixing it, the solvent dispersion is used as a sample. Weigh 0.3g of the sample and place it in a threaded bottle, gradually add 30g of propylene glycol monomethyl ether acetate using a pipette, and disperse the sample by shaking the threaded bottle to make an adjustment sample. The adjustment sample is not externally dispersed or pre-dispersed. Then, the adjustment sample is measured. Click on the particle size distribution measurement of the software attached to Microtrac and open the sample loading screen. Use a pipette to drip a few drops of the adjustment sample into the sample inlet of the main body. In the sample loading screen, when the red indicator bar is displayed, drip the adjustment sample into the sample inlet until it enters the green range from red. After entering the green range, press the measurement button to start the measurement. From sample adjustment to the measurement of the adjustment sample is carried out within 5 minutes. The value of the cumulative volume average diameter 50% shown as the measurement result was defined as the value of the average particle diameter D50.
[0051] At least a portion of the surface of the inorganic filler is preferably a treated inorganic filler to improve the dispersibility in the photosensitive resin composition. In particular, it is preferred to implement a surface treatment that can introduce curable reactive groups to the surface of the inorganic filler. Here, as long as the curable reactive group is a group that undergoes a curing reaction with a compound having at least one acryloyl or methacryloyl group in one molecule of (B) and a curable compound such as a carboxyl-containing resin (E), there is no particular limitation, and it can be a photocurable reactive group or a thermosetting reactive group. As photocurable reactive groups, acryloyl, methacryloyl, vinyl, styryl, etc. can be cited. As thermosetting reactive groups, epoxy, amino, hydroxyl, carboxyl, isocyanate, imino, oxetanyl, mercapto, methoxymethyl, methoxyethyl, ethoxymethyl, ethoxyethyl, oxazoline, etc. can be cited.
[0052] The method for introducing curable reactive groups into the surface of the inorganic filler is not particularly limited, and it can be introduced by using a known and conventional method. For the surface treatment agent having curable reactive groups, for example, it can be treated with a coupling agent having curable reactive groups as an organic group. As the coupling agent, coupling agents such as silane, titanate, aluminate, and aluminozirconate can be used. Among them, silane coupling agents are preferred. Examples of silane coupling agents include vinyl trimethoxysilane, vinyl triethoxysilane, N-(2-aminomethyl)-3-aminopropyl methyl dimethoxysilane, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 3-anilinopropyl trimethoxysilane, 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl methyl dimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-mercaptopropyl trimethoxysilane, etc. They can be used alone or in combination. The treatment amount of the silane coupling agent is preferably 0.5 to 10 parts by mass relative to 100 parts by mass of the inorganic filler.
[0053] The type of inorganic filler is not particularly limited, and conventionally known inorganic fillers can be used. As the inorganic filler, for example, silicon dioxide, crystalline silicon dioxide, Neuburg Siliceous Earth, aluminum hydroxide, glass powder, talc, clay, magnesium carbonate, calcium carbonate, natural mica, synthetic mica, aluminum hydroxide, barium sulfate, barium titanate, iron oxide, non-fibrous glass, hydrotalcite, mineral wool, aluminum silicate, calcium silicate, zinc flower, etc. can be used. Among them, silicon dioxide is preferred, and spherical silicon dioxide is more preferred.
[0054] The amount of the inorganic filler in terms of solid content relative to the total amount of the photosensitive resin composition is preferably 2.4% by mass or more, more preferably 2.4% by mass or more and less than 60.0% by mass, and further preferably 2.4% by mass or more and less than 50.0% by mass. If the amount of the inorganic filler is within the above numerical range, the embedding property is good.
[0055] Relative to the total amount of the photosensitive resin composition, the total amount of the inorganic filler and the inorganic colloid described later is converted to 30.0 mass % or more according to the solid content, preferably 30.0 mass % or more and less than 60.0 mass %, more preferably 30.0 mass % or more and less than 50.0 mass %. If the total amount of the inorganic filler and the inorganic colloid is within the above numerical range, a cured product with a low thermal expansion coefficient can be formed, and the embedding property is good.
[0056] ((B) Compound having at least one acryloyl group or methacryloyl group in one molecule)
[0057] The compound having at least one acryloyl group or methacryloyl group in one molecule is used as a reactive diluent to reduce the melt viscosity of the photosensitive resin composition. The compound having at least one acryloyl group or methacryloyl group in one molecule may be used alone or in combination of two or more.
[0058] The upper limit of the molecular weight of the compound having at least one acryloyl group or methacryloyl group in one molecule is preferably 600 g / mol or less, and more preferably 550 g / mol or less. In addition, the lower limit of the molecular weight of the compound having at least one acryloyl group or methacryloyl group in one molecule is not particularly limited, and may also be preferably 300 g / mol or more. By setting the molecular weight of the compound having at least one acryloyl group or methacryloyl group in one molecule to 600 g / mol or less, the melt viscosity of the photosensitive resin composition is reduced, and the embedding property of the circuit can be improved.
[0059] As a compound having at least one acryloyl group or methacryloyl group in one molecule, it is sufficient as long as the above-mentioned molecular weight is satisfied, and examples thereof include well-known and commonly used polyester (meth)acrylates, polyether (meth)acrylates, polyurethane (meth)acrylates, carbonate (meth)acrylates, epoxy (meth)acrylates, etc. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; alkyl acrylates such as hydroxy 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or di-acrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-hydroxymethylacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; polyols such as hexyl glycol, trimethylolpropane, pentaerythritol, di(trimethylol)propane, dipentaerythritol, and trihydroxyethyl isocyanurate, or these alkylene oxides. Polyacrylates such as polyols such as propylene glycol adducts or ε-caprolactone adducts; polyacrylates such as phenols such as phenoxy acrylate and bisphenol A diacrylate or these alkylene oxide adducts; acrylates from glycidyl ethers such as glycerol diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; not limited to the above, it can be appropriately selected from acrylates obtained by directly acrylateing polyols such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadiene, and polyester polyols, or urethane acrylated via diisocyanates, melamine acrylates, and at least any one of the methacrylates corresponding to the above acrylates.
[0060] The amount of the compound having at least one acryloyl group or methacryloyl group in one molecule is preferably 4.0% by mass or more, more preferably 4.0% by mass or more and 10% by mass or less, and further preferably 4.0% by mass or more and 8.0% by mass or less, relative to the total amount of the photosensitive resin composition. When the amount of the compound having at least one acryloyl group or methacryloyl group in one molecule is 4.0% by mass or more, the viscosity of the photosensitive resin composition is suppressed from increasing, the photocurability is good, and a pattern is easily formed in the alkali development after irradiation with active energy rays.
[0061] ((C) Photopolymerization initiator)
[0062] The photopolymerization initiator is a photopolymerization initiator used to react at least one of (B) a compound having at least one acryloyl group or methacryloyl group in one molecule and (E) a carboxyl group-containing resin by exposure. As the photopolymerization initiator, any known photopolymerization initiator can be used. The photopolymerization initiator can be used alone or in combination of two or more.
[0063] Specific examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-xylylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-xylylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bisacylphosphine oxide; 2,6-dimethoxybenzoyl 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphine oxide, methyl 2,4,6-trimethylbenzoylphenylphosphine oxide, 2-methylbenzoyldiphenylphosphine oxide, isopropyl pivaloylphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide and other monoacylphosphine oxides; ethyl phenyl (2,4,6-trimethylbenzoyl) phosphonate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane-1-one, 2-hydroxy-2-methyl-1-phenylpropane-1-one, etc. Hydroxyacetophenones; benzoins such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylaminobenzophenone) and other benzophenones; acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholine-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)-butanone-1,2-(dimethylamino)- Acetophenones such as 2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone, N,N-dimethylaminoacetophenone, etc.; thioxanthones such as 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone, etc.; anthraquinones such as anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, 2-aminoanthraquinone, etc.; ketals such as acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.; benzoates such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and ethyl p-dimethylbenzoate;1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime)], ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyloxime) and other oxime esters; bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium and other titanocenes; phenyl disulfide 2-nitrofluorene, butyroquinone, anisole ether, azobisisobutyronitrile, tetramethylthiuram disulfide, etc.;
[0064] Examples of commercially available products of the α-aminoacetophenone-based photopolymerization initiator include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins BV.
[0065] Examples of commercially available products of the acylphosphine oxide-based photopolymerization initiator include Omnirad 819 manufactured by IGM Resins B.V. and the like.
[0066] Examples of commercially available oxime ester photopolymerization initiators include Irgacure OXE01 and OXE02 manufactured by BASF Japan, N-1919, Adeka Arkls NCI-831 and NCI-831E manufactured by Adeka Corporation, and TR-PBG-304 manufactured by Changzhou Qiangli Electronic New Materials Co., Ltd.
[0067] In addition, carbazole oxime ester compounds described in JP-A-2004-359639, JP-A-2005-097141, JP-A-2005-220097, JP-A-2006-160634, JP-A-2008-094770, JP-T-2008-509967, JP-T-2009-040762, and JP-A-2011-80036 can be cited.
[0068] Relative to the total amount of the photosensitive resin composition, the amount of the photopolymerization initiator is preferably 0.5% by mass or more and 5.0% by mass or less, and more preferably 0.5% by mass or more and 3.0% by mass or less, in terms of solid content. When the amount of the photopolymerization initiator is 0.5% by mass or more, the photocurability of the photosensitive resin composition is good, and the coating properties such as chemical resistance are also good. On the other hand, when the amount of the photopolymerization initiator is 5.0% by mass or less, the light absorption on the surface of the resist film (cured coating) is good, and the deep curability is difficult to reduce.
[0069] A photoinitiator aid or sensitizer can be used together with the above-mentioned photopolymerization initiator. As a photoinitiator aid or sensitizer, benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds and xanthone compounds can be cited. Particularly preferably, thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 4-isopropylthioxanthone are used. By containing thioxanthone compounds, deep curing can be improved. These compounds can sometimes also be used as photopolymerization initiators, preferably in combination with photopolymerization initiators. In addition, a photoinitiator aid or sensitizer can be used alone or in combination of two or more.
[0070] It should be noted that these photopolymerization initiators, light initiation auxiliary agents and sensitizers absorb specific wavelengths, so that, depending on the circumstances, the sensitivity decreases and sometimes plays a role as a UV absorber. However, these are not only used to improve the sensitivity of resin combination. As required, absorbing the light of a specific wavelength improves the photoreactivity on the surface, and the line shape and opening of the resist pattern can be changed into vertical, cone-shaped, inverted cone-shaped and the precision of line width and opening diameter can be improved.
[0071] ((D) Inorganic colloid)
[0072] The inorganic colloid in the present invention can use a known and commonly used inorganic colloid, preferably synthesized by various liquid phase methods, and therefore, preferably not once become a dry powder until it is incorporated into the photosensitive resin composition. The nanoparticles of the dry powder are difficult to redisperse, causing secondary aggregation, and the reduction of the melt viscosity becomes unstable.
[0073] The amount of the inorganic colloid is 2% or more, preferably 2.0% or more and less than 47.0% or more, more preferably 2.0% or more and less than 30.0% or more, based on the solid content relative to the total amount of the photosensitive resin composition. If the amount of the inorganic colloid is within the above numerical range, the embedding property is good.
[0074] The surface area of the inorganic colloid is preferably 100 m 2 / g or more, more preferably 100m 2 / g and above and 250m 2 / g or less, more preferably 150m 2 / g and above and 250m 2 When the surface area of the inorganic colloid is within the above numerical range, the landfilling property is good. In the present invention, the surface area of the inorganic colloid is a value calculated by the BET method using a nitrogen adsorption device.
[0075] In order to improve the dispersibility in the photosensitive resin composition, the inorganic colloid is preferably colloidal silica after at least a portion of the surface is treated. In particular, it is preferred to implement a surface treatment that can introduce curable reactive groups into the surface of the inorganic colloid. Here, as long as the curable reactive group is a group that undergoes a curing reaction with a compound having at least one acryloyl or methacryloyl group in one molecule of (B) and a curable compound such as a carboxyl-containing resin (E), there is no particular limitation, and it can be a photocurable reactive group or a thermosetting reactive group. As photocurable reactive groups, acryloyl, methacryloyl, vinyl, styrene, etc. can be cited. As thermosetting reactive groups, epoxy, amino, hydroxyl, carboxyl, isocyanate, imino, oxetane, mercapto, methoxymethyl, methoxyethyl, ethoxymethyl, ethoxyethyl, oxazoline, etc. can be cited. Among them, acryloyl or methacryloyl is preferred. In particular, it is preferred that the inorganic colloid has acryloyl or methacryloyl in a portion less than 50% of the total surface area.
[0076] The method for introducing curable reactive groups into the surface is not particularly limited, and any known and commonly used method can be used, as long as the surface of the inorganic filler is treated with a surface treatment agent having a curable reactive group, such as a coupling agent having a curable reactive group as an organic group. As the coupling agent, the same coupling agent as that used for the surface treatment of the inorganic filler can be used. The treatment amount of the silane coupling agent is preferably 0.5 to 10 parts by mass relative to 100 parts by mass of the inorganic colloid.
[0077] The average particle size of the inorganic colloid is preferably 30 nm or less, more preferably 5 nm or more and 25 nm or less, further preferably 5 nm or more and 15 nm or less, and particularly preferably 5 nm or more and 12 nm or less. The photosensitive resin composition containing the inorganic colloid having the above average particle size can reduce the melt viscosity and improve the embedding property.
[0078] Colloidal silicon dioxide is preferably in the form of sodium silicate (Na 2 SiO 3 , also called "water glass") as a raw material and converted into colloidal silica by neutralization or ion exchange. The method for producing colloidal silica is not particularly limited. As an example, sodium silicate is used as a raw material to prepare a sodium silicate aqueous solution (also called water glass), acid is added to the sodium silicate aqueous solution to obtain colloidal particles, the colloidal particles are treated with an ion exchange resin, and then a base is added to adjust the pH to obtain colloidal silica. The average particle size of colloidal silica can be adjusted by the concentration of the aqueous solution when preparing the colloidal particles. Specifically, colloidal silica having a desired average particle size can be obtained by a known method such as that described in Japanese Patent Publication No. 06-16414.
[0079] The average particle size of colloidal silica derived from sodium silicate can be adjusted according to the conditions during manufacturing. In addition, as colloidal silica derived from sodium silicate, a commercially available product having an average particle size within the above range can be used directly. As specific examples, Snowtex (registered trademark) manufactured by Nissan Chemical Co., Ltd. can be cited: (product number) ST-XS, ST-S, ST-30, ST-50-T, ST-UP, ST-PS-S, ST-PS-M, ST-OXS, ST-OS, ST-O, ST-O-40, ST-OUP, ST-PS-SO, ST-PS-MO, ST-NXS, ST-NS, ST-N, ST-N-40, ST-CXS, ST-C, ST-CM, ST-AK; organic silica sol manufactured by Nissan Chemical Co., Ltd.: (product number) MA-ST-M , IPA-ST, IPA-ST-UP, NPC-ST-30, PGM-ST, PGM-ST-UP, DMAC-ST, NMP-ST, MEK-ST-40, MEK-ST-UP, MIBK-ST, CHO-ST-M, EAC-ST, PMA-S T, TOL-ST, MEK-AC-2140Z, PGM-AC-2140Y, PGM-AC-3140Y, MIBK-AC-2140Z, MEK-EC-2130Y, MEK-EC-2430Z, EP-M2130Y, EP-M2230Y, etc.
[0080] Colloidal silica derived from sodium silicate may also be blended in a slurry state. By blending in a slurry state, high dispersion is easily achieved, aggregation is prevented, and silica having an average particle size within the above-specified range is easy to handle.
[0081] The colloidal silica derived from sodium silicate may be used alone or in combination of two or more.
[0082] The density of colloidal silica is preferably 1.9 or more and 2.2 or less, and more preferably 2.0 or more and 2.2 or less. When the density of colloidal silica is within the above numerical range, the embedding property is good.
[0083] ((E) Carboxyl-containing resin)
[0084] As the carboxyl-containing resin, various resins known in the past having a carboxyl group in the molecule can be used. The carboxyl-containing resin may or may not have an ethylenically unsaturated double bond in the molecule. In particular, from the aspects of photocurability and development resistance, a carboxyl-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is preferred. It should be noted that when the photosensitive resin composition of the present invention contains a carboxyl-containing resin, it can be used not only for purposes of alkali development, but also for purposes without alkali development. Preferably, the ethylenically unsaturated double bond is derived from acrylic acid or methacrylic acid or their derivatives. When only a carboxyl-containing resin without an ethylenically unsaturated double bond is used, in order to make the composition photocurable, a compound having at least one acryloyl or methacryloyl group in one molecule of the above-mentioned (B) is required. As specific examples of carboxyl-containing resins, the following compounds (which may be any one of oligomers and polymers) can be cited.
[0085] (1) Carboxyl group-containing resins obtained by copolymerization of an unsaturated carboxylic acid such as (meth)acrylic acid with a compound containing an unsaturated group such as styrene, α-methylstyrene, a lower alkyl (meth)acrylate, or isobutylene (as the lower alkyl (meth)acrylate, methyl (meth)acrylate can be mentioned).
[0086] (2) Carboxyl-containing polyurethane resins produced by the addition polymerization of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds containing carboxyl groups such as dimethylol propionic acid and dimethylol butyric acid, and dihydroxy compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0087] (3) Carboxyl-containing photosensitive polyurethane resins produced by the addition reaction of diisocyanates with (meth)acrylates of bifunctional epoxy resins such as bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, dimethylol epoxy resin, biphenol epoxy resin or their partially anhydride-modified products, carboxyl-containing diol compounds and diol compounds.
[0088] (4) In the synthesis of the resin of (2) or (3), a compound having one hydroxyl group and one or more (meth)acryloyl groups is added to a molecule of a hydroxyalkyl (meth)acrylate to prepare a carboxyl-containing photosensitive polyurethane resin having terminal (meth)acryloyl groups.
[0089] (5) In the synthesis of the resin of (2) or (3), a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as equimolar reactants of isophorone diisocyanate and pentaerythritol triacrylate, is added to obtain a carboxyl-containing photosensitive polyurethane resin that is terminally (meth)acryloylated.
[0090] (6) A carboxyl group-containing photosensitive resin obtained by reacting a bifunctional or higher polyfunctional (solid) epoxy resin with (meth)acrylic acid to add a dibasic acid anhydride to a hydroxyl group present in a side chain.
[0091] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin obtained by epoxidizing the hydroxyl groups of a bifunctional (solid) epoxy resin using epichlorohydrin with (meth)acrylic acid, and adding a dibasic acid anhydride to the generated hydroxyl groups.
[0092] (8) A carboxyl-containing polyester resin obtained by reacting a bifunctional oxetane resin with a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid, and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the generated primary hydroxyl group.
[0093] (9) A carboxyl-containing photosensitive resin is obtained by reacting an epoxy compound having a plurality of epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule such as p-hydroxyphenylethanol and a monocarboxylic acid containing an unsaturated group such as (meth)acrylic acid, so that the alcoholic hydroxyl group of the reaction product reacts with a polyacid anhydride such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, etc.
[0094] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0095] (11) A carboxyl-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, the resulting reaction product with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polyacid anhydride.
[0096] (12) A carboxyl-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins of (1) to (11).
[0097] It should be noted that, in the present specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and a mixture thereof, and the same applies to other similar expressions.
[0098] The carboxyl group-containing resin that can be used in the present invention is not limited to the carboxyl group-containing resins listed above. In addition, the carboxyl group-containing resins listed above can be used alone or in combination of a plurality of types.
[0099] In the present invention, considering the developability when using a weak alkaline developer such as sodium carbonate aqueous solution and the drawing property of the resist pattern, the acid value of the carboxyl-containing resin is preferably in the range of 30 to 150 mgKOH / g, and more preferably in the range of 50 to 120 mgKOH / g. The higher the acid value of the carboxyl-containing resin, the more the developability is improved, but in order to dissolve the exposed part with the developer, sometimes the exposed part and the unexposed part are not distinguished and dissolved and peeled with the developer.
[0100] The weight average molecular weight of carboxyl resin is different because of the difference of resin skeleton, and is usually in the range of 1500 to 150000, and is preferably in the range of 1800 to 100000. By using carboxyl resin with a weight average molecular weight of more than 2000, clarity and surface dryness can be improved. In addition, by using carboxyl resin with a weight average molecular weight of less than 150000, developability and storage stability can be improved. The weight average molecular weight can be measured by gel permeation chromatography (GPC).
[0101] Relative to the total amount of the photosensitive resin composition, the amount of the carboxyl resin is preferably 20.0% by mass or more and 40.0% by mass or less, more preferably 20.0% by mass or more and 30.0% by mass or less, based on solid content. By setting the amount of the carboxyl resin to 20.0% by mass or more, the photoreactivity of the photosensitive resin composition can be improved. In addition, by setting the amount of the carboxyl resin to 40.0% by mass or less, the thermal linear expansion coefficient can be reduced.
[0102] (Thermosetting component)
[0103] The photosensitive resin composition of the present invention may contain a thermosetting component in addition to the above-mentioned components. Examples of the thermosetting component include known and commonly used compounds such as isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy resins, oxetane compounds, and episulfide resins. Among them, the preferred thermosetting component is epoxy resin.
[0104] Examples of the epoxy resin include bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, triphenylmethane type epoxy resin, and the like. These may be used alone or in combination of two or more.
[0105] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Group Corporation, YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by NIPPON STEEL Chemical & Material Co., Ltd., EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation, and RE-306 manufactured by Nippon Kayaku Co., Ltd.
[0106] The equivalent of the epoxy group of the epoxy resin in the photosensitive resin composition is preferably 0.5 to 2.5 in terms of solid content relative to 1 equivalent of the carboxyl group of the carboxyl-containing resin. By setting it to 0.5 equivalents or more, the residual carboxyl group in the cured product can be prevented, and good heat resistance, alkali resistance, electrical insulation, etc. can be obtained. In addition, by setting the above-mentioned amount to 2.5 equivalents or less, it is possible to prevent low-molecular-weight cyclic (sulfide) ether groups from remaining in the dried coating film, and the strength of the cured product can be well ensured.
[0107] When the photosensitive resin composition of the present invention contains a thermosetting component, a thermosetting catalyst for accelerating the curing of the thermosetting component may also be contained. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, 4-methyl-N,N-dimethylbenzylamine, hydrazine compounds such as adipic acid dihydrazide, sebacic acid dihydrazide, and phosphorus compounds such as triphenylphosphine. In addition, commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole compounds) manufactured by Shikoku Chemical Industry Co., Ltd., U-CAT 3513N (a trade name of a dimethylamine compound) manufactured by San-Apro Ltd., DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and salts thereof), etc.
[0108] It is not limited to the above-mentioned compound, as long as it is a thermosetting catalyst of epoxy resin, oxetane compound or a compound that promotes at least any one of epoxy group and oxetane and the reaction of carboxyl, it can be used alone or by mixing more than two kinds. In addition, it is also possible to use guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine-isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-S-triazine-isocyanuric acid adduct, etc. S-triazine derivatives, preferably these are also used as the compound and thermosetting catalyst that the adhesion imparting agent plays a role.
[0109] The thermosetting catalyst may be used alone or in combination of two or more. From the viewpoint of the storage stability of the photosensitive resin composition and the heat resistance of the cured coating film, the amount of the thermosetting catalyst is preferably 0.1% by mass or more and 10.0% by mass or less, and more preferably 0.3% by mass or more and 5.0% by mass or less, based on the solid content relative to the total amount of the photosensitive resin composition.
[0110] (Cationic collector)
[0111] As the cation-trapping agent, a compound capable of trapping cations by ion exchange can be used. The cation-trapping agent may be used alone or in combination of two or more.
[0112] The cation trapping agent is preferably an inorganic compound with a positively or negatively charged layered structure, preferably an inorganic compound with a positively charged layered structure. In particular, with respect to the ion exchange capacity of the cation trapping agent, Na + Preferably 2.0 meq / g or more or Cu 2+ It is preferably 2.2 meq / g or more.
[0113] Examples of the cation scavenger include hydrotalcite. Hydrotalcite is a compound represented by the following formula (1).
[0114] Mg a Al b (OH) c (CO 3 ) d ·nH 2 O(1)
[0115] (In formula (1), a, b, c and d are positive numbers, satisfying 2a+3b-c-2d=0. In addition, n represents the number of hydrations, which is 0 or a positive number, preferably 1 to 5.)
[0116] In formula (1), those in which a part of Mg is replaced by other divalent metal ions can also be preferably used. Among other divalent metal ions, Zn is particularly preferred.
[0117] Specific examples of hydrotalcite include, but are not particularly limited to, Mg 4.5 Al 2 (OH) 13 CO 3 ·nH 2 O、Mg 5 Al 1.5 (OH) 12.5 CO 3 ·nH 2 O、Mg 6 Al 2 (OH) 16 CO 3 ·nH 2 O、Mg 4.2 Al 2 (OH) 12.4 CO 3 ·nH 2 O、Mg 4.3 Al 2 (OH) 12.6 CO 3 ·nH 2 O、Mg 2.5 Zn 2 Al 2 (OH) 13 CO3 ·nH 2 O、Mg 4.2 Al 2 (OH) 12.4 CO 3 ·nH 2 O、Mg 4.2 Al 2 (OH) 12.4 CO 3 ·nH 2 O、Mg 4 Al 2 (OH) 12 CO 3 ·nH 2 O, etc. (In the above, n represents the number of hydration, which is 0 or a positive number, preferably 1 to 5.), among which Mg is preferred 4.3 Al 2 (OH) 12.6 CO 3 ·nH 2 O.
[0118] In the hydrotalcite represented by the formula (1), a / b is preferably 1.5 or more and 5 or less, more preferably 1.7 or more and 3 or less, and further preferably 1.8 or more and 2.5 or less.
[0119] As the cation scavenger, commercially available products may be used, and examples thereof include "IXEPLAS-A1", "IXEPLAS-A2", and "IXEPLAS-B1" manufactured by Toagosei Co., Ltd.
[0120] The amount of the cation scavenger is 0.2% by mass or more, preferably 0.2% by mass or more and 5.0% by mass or less, and more preferably 0.2% by mass or more and 3.0% by mass or less, based on the solid content relative to the total amount of the photosensitive resin composition. By setting the amount of the cation scavenger to 0.2% by mass or more, the insulation reliability can be improved.
[0121] (Colorant)
[0122] The photosensitive resin composition of the present invention can be mixed with a colorant. The colorant is not particularly limited, and known colorants such as red, blue, green, and yellow can be used. The colorant may be any of a pigment, a dye, and a coloring agent, but from the viewpoint of reducing environmental load and having little effect on the human body, a halogen-free colorant is preferred.
[0123] As red colorants, there are monoazo colorants, disazo colorants, azo lake colorants, benzimidazolone colorants, perylene colorants, diketopyrrolopyrrole colorants, condensed azo colorants, anthraquinone colorants, quinacridone colorants, etc. Specifically, colorants with color index (CI; issued by The Society of Dyers and Colourists) numbers as shown below can be cited.
[0124] Examples of the monoazo red colorant include Pigment Red 1, 2, 3, 4, 5, 6, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 112, 114, 146, 147, 151, 170, 184, 187, 188, 193, 210, 245, 253, 258, 266, 267, 268, and 269. Examples of the disazo red colorant include Pigment Red 37, 38, and 41. In addition, examples of monoazo lake red colorants include Pigment Red 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 52:2, 53:1, 53:2, 57:1, 58:4, 63:1, 63:2, 64:1, 68, etc. In addition, examples of benzimidazolone red colorants include Pigment Red 171, 175, 176, 185, 208, etc. In addition, examples of perylene red colorants include Solvent Red 135, 179, Pigment Red 123, 149, 166, 178, 179, 190, 194, 224, etc. In addition, examples of diketopyrrolopyrrole red colorants include Pigment Red 254, 255, 264, 270, 272, etc. In addition, examples of condensed azo red colorants include Pigment Red 220, 144, 166, 214, 220, 221, and 242. In addition, examples of anthraquinone red colorants include Pigment Red 168, 177, and 216, and Solvent Red 149, 150, 52, and 207. In addition, examples of quinacridone red colorants include Pigment Red 122, 202, 206, 207, and 209.
[0125] As blue colorants, there are phthalocyanine-based and anthraquinone-based colorants. As pigment-based colorants, there are compounds classified as pigments, such as Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, and 60. As dye-based colorants, there are solvent blue 35, 63, 68, 70, 83, 87, 94, 97, 122, 136, 67, and 70. In addition to the above, metal-substituted or unsubstituted phthalocyanine compounds can also be used.
[0126] Examples of yellow colorants include monoazo colorants, disazo colorants, condensed azo colorants, benzimidazolone colorants, isoindolinone colorants, and anthraquinone colorants. For example, anthraquinone yellow colorants include solvent yellow 163, pigment yellow 24, 108, 193, 147, 199, and 202. Examples of isoindolinone yellow colorants include pigment yellow 110, 109, 139, 179, and 185. Examples of condensed azo yellow colorants include pigment yellow 93, 94, 95, 128, 155, 166, and 180. Examples of benzimidazolone yellow colorants include pigment yellow 120, 151, 154, 156, 175, and 181. Examples of the monoazo yellow colorant include Pigment Yellow 1, 2, 3, 4, 5, 6, 9, 10, 12, 61, 62, 62:1, 65, 73, 74, 75, 97, 100, 104, 105, 111, 116, 167, 168, 169, 182, and 183. Examples of the disazo yellow colorant include Pigment Yellow 12, 13, 14, 16, 17, 55, 63, 81, 83, 87, 126, 127, 152, 170, 172, 174, 176, 188, and 198.
[0127] In addition, a colorant such as purple, orange, brown, or black may be added. Specifically, pigment black 1, 6, 7, 8, 9, 10, 11, 12, 13, 18, 20, 25, 26, 28, 29, 30, 31, 32, pigment violet 19, 23, 29, 32, 36, 38, 42, solvent violet 13, 36, CI pigment orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, 73, pigment brown 23, 25, and carbon black may be mentioned.
[0128] The amount of the colorant blended is preferably 0.3% by mass or more and 1.0% by mass or less, and more preferably 0.3% by mass or more and 0.6% by mass or less, in terms of solid content, relative to the total amount of the photosensitive resin composition.
[0129] (Organic Solvent)
[0130] The photosensitive resin composition of the present invention may contain an organic solvent for the purpose of preparing the composition, adjusting the viscosity when coating on a substrate or a film, etc. As the organic solvent, ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, diethylene glycol monoethyl ether acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha, and the like, and the well-known and commonly used organic solvents. These organic solvents may be used alone or in combination of two or more.
[0131] The amount of the organic solvent to be added is not particularly limited, and can be appropriately set according to the target viscosity so that the photosensitive resin composition can be easily prepared.
[0132] (Other added ingredients)
[0133] According to need, the photosensitive resin composition of the present invention can also be formulated with cyanate compounds, elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper poison inhibitors, antioxidants, rust inhibitors, thickeners, silicon-based, fluorine-based, polymer-based defoamers and leveling agents, at least one of imidazole-based, thiazole-based, triazole-based silane coupling agents, phosphonates, phosphate derivatives, phosphorus compounds such as phosphazene compounds, and other flame retardants. These can use substances known in the field of electronic materials.
[0134] The photosensitive resin composition of the present invention can also be used in the form of a dry film.
[0135] [Preparation method]
[0136] In the preparation of the photosensitive resin composition of the present invention, each component is weighed and blended, and then pre-stirred with a stirrer. Then, each component is dispersed with a kneading machine and kneaded to prepare the composition.
[0137] As the above-mentioned kneading machine, for example, a bead mill, a ball mill, a sand mill, a three-roll mill, a two-roll mill, etc. can be cited. Among them, in order to improve dispersibility, a bead mill is preferably used. The dispersion conditions such as the type and particle size of the beads of the bead mill can be appropriately set according to the target viscosity.
[0138] [use]
[0139] The photosensitive resin composition of the present invention is useful for forming a pattern layer as a permanent coating of a printed wiring board such as a solder resist, a cover layer, or an interlayer insulating layer, and is particularly useful for forming a solder resist. In addition, since the photosensitive resin composition of the present invention can form a cured product having excellent film strength even in the form of a thin film, it can also be applied to forming a pattern layer in a printed wiring board that requires thin filming, such as a package substrate (a printed wiring board for a semiconductor package).
[0140] The photosensitive resin composition of the present invention can be used not only for forming a pattern layer of a cured coating film but also for forming no pattern layer, for example, molding (encapsulation).
[0141] [Dry film]
[0142] The photosensitive resin composition of the present invention can also be set to a dry film form having a first film and a resin layer composed of a dry coating film of the above-mentioned photosensitive resin composition formed on the first film. The first film in the present invention refers to a film that is at least bonded to the resin layer when laminated and integrally molded in a manner such that the resin layer side composed of the above-mentioned photosensitive resin layer formed on the dry film contacts a substrate such as a substrate by heating, etc. The first film can be peeled off from the resin layer in the process after lamination. In particular, in the present invention, it is preferably peeled off from the resin layer in the process after exposure. When the dry film is formed, the photosensitive resin composition of the present invention is diluted with the above-mentioned organic solvent and adjusted to an appropriate viscosity, and applied to the first film with a uniform thickness by a comma coater, a blade coater, a lip coater, a rod coater, an extrusion coater, a reverse coating method, a transfer roll coater, a gravure coater, a spray coater, etc., and usually dried at a temperature of 50 to 130°C for 1 to 30 minutes, so that a film can be obtained. The coating film thickness is not particularly limited, but is usually appropriately selected within the range of 1 to 150 μm, preferably 5 to 60 μm, as the film thickness after drying.
[0143] As the first film, any known film can be used without particular limitation, and for example, films made of thermoplastic resins such as polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamide-imide films, polypropylene films, and polystyrene films can be preferably used. Among them, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, and operability. In addition, a laminate of these films can also be used as the first film.
[0144] Furthermore, from the viewpoint of improving mechanical strength, the thermoplastic resin film as described above is preferably a film stretched in a uniaxial direction or a biaxial direction.
[0145] The thickness of the first film is not particularly limited, and can be, for example, 10 μm to 150 μm.
[0146] After forming a resin layer consisting of a dry coating of the photosensitive resin composition of the present invention on the first film, further, for the purpose of preventing dust from adhering to the surface of the resin layer, a second film that can be peeled off is preferably stacked on the surface of the resin layer. The second film in the present invention refers to a film that is peeled off from the photosensitive resin layer before lamination when the resin layer side of the photosensitive film laminate is laminated and integrally formed on a substrate such as a substrate by heating, etc. As a second film that can be peeled off, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used, as long as the adhesion between the resin layer and the second film is smaller than the adhesion between the resin layer and the first film when the second film is peeled off.
[0147] The thickness of the second film is not particularly limited, and can be, for example, 10 μm to 150 μm.
[0148] In order to make a cured coating film on a printed wiring board using a dry film, the second film is peeled off from the dry film, the resin layer exposed by the dry film is overlapped on the substrate formed with a circuit, and a laminator is used to close it to form a resin layer on the substrate formed with a circuit. Then, as long as the formed resin layer is exposed, developed, and heat-cured, a cured coating film can be formed. The second film can be peeled off before or after exposure.
[0149] [cured material]
[0150] The cured product of the present invention is a cured product obtained by curing the resin layer of the photosensitive resin composition of the present invention or the dry film of the present invention. The manufacturing conditions such as curing conditions will be described later in [Printed Wiring Board]. The cured product of the present invention can be applied to printed wiring boards, electronic components, etc.
[0151] [Printed wiring board]
[0152] The printed wiring board of the present invention has a cured product obtained from the resin layer of the photosensitive resin composition or dry film of the present invention. As a method for manufacturing the printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for the coating method by using the above-mentioned organic solvent, and after coating on the substrate by a dip coating method, flow coating method, roller coating method, rod coating method, screen printing method, curtain coating method, etc., the organic solvent contained in the composition is volatilized and dried (pre-dried) at a temperature of 60 to 100° C. for 15 to 90 minutes to form a surface-dried resin layer. In addition, in the case of a dry film, after being bonded to the substrate by a laminator or the like in a manner that the resin layer contacts the substrate, the first film is peeled off to form a resin layer on the substrate.
[0153] As the above-mentioned substrate, in addition to printed wiring boards or flexible printed wiring boards in which circuits are pre-formed with copper or the like, substrates made of materials such as copper-clad laminates for high-frequency circuits using paper phenolic resin, paper epoxy resin, glass cloth epoxy resin, glass polyimide, glass cloth / non-woven fabric epoxy resin, glass cloth / paper epoxy resin, synthetic fiber epoxy resin, fluororesin-polyethylene-polyphenylene ether, polyphenylene ether-cyanate ester, etc. are also used. Copper-clad laminates of all grades (FR-4, etc.) can be cited, as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, chip boards, etc.
[0154] Preferably, the dry film is bonded to the substrate using a vacuum laminator or the like under pressure and heating conditions. By using such a vacuum laminator, when a substrate having a circuit is used, even if there are irregularities on the surface of the circuit substrate, the dry film is closely attached to the circuit substrate, so that bubbles are not mixed in, and the filling property of the recessed portion on the surface of the substrate is also improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0155] The volatilization drying after coating the photosensitive resin composition of the present invention on the substrate can be carried out using a hot air circulation drying furnace, an IR furnace, a hot plate, a convection oven, etc. (using a device having a heat source of air heating method using steam, a method of making hot air in the dryer convectively contact, and a method of spraying from a nozzle to the support). As an apparatus, as a hot air circulation drying furnace, DF610 manufactured by Yamato Scientific Co., Ltd. can be cited.
[0156] After forming a resin layer on a substrate, a photomask having a predetermined pattern is formed and selectively exposed using active energy rays, and the unexposed portion is developed using a dilute alkali aqueous solution (e.g., a 0.3 to 3.0 mass % sodium carbonate aqueous solution) to form a pattern of a cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film for development, thereby forming a patterned cured product on the substrate. It should be noted that, as long as it is within the range that does not impair the characteristics, the first film may be peeled off from the dry film before exposure and the exposed resin layer may be exposed and developed.
[0157] As an exposure machine for irradiating the above-mentioned active energy rays, any device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, etc., and irradiating ultraviolet rays in the range of 350 to 450 nm can be used. Furthermore, a direct drawing device (for example, a laser direct imaging device that directly draws an image with a laser using CAD data from a computer) can also be used. The lamp light source or laser light source of the direct drawing machine can be a light source with a maximum wavelength in the range of 350 to 450 nm. The exposure amount used to form an image varies depending on the film thickness, etc., and can usually be set to 10 to 1000 mJ / cm2 , preferably, it can be set to 20 to 800 mJ / cm 2 As an exposure device equipped with a metal halide lamp, HMW-680-GW20 manufactured by ORC MANUFACTURING CO., LTD. and the like can be cited.
[0158] As the above-mentioned development method, an immersion method, a shower method, a spray method, a brush method, etc. can be used, and as the developer, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, and amines can be used.
[0159] Furthermore, the cured product is irradiated with active energy rays and then heat-cured (for example, at a temperature of 100 to 220° C. for 30 to 90 minutes), or the cured product is heat-cured and then irradiated with active energy rays (for example, at a temperature of 1000 to 2000 mJ / cm 2 ), or only by heating and curing to make it finally fine-cured (formal curing), thereby forming a cured coating film with excellent properties such as adhesion and hardness. As an apparatus, as a UV conveyor belt using a high-pressure mercury lamp, QRM-2082 manufactured by Oak Co., Ltd. can be cited.
[0160] Example
[0161] Hereinafter, the present invention will be described in detail using examples, but the present invention is not limited to the following examples. It should be noted that "parts" and "%" in the following description are all based on mass unless otherwise specified.
[0162] (Preparation of Inorganic Filler A-1 Dispersion Liquid)
[0163] 70 g of spherical silica particles (SO-C2 manufactured by ADMATECHS COMPANY LIMITED, average particle size: 500 nm), 28 g of propylene glycol monomethyl ether acetate as a solvent, and 2 g of a silane coupling agent having a methacryloyl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) were uniformly dispersed to obtain a dispersion of an inorganic filler A-1 treated with methacryloyl silane having a solid content of 70%.
[0164] (Preparation of Inorganic Filler A-2 Dispersion Liquid)
[0165] 70 g of spherical silica particles (SFP-30MHE manufactured by Denka Company Limited., average particle size: 600 nm), 28 g of propylene glycol monomethyl ether acetate as a solvent, and 2 g of a silane coupling agent having a methacryloyl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) were uniformly dispersed to obtain a dispersion of an inorganic filler A-2 treated with methacryloyl silane having a solid content of 70%.
[0166] (Synthesis of carboxyl-containing resin E-1)
[0167] 456 parts of bisphenol A, 228 parts of water, and 649 parts of 37% formalin were added to a flask equipped with a cooling tube and a stirrer, and the temperature was maintained below 40°C. 228 parts of a 25% sodium hydroxide aqueous solution were added, and after the addition was completed, the reaction was carried out at 50°C for 10 hours. After the reaction was completed, it was cooled to 40°C, and neutralized to pH 4 with a 37.5% phosphoric acid aqueous solution while maintaining it below 40°C. Then, the water layer was separated by standing. After separation, 300 parts of methyl isobutyl ketone were added and dissolved uniformly, and then washed 3 times with 500 parts of distilled water, and water, solvent, etc. were removed under reduced pressure at a temperature below 50°C. The obtained polyhydroxymethyl compound was dissolved in 550 parts of methanol to obtain 1230 parts of a methanol solution of the polyhydroxymethyl compound. A portion of the obtained methanol solution of the polyhydroxymethyl compound was dried at room temperature in a vacuum dryer, and as a result, the solid content was 55.2%.
[0168] 500 parts of the methanol solution of the obtained polymethylol compound and 440 parts of 2,6-dimethylphenol were added and uniformly dissolved at 50°C. After uniformly dissolved, methanol was removed under reduced pressure at a temperature below 50°C. Then, 8 parts of oxalic acid were added and reacted at 100°C for 10 hours. After the reaction was completed, the fraction was removed under reduced pressure at 180°C and 50 mmHg to obtain 550 parts of novolac resin A.
[0169] Furthermore, 130 parts of the above-mentioned novolac resin A, 2.6 parts of a 50% sodium hydroxide aqueous solution, and 100 parts of toluene / methyl isobutyl ketone (mass ratio = 2 / 1) were added to an autoclave equipped with a thermometer, a nitrogen introduction device and an alkylene oxide introduction device, and a stirring device. The system was replaced with nitrogen while stirring. Then, the temperature was raised to 150° C. and 8 kg / cm 2 45 parts of ethylene oxide were gradually introduced to react. The reaction was continued for about 4 hours until the gauge pressure reached 0.0 kg / cm 2Afterwards, the mixture was cooled to room temperature. 3.3 parts of 36% aqueous hydrochloric acid solution was added to the reaction solution and mixed to neutralize the sodium hydroxide. The neutralization reaction product was diluted with toluene, washed with water three times, and desolventized using an evaporator to obtain an ethylene oxide adduct of novolac resin A having a hydroxyl value of 175 g / eq. This product is obtained by adding an average of 1 mol of ethylene oxide per equivalent of phenolic hydroxyl groups.
[0170] In a reactor equipped with a stirrer, a thermometer, and an air blowing tube, 175 parts of the ethylene oxide adduct of the novolac resin A obtained as described above, 50 parts of acrylic acid, 3.0 parts of p-toluenesulfonic acid, 0.1 parts of hydroquinone monomethyl ether, and 130 parts of toluene were added, and stirred while blowing air, and the temperature was raised to 115° C., and the water generated by the reaction and toluene were distilled off to form an azeotropic mixture, and then the mixture was allowed to react for another 4 hours, and then cooled to room temperature. The obtained reaction solution was washed with a 5% NaCl aqueous solution, and toluene was removed by reduced pressure distillation, and then diethylene glycol monoethyl ether acetate was added to obtain an acrylic resin solution with a solid content of 68%.
[0171] Then, 312 parts of the obtained acrylic resin solution, 0.1 parts of hydroquinone monomethyl ether and 0.3 parts of triphenylphosphine were added to a four-necked flask equipped with a stirrer and a reflux cooler, the mixture was heated to 110° C., 45 parts of tetrahydrophthalic anhydride were added, and the mixture was reacted for 4 hours. After cooling, a solution of carboxyl resin E-1 with a solid content of 70% and a solid content acid value of 65 mgKOH / g was obtained.
[0172] (Synthesis of carboxyl-containing resin E-2)
[0173] 220 parts of cresol novolac epoxy resin (manufactured by DIC Corporation, EPICLON N-695, epoxy equivalent: 220) were placed in a four-necked flask equipped with a stirrer and a reflux cooler, and 214 parts of carbitol acetate were added and heated to dissolve. Then, 0.1 parts of hydroquinone as a polymerization inhibitor and 2.0 parts of dimethylbenzylamine as a reaction catalyst were added. The mixture was heated to 95-105°C, 72 parts of acrylic acid were gradually dropped, and the mixture was reacted for 16 hours. The reaction product was cooled to 80-90°C, 106 parts of tetrahydrophthalic anhydride were added, the mixture was reacted for 8 hours, cooled, and taken out.
[0174] In the above manner, a solution of carboxyl group-containing resin E-2 having a solid content of 65%, a solid acid value of 100 mgKOH / g, and a weight average molecular weight Mw of about 3500 was obtained.
[0175] [Examples 1 to 15, Comparative Examples 1 to 4]
[0176] (Preparation of photosensitive resin composition)
[0177] Each composition was prepared by blending each component according to the formulation shown in Tables 1 and 2, stirring with a stirrer, and kneading with a three-roll mill. In addition, each numerical value in the table represents parts by mass (solid content conversion amount).
[0178] Table 1
[0179]
[0180] Table 2
[0181]
[0182] The details of each component in Tables 1 and 2 are as follows.
[0183] ※1: YA010C: spherical silica, average particle size 10 nm, methacryloyl surface treatment, manufactured by ADMATECHS COMPANY LIMITED.
[0184] ※2: DA-600: Dipentaerythritol hexaacrylate, manufactured by Sanyo Chemical Industries, Ltd.
[0185] *3: Omnirad 819: acylphosphine oxide-based photopolymerization initiator, manufactured by IGM Resins B.V.
[0186] ※4: PGM-AC-2140Y: spherical silica, average particle size 12nm, surface area 230m 2 / g, methacryloyl surface treatment, methacryloyl treatment rate less than 50%, density 2.0-2.2, manufactured by Nissan Chemical Co., Ltd.
[0187] ※5: PGM-AC-3140Y: spherical silica, average particle size 22nm, surface area 120m 2 / g, methacryloyl surface treatment rate is less than 50%, density is 2.0 to 2.2, manufactured by Nissan Chemical Co., Ltd.
[0188] ※6: PGM-AC-4130Y: spherical silica, average particle size 45nm, surface area 60m 2 / g, methacryloyl surface treatment rate is less than 50%, density is 2.0 to 2.2, manufactured by Nissan Chemical Co., Ltd.
[0189] ※7: PMA-ST: spherical silica, average particle size 12nm, surface area 230m 2 / g, no surface treatment, density 2.0-2.2, manufactured by Nissan Chemical Co., Ltd.
[0190] ※8: PL-1: spherical silica, average particle size 15nm, surface treated, density 0.86 to 1.16, manufactured by Fuso Chemical Industries, Ltd.
[0191] ※9: N-730A: Phenol novolac type epoxy resin, manufactured by DIC Corporation.
[0192] ※10: VG3101L: trifunctional epoxy resin, manufactured by Air Water Inc.
[0193] ※11: IXEPLAS-A1: Cationic scavenger, hydrotalcite, manufactured by Toagosei Co., Ltd.
[0194] ※12: BYK-361N: Surface conditioner, manufactured by BYK JAPAN KK.
[0195] ※13: QS-30: polymerization inhibitor, manufactured by Air Water Performance Chemical Inc.
[0196] (Dry film production)
[0197] Each of the prepared photosensitive resin compositions was applied onto a first film (T-60, manufactured by Toray Industries, Inc., thickness 38 μm) using an applicator so that the film thickness after drying reached 20 μm, and dried at 80° C. for 10 minutes in a hot air circulation drying oven to obtain a dry film having a resin layer composed of a dry coating film of each photosensitive resin composition.
[0198] (Measurement of Melt Viscosity of Photosensitive Composition)
[0199] The melt viscosity (dPa·s) of each photosensitive composition prepared above at 100°C was measured using a vacuum laminator CVP-300 manufactured by Nikko Materials Co., Ltd., by laminating the dry films prepared above at a lamination temperature of 30 to 40°C to prepare a resin layer having a thickness of 300 μm and a width of 20 mm, and a rheometer MARS40 was used under the following conditions. The measurement results are shown in Tables 3 and 4.
[0200] (Measuring conditions of melt viscosity)
[0201] Heating rate: 5℃ / min.
[0202] Frequency: 1Hz.
[0203] Pressure: 3Pa.
[0204] (Landfill)
[0205] Using each photosensitive composition prepared as described above, the embedding property was evaluated by the following method. The dry film was heated and laminated on a substrate having a grid pattern at 100°C for 1 minute using a vacuum laminator (CVP-300, manufactured by Nikko Materials Co., Ltd.), and pressed at 80°C for 1 minute to obtain an evaluation substrate. An optical microscope was used to confirm the number of bubbles generated on the evaluation substrate, and the embedding property was evaluated based on the incidence rate. The embedding property was evaluated according to the following criteria, and the results are shown in Tables 3 and 4. If the evaluation result is "◎" to "△", it is qualified.
[0206] [Evaluation criteria]
[0207] ◎: 0% or more and less than 10%.
[0208] ○: 10% or more and less than 30%.
[0209] △: 30% or more and less than 60%.
[0210] ×: 60% or more.
[0211] (Determination of thermal expansion coefficient)
[0212] The coefficient of thermal expansion was measured by the following method using each photosensitive composition prepared above. The dry film was heated and laminated on a copper foil at 100°C for 1 minute using a vacuum laminator (CVP-300, manufactured by Nikko Materials Co., Ltd.) and pressed at 80°C for 1 minute. Then, the entire surface was exposed at an optimal exposure amount using an exposure device equipped with a high-pressure mercury lamp (short arc lamp). After peeling off the first film, 1% by mass Na 2 O was used at 30°C. 2 CO 3 The aqueous solution is sprayed at a pressure of 2 kg / cm 2 After development, the film was developed for 60 seconds under the conditions of UV conveyor belt with a cumulative light intensity of 2000mJ / cm 2 The cured coating was photocured to obtain a cured coating film after heating at 170°C for 60 minutes in a hot air circulation drying oven. The average thermal linear expansion coefficient of the obtained cured coating film (3 mm × 10 mm size) was measured twice using TMA-Q400EM1797 under the following conditions, and the linear expansion coefficient was determined using the second measurement result. The linear expansion coefficient was evaluated according to the following criteria, and the evaluation results are shown in Tables 3 and 4.
[0213] (Measurement conditions)
[0214] Heating rate: 10℃ / min.
[0215] Test load: 5g.
[0216] [Evaluation criteria]
[0217] Thermal expansion coefficient α1.
[0218] ○: 35 ppm or less. ×: more than 35 ppm.
[0219] Thermal expansion coefficient α2
[0220] ○: 100 ppm or less. ×: more than 100 ppm.
[0221] Table 3
[0222]
[0223] Table 4
[0224]
Claims
1. A photosensitive resin composition comprising (A) an inorganic filler, (B) a compound having at least one acryloyl group or methacryloyl group in one molecule, (C) a photopolymerization initiator, and (D) an inorganic colloid, wherein: The total amount of the inorganic filler (A) and the inorganic colloid (D) is 30.0% by mass or more based on the solid content relative to the total amount of the photosensitive resin composition. The amount of the inorganic colloid (D) is 2.0% by mass or more based on the solid content relative to the total amount of the photosensitive resin composition. The photosensitive resin composition has a melt viscosity of less than 1000 dPa·s at 100° C.
2. The photosensitive resin composition according to claim 1, wherein The surface area of the inorganic colloid (D) is 100 m 2 / g or above.
3. The photosensitive resin composition according to claim 1, wherein The (D) inorganic colloid is colloidal silica having an average particle size of 30 nm or less and subjected to a silane coupling treatment on the surface.
4. The photosensitive resin composition according to claim 3, wherein The colloidal silica is obtained by adding acryloyl groups or methacryloyl groups to a portion less than 50% of the entire surface area.
5. The photosensitive resin composition according to claim 3, wherein The colloidal silica is colloidal silica derived from sodium silicate.
6. The photosensitive resin composition according to claim 3, wherein The density of the colloidal silica is 1.9-2.
2.
7. The photosensitive resin composition according to claim 1, wherein The average particle size of the (A) inorganic filler is 200 nm or more and less than 1000 nm.
8. The photosensitive resin composition according to claim 1, wherein The (A) inorganic filler is silica having acryloyl groups or methacryloyl groups added to the surface by silane coupling treatment.
9. The photosensitive resin composition according to claim 1, wherein The (A) inorganic filler and the (D) inorganic colloid are spherical.
10. The photosensitive resin composition according to claim 1, wherein The ratio of the average particle size of the (A) inorganic filler to the average particle size of the (D) inorganic colloid is 8 or more.
11. The photosensitive resin composition according to claim 1, wherein The photosensitive resin composition further comprises (E) a carboxyl group-containing resin.
12. A dry film, characterized in that: The dry film includes a first film and a resin layer formed on the first film and composed of a dry coating film of the photosensitive resin composition according to any one of claims 1 to 11.
13. A solidified product, characterized in that: The cured product is a cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 11.
14. A solidified product, characterized in that: The cured product is a cured product obtained by curing the resin layer of the dry film according to claim 12 .
15. A printed wiring board, characterized in that: The printed wiring board comprises the cured product according to claim 13 .